Graphene-based composite material, preparation method thereof and application of graphene-based composite material as biosensor
By forming a layered porous structure in graphene-based composite materials and modifying the nickel layer, the problems of poor conductivity and poor stability of traditional electrode materials are solved, and the high sensitivity and rapid response detection effects of graphene-based composite materials in biosensors are achieved. .
Patent Information
- Application Number
- CN202410730952.2
- Authority / Receiving Office
- CN · China
- Patent Type
- Applications(China)
- Current Assignee / Owner
- Filing Date
- 2024-06-06
- Publication Date
- 2024-10-08
AI Technical Summary
Traditional electrode materials have limitations such as poor conductivity, poor stability, and poor flexibility in electrochemical biosensors, and cannot meet the needs of wearable devices and flexible electronics in human health monitoring.
Using the preparation method of graphene-based composite materials, graphene oxide is dispersed to form a layered film, and a nickel layer is modified on the surface to form a layered porous structure, which improves the conductivity and reaction area and is suitable for biosensors.
The prepared graphene-based composite material has good stability and flexibility, can specifically detect glucose, is suitable for wearable biosensors, and achieves high sensitivity and rapid response detection results.
Smart Images

Figure CN118744984A_ABST
Abstract
Description
Technical Field
[0001] The present invention relates to the technical field of graphene composite material preparation, and in particular to a graphene-based composite material, a preparation method thereof, and an application of the graphene-based composite material as a biosensor. Background Art
[0002] Graphene film is a new material with a single-layer sheet structure composed of carbon atoms. It has excellent electrical and thermal conductivity and is considered to be the thinnest, hardest, and best conductive and thermally conductive nanomaterial in the world. With the research and development of graphene-based materials, new sensors based on graphene composites are of great significance to scientific research and the consumer market.
[0003] Electrochemical biosensors have been widely studied as a convenient and rapid detection method. Electrodes, as key components of electrochemical biosensors, provide a direct reaction interface for the reaction and play an important role in the performance of electrochemical biosensors (sensitivity, detection limit, stability, response time, etc.). However, traditional electrodes (glassy carbon electrodes, carbon paper electrodes, screen-printed electrodes, etc.) are currently limited by their own electrode material properties (low specific surface area, poor conductivity, poor stability, sluggish electrochemical kinetics, poor flexibility, etc.), which restricts the development and practical application of sensors and cannot meet the needs of wearable devices and flexible electronics in human health monitoring. Therefore, there is an urgent need to develop new electrode materials.
[0004] In view of this, it is necessary to design an improved graphene-based composite material and a preparation method thereof and an application as a biosensor to solve the above problems. Summary of the invention
[0005] The object of the present invention is to provide a graphene-based composite material and a preparation method thereof and application of the graphene-based composite material as a biosensor.
[0006] To achieve the above-mentioned object of the invention, on the one hand, the present invention provides a method for preparing a graphene-based composite material, comprising the following steps:
[0007] S1, dispersing graphene oxide in water to form a GO dispersion; homogenizing the GO dispersion to obtain a GO slurry; applying a doctor blade to the GO slurry to obtain a GO membrane; then, sequentially subjecting the GO membrane to a thermal reduction treatment, washing and drying treatment to obtain a layered graphene membrane;
[0008] S2, using a graphite rod as an anode, an electrode made of the layered graphene film obtained in step S1 as a cathode, and a Ni salt solution as an electroplating solution for electrolysis, and modifying nickel on the surface of the graphene film to obtain a graphene-based composite material.
[0009] Preferably, in step S1, the thickness of the GO film is 10-50 μm.
[0010] Preferably, in step S1, the temperature of the thermal reduction treatment is 500-3000°C and the time is 1-5h.
[0011] Preferably, in step S2, the current density of the electrolysis process is 0.2-0.4 A / cm 2 , the electrodeposition time is 30-40s.
[0012] Preferably, in step S1, the mass ratio of graphene oxide to water during the formation of the GO dispersion is 1:(30-100).
[0013] Preferably, in step S1, the homogenization treatment is achieved by stirring with a planetary mixer at a speed of 1000-2000 rpm for 10-30 min.
[0014] On the other hand, the preparation method provided by the present invention can be used to prepare a graphene-based composite material, which includes a layered graphene film and a nickel layer deposited on the surface of the graphene film, and the layered graphene film is a layered porous structure.
[0015] In particular, the graphene-based composite material prepared by the preparation method proposed in the present invention can be applied to the field of biosensors, and is particularly suitable as a biosensor for glucose detection.
[0016] The beneficial effects of the present invention are:
[0017] 1. The method for preparing a graphene-based composite material provided by the present invention comprises first preparing a layered graphene film and then using the layered graphene film as a template to construct a sensor. This process can give full play to the structural characteristics of graphene oxide, and finally obtain a graphene-based composite material with stable performance, good flexibility and the ability to specifically detect glucose.
[0018] 2. The preparation method of the graphene-based composite material provided by the present invention can repair the defective structure inside the graphene film by treating the graphene film with a thermal reduction method, and form a layer structure in the film, which is conducive to forming a complete conductive path in the film and improving the conductivity of the graphene film; at the same time, during the treatment process, it can help the cracking and release of oxygen-containing functional groups on the graphene film to form a pore structure, thereby promoting its contact with the electrolyte, increasing the reaction area, and facilitating the subsequent nickel deposition. BRIEF DESCRIPTION OF THE DRAWINGS
[0019] Figure 1 is a SEM image of the graphene film prepared in Example 1 of the present invention;
[0020] Figure 2is the XRD pattern of the graphene film prepared in Example 1 of the present invention;
[0021] Figure 3 This is a Raman image of the graphene film prepared in Example 1 of the present invention;
[0022] Figure 4 This is a SEM image of the graphene-based composite material prepared in Example 1 of the present invention;
[0023] Figure 5 This is an XPS graph of the graphene-based composite material prepared in Example 1 of the present invention;
[0024] Figure 6 This is a comparison chart of the detection performance of Examples 1-4 in the present invention in 1 mM glucose solution under different electrodeposition conditions;
[0025] Figure 7 The schematic diagram of the graphene-based composite material prepared by the present invention for detecting glucose;
[0026] Figure 8 The ampere response diagram of the graphene-based composite material electrode prepared in Example 1 of the present invention under different glucose concentrations;
[0027] Fig. 9 This is a linear relationship diagram between the ampere test current and the glucose concentration of the graphene-based composite material electrode prepared in Example 1 of the present invention at different glucose concentrations;
[0028] Fig.10 This is a test graph of the reaction time of the graphene-based composite material electrode prepared in Example 1 of the present invention under the ampere test;
[0029] Fig.11 This is a test diagram of the anti-interference performance of the graphene-based composite material electrode prepared in Example 1 of the present invention;
[0030] Fig.12 This is a stability test diagram of the graphene-based composite material electrode prepared in Example 1 of the present invention;
[0031] Fig.13 This is a cyclic voltammetry test diagram of the graphene-based composite material electrode prepared in Example 1 of the present invention under different bending states. DETAILED DESCRIPTION
[0032] In order to make the purpose, technical solutions and advantages of the present invention more clear, the present invention is described in detail below with reference to the accompanying drawings and specific embodiments.
[0033] It should also be noted that, in order to avoid obscuring the present invention due to unnecessary details, only structures and / or processing steps closely related to the scheme of the present invention are shown in the drawings, while other details that are not closely related to the present invention are omitted.
[0034] In addition, it should be noted that the terms "comprises", "includes" or any other variations thereof are intended to cover non-exclusive inclusion, so that a process, method, article or apparatus that includes a series of elements includes not only those elements, but also other elements not explicitly listed, or also includes elements inherent to such process, method, article or apparatus.
[0035] On the one hand, the present invention provides a method for preparing a graphene-based composite material. The graphene-based composite material is prepared by using a graphene film with a layered porous structure as a substrate and modifying a nickel layer thereon. The specific preparation method comprises the following steps:
[0036] S1. Preparation of layered graphene film: dispersing graphene oxide (GO) in water to form a GO dispersion; homogenizing the GO dispersion to obtain a GO slurry, and applying a doctor blade to the GO slurry to obtain a GO film; then, sequentially subjecting the GO film to a thermal reduction treatment, washing, and drying treatment to obtain a layered graphene film;
[0037] S2. Preparation of graphene-based composite materials: Using a graphite rod as an anode, an electrode made of a layered graphene film as a cathode, and a Ni salt solution as an electroplating solution for electrolysis, nickel is modified on the surface of the graphene film to obtain a graphene-based composite material.
[0038] As an embodiment of the present invention, in step S1, the mass ratio of graphene oxide to water during the formation of the GO dispersion is 1:(30-100). Preferably, the mass ratio of graphene oxide to water is 1:60.
[0039] As an embodiment of the present invention, in step S1, the homogenization treatment is achieved by stirring with a planetary mixer at a speed of 1000-2000 rpm for 10-30 min, preferably at a speed of 1500 rpm for 20 min.
[0040] As an embodiment of the present invention, in step S1, the thickness of the GO film is 10-50 μm.
[0041] As an embodiment of the present invention, in step S1, the temperature of the thermal reduction treatment is 500-3000° C. and the time is 1-5 hours.
[0042] In the above process, the defective structure inside the graphene film can be repaired through thermal reduction treatment, and a layer structure can be formed in the film, which is conducive to forming a complete conductive path in the film and improving the conductivity of the graphene film; at the same time, the treatment process can help the cracking and release of oxygen-containing functional groups on the graphene film to form a pore structure, thereby promoting its contact with the electrolyte, increasing the reaction area, and facilitating the deposition of nickel.
[0043] As an embodiment of the present invention, in step S2, the Ni salt solution is obtained by mixing a nickel sulfate hexahydrate solution (NiSO4·6H2O) and a nickel chloride hexahydrate solution (NiCl2·6H2O), and the pH of the Ni salt solution is adjusted to about 4.8. The pH can be adjusted by adding H3BO3. Since the role of H3BO3 here is to regulate the pH of the Ni salt solution, other solutions can also be used in the actual preparation process, which is not limited to this. Preferably, Ni in the Ni salt solution 2+ The concentration is 2.4M.
[0044] As an embodiment of the present invention, in step S2, the current density of the electrolysis process is 0.2-0.4A / cm 2 , the electrodeposition time is 30-40s.
[0045] In the above technical solution, nickel is deposited on the graphene film by electrodeposition, which ensures the uniformity of nickel on the graphene film. In addition, since the deposition process occurs along with the electrolysis process, it can ensure that the formed nickel layer is denser and the performance of the composite material is more stable.
[0046] In particular, the graphene-based composite material prepared by the preparation method proposed in the present invention can be applied to the field of biosensors, and is particularly suitable as a biosensor for glucose detection.
[0047] The graphene-based composite material of the present invention, its preparation method and its application as a biosensor are further described below in conjunction with specific embodiments:
[0048] Example 1
[0049] This embodiment prepares a graphene-based composite material, and its specific preparation method includes the following steps:
[0050] S1, dispersing the graphene oxide filter cake into ultrapure water at a mass ratio of 1:60, and uniformly dispersing the graphene oxide in the water by ultrasound and stirring to obtain a graphene oxide gel;
[0051] The obtained graphene oxide gel is degassed by using a planetary homogenizer, and the obtained product is scraped into a GO film by scraping, and the thickness of the GO film is controlled to be 15-25 μm;
[0052] The obtained GO membrane was heat treated. The specific treatment method was as follows: the GO membrane was pretreated at 100°C, then the temperature was raised to 1200°C at a heating rate of 10°C / min, and kept warm for 1h, and then the temperature was further raised to 2800°C at a heating rate of 5°C / min, and kept warm for 1h, thereby obtaining a layered graphene membrane;
[0053] S2, cutting the layered graphene film obtained in step S1 into a 1×2 cm rectangle, immersing it in 30 mL of an electroplating solution having a concentration of 2.3 M NiSO4·6H2O, 0.1 M NiCl2·6H2O and 0.3 M H3BO3, wherein the pH of the electroplating solution is 4.8, and controlling the area of the graphene film immersed in the electroplating solution to be 1×1 cm;
[0054] The electroplating solution was placed in a water bath and the water bath temperature was set to 55°C, which was conducive to the deposition of nickel particles on the electrode. Then, the graphite rod was used as the anode and the electrode made of layered graphene film was used as the cathode. The DC power supply discharge current density was controlled to be 0.2A / cm 2 , the electrodeposition time is 30s, and the graphene-based composite material is obtained.
[0055] It should be noted that the GO filter cake used in the embodiment of the present invention was purchased from Wuxi Chengyi Education Technology Co., Ltd., wherein the solid content of graphene oxide was 45%. Other raw materials and reagents, unless otherwise specified, can be obtained by purchasing on the market.
[0056] The SEM image of the graphene film prepared in this embodiment is as follows: Figure 1 As shown in the figure, the layered structure of graphene can be clearly seen. The graphene film with this structure has a larger specific surface area, which is not only conducive to the electrodeposition of more nickel active sites, but also enhances the contact between the electrode and the electrolyte; the XRD pattern of the graphene film is shown in Figure 2 As shown in the figure, the sharp diffraction peak (002) at about 26.5° proves the regular arrangement of graphene layers, with an interlayer spacing of 0.336nm; the Raman map is shown in Figure 3 As shown in the curve, the weak D peak and strong G peak indicate that the GF with a high degree of graphitization has good lattice integrity, which is consistent with the 2714 cm- 1 The strong 2D peaks at 100 nm and 100 nm are consistent, which proves that the prepared graphene film is highly graphitized and defect-free. The SEM images of the graphene-based composite materials are shown in Figure 4 As shown in the figure, it can be seen that a uniform coating with nickel particles tightly connected is formed on the surface of the graphene film; the XPS figure is as follows Figure 5 As shown in the figure, we can see that Ni 2p The peak at 852.83 eV represents metallic Ni. In addition, Ni 2p3 / 2 (856.67eV) and Ni2p1 / 2 (874.38 eV) two significant peaks, indicating that part of the Ni is in an oxidized state, indicating that the nickel coating exists on the graphene-based composite material in zero-valent and divalent states.
[0057] In order to explore the detection ability of the graphene-based composite material prepared by the above process as a sensor for detecting glucose, the glucose detection performance under different electrodeposition conditions was firstly compared and tested. Figure 6 It can be seen that at a current density of 0.2A / cm 2 When the electrodeposition time is 30s, the performance of graphene-based composite materials in detecting glucose is optimal.
[0058] In order to accurately and quantitatively detect glucose, the ampere method was used to test the detection performance of graphene-based composite materials for different concentrations of glucose. The graphene-based composite materials were used as working electrodes, the working voltage was set to 0.55V, and the relationship between the ampere test current and the glucose concentration was explored. The schematic diagram of the use of graphene-based composite materials to detect glucose is shown in the figure. Figure 7 As shown, the detection process is achieved by converting glucose into gluconolactone with the help of the catalytic effect of the graphene-based composite material. The specific detection mechanism is carried out according to the following reaction formula:
[0059] Ni+2OH - →Ni(OH)2+2e - Formula 1
[0060] Ni(OH)2+OH - →NiOOH+H2O+2e - Formula 2
[0061] NiOOH+Glucose→Ni(OH)2+Gluconolactone Formula 3
[0062] The amperometric test of graphene-based composite materials for different concentrations of glucose is shown in the figure below. Figure 8 As shown in the figure, it can be seen that the addition of glucose will cause the current to change, and as the glucose concentration increases, the current gradually increases. The test concentration range of glucose in this embodiment is 0.5μM-1mM.
[0063] Make a calibration curve of glucose concentration and corresponding current. Fig. 9 It can be seen that there is an obvious linear relationship between the two. The relevant linear equation obtained by calculation is: y = 0.0017C glu +0.084, where the linear correlation coefficient R 2 is 0.997, and the sensitivity of the graphene-based composite electrode for detecting glucose is calculated to be 1719.4 μA·mM -1 cm -2The detection limit was calculated to be 0.2 μM from the standard deviation and slope of the calibration curve with a confidence factor of 3 (S / N = 3), where the time required for the steady-state circuit change between adjacent concentrations was 3 s ( Fig.10 ), indicating that graphene-based composite materials have a faster response speed and can be suitable for the demand of rapid detection of glucose.
[0064] In order to meet the practical application of glucose sensors in the detection process, anti-interference and stability are both essential. In actual application, body fluids often contain interfering substances, such as sucrose (Suc), fructose (Fru), lactose (Lac), ascorbic acid (AA), uric acid (UA), aspartic acid (Asp), NaCl, etc., which will have different effects on the test results of glucose. For this reason, the experiment also explored the effect of the addition of the above-mentioned interfering substances on the glucose detection process. During the test, by adding interfering substances to the glucose system, the effect of interfering substances on the steady-state current of glucose was measured. The results are as follows: Fig.11 As shown in the figure, it can be seen that with the addition of interfering substances (Suc, Fru, Lac, AA, UA, Asp, NaCl), the steady-state current of the electrode detecting glucose only fluctuates slightly, which is much smaller than the current change caused by the addition of glucose (Glu). The main reason for this phenomenon is that the oxidation potential of the interfering substances is higher than that of glucose, and their electro-oxidation is not conducive in an alkaline environment. The results show that graphene-based composite materials can achieve specific detection of glucose.
[0065] Secondly, this example also characterized the stability of the non-enzymatic glucose sensor by measuring the CV response to 1 mM glucose. Fig.12 As shown in the figure, it can be seen that after 7 days of continuous testing, the current size still maintains 96.5% of the original current, proving the excellent stability of the sensor.
[0066] In particular, this example also explores the flexibility of graphene-based composite materials, and the results are as follows Fig.13 As shown, 90° in the figure means that the graphene-based composite material is bent 90°. The results show that the detection current of glucose does not change basically before and after the composite material is bent. This result shows that the composite material has good flexibility and has great application prospects in wearable devices.
[0067] Example 2
[0068] This embodiment prepares a graphene-based composite material, and its specific preparation method includes the following steps:
[0069] S1, dispersing the graphene oxide filter cake into ultrapure water at a mass ratio of 1:60, and uniformly dispersing the graphene oxide in the water by ultrasound and stirring to obtain a graphene oxide gel;
[0070] The obtained graphene oxide gel is degassed by using a planetary homogenizer, and the obtained product is scraped into a GO film by a doctor blade coating method, and the thickness of the GO film is controlled;
[0071] The obtained GO membrane was heat treated. The specific treatment method was as follows: the GO membrane was pretreated at 100°C, then the temperature was raised to 1200°C at a heating rate of 10°C / min, and kept warm for 1h, and then the temperature was further raised to 2800°C at a heating rate of 5°C / min, and kept warm for 1h, thereby obtaining a layered graphene membrane;
[0072] S2, cutting the layered graphene film obtained in step S1 into a 1×2 cm rectangle, immersing it in 30 mL of an electroplating solution having a concentration of 2.3 M NiSO4·6H2O, 0.1 M NiCl2·6H2O and 0.3 M H3BO3, wherein the pH of the electroplating solution is 4.8, and controlling the area of the graphene film immersed in the electroplating solution to be 1×1 cm;
[0073] The electroplating solution was placed in a water bath and the water bath temperature was set to 55°C, which was conducive to the deposition of nickel particles on the electrode. Then, the graphite rod was used as the anode and the electrode made of layered graphene film was used as the cathode. The DC power supply discharge current density was controlled to be 0.3A / cm 2 , the electrodeposition time is 30s, and the graphene-based composite material is obtained.
[0074] Example 3
[0075] This embodiment prepares a graphene-based composite material, and its specific preparation method includes the following steps:
[0076] S1, dispersing the graphene oxide filter cake into ultrapure water at a mass ratio of 1:60, and uniformly dispersing the graphene oxide in the water by ultrasound and stirring to obtain a graphene oxide gel;
[0077] The obtained graphene oxide gel is degassed by using a planetary homogenizer, and the obtained product is scraped into a GO film by a doctor blade coating method, and the thickness of the GO film is controlled;
[0078] The obtained GO membrane was heat treated. The specific treatment method was as follows: the GO membrane was pretreated at 100°C, then the temperature was raised to 1200°C at a heating rate of 10°C / min, and kept warm for 1h, and then the temperature was further raised to 2800°C at a heating rate of 5°C / min, and kept warm for 1h, thereby obtaining a layered graphene membrane;
[0079] S2, cutting the layered graphene film obtained in step S1 into a 1×2 cm rectangle, immersing it in 30 mL of an electroplating solution having a concentration of 2.3 M NiSO4·6H2O, 0.1 M NiCl2·6H2O and 0.3 M H3BO3, wherein the pH of the electroplating solution is 4.8, and controlling the area of the graphene film immersed in the electroplating solution to be 1×1 cm;
[0080] The electroplating solution was placed in a water bath and the water bath temperature was set to 55°C, which was conducive to the deposition of nickel particles on the electrode. Then, the graphite rod was used as the anode and the electrode made of layered graphene film was used as the cathode. The DC power supply discharge current density was controlled to be 0.4A / cm 2 , the electrodeposition time is 30s, and the graphene-based composite material is obtained.
[0081] Example 4
[0082] This embodiment prepares a graphene-based composite material, and its specific preparation method includes the following steps:
[0083] S1, dispersing the graphene oxide filter cake into ultrapure water at a mass ratio of 1:60, and uniformly dispersing the graphene oxide in the water by ultrasound and stirring to obtain a graphene oxide gel;
[0084] The obtained graphene oxide gel is degassed by using a planetary homogenizer, and the obtained product is scraped into a GO film by a doctor blade coating method, and the thickness of the GO film is controlled;
[0085] The obtained GO membrane was heat treated. The specific treatment method was as follows: the GO membrane was pretreated at 100°C, then the temperature was raised to 1200°C at a heating rate of 10°C / min, and kept warm for 1h, and then the temperature was further raised to 2800°C at a heating rate of 5°C / min, and kept warm for 1h, thereby obtaining a layered graphene membrane;
[0086] S2, cutting the layered graphene film obtained in step S1 into a 1×2 cm rectangle, immersing it in 30 mL of an electroplating solution having a concentration of 2.3 M NiSO4·6H2O, 0.1 M NiCl2·6H2O and 0.3 M H3BO3, wherein the pH of the electroplating solution is 4.8, and controlling the area of the graphene film immersed in the electroplating solution to be 1×1 cm;
[0087] The electroplating solution was placed in a water bath and the water bath temperature was set to 55°C, which was conducive to the deposition of nickel particles on the electrode. Then, the graphite rod was used as the anode and the electrode made of layered graphene film was used as the cathode. The DC power supply discharge current density was controlled to be 0.2A / cm 2 , the electrodeposition time is 40s, and the graphene-based composite material is obtained.
[0088] The above embodiments are only used to illustrate the technical solution of the present invention rather than to limit it. Although the present invention has been described in detail with reference to the preferred embodiments, those skilled in the art should understand that the technical solution of the present invention may be modified or replaced by equivalents without departing from the spirit and scope of the technical solution of the present invention.
Claims
1. A method for preparing a graphene-based composite material, characterized in that: The steps include: S1, dispersing graphene oxide in water to form a GO dispersion; homogenizing the GO dispersion to obtain a GO slurry; applying a doctor blade to the GO slurry to obtain a GO membrane; then, sequentially subjecting the GO membrane to a thermal reduction treatment, washing and drying treatment to obtain a layered graphene membrane; S2, using a graphite rod as an anode, an electrode made of the layered graphene film obtained in step S1 as a cathode, and a Ni salt solution as an electroplating solution for electrolysis, and modifying nickel on the surface of the graphene film to obtain a graphene-based composite material.
2. The method for preparing a graphene-based composite material according to claim 1, characterized in that: In step S1, the thickness of the GO film is 10-50 μm.
3. The method for preparing a graphene-based composite material according to claim 1, characterized in that: In step S1, the temperature of the thermal reduction treatment is 500-3000°C and the time is 1-5h.
4. The method for preparing a graphene-based composite material according to claim 1, characterized in that: In step S2, the current density of the electrolysis process is 0.2-0.4A / cm 2 , the electrodeposition time is 30-40s.
5. The method for preparing a graphene-based composite material according to claim 1, characterized in that: In step S1, the mass ratio of graphene oxide to water during the formation of the GO dispersion is 1:(30-100).
6. The method for preparing a graphene-based composite material according to claim 1, characterized in that: In step S1, the homogenization treatment is achieved by stirring with a planetary mixer at a speed of 1000-2000 rpm for 10-30 min.
7. A graphene-based composite material prepared by the preparation method according to any one of claims 1 to 6, characterized in that: It comprises a layered graphene film and a nickel layer deposited on the surface of the graphene film, and the layered graphene film is a layered porous structure.
8. Application of a graphene-based composite material prepared by the preparation method described in any one of claims 1 to 6 in the field of biosensors.
9. Use of a graphene-based composite material prepared by the preparation method described in any one of claims 1 to 6 in glucose detection.
Citation Information
Patent Citations
Preparation method of nickel-graphene complex phase
CN103938255A
Glassy carbon electrode modified by nickel-copper alloy and composite graphene as well as application of glassy carbon electrode
CN104614427A
Graphene-modified high strength nickel-based composite material and preparation method thereof
CN111254477A
High-conductivity and high-stability flexible graphene electrode and preparation method thereof
CN112366023A
Preparation method and system of graphene film
CN117342548A