Heterostructure electromagnetic wave absorbent composed of multiple layers of titanium carbide and cobalt ferrite nanosheets and preparation method and application thereof

By in-situ growth of cobalt ferrite nanosheets on multi-layer Ti3C2Tx, a house of cards heterostructure is constructed, which solves the problems of agglomeration of cobalt ferrite nanoparticles and poor microwave absorption performance of Ti3C2Tx, and achieves efficient electromagnetic wave absorption performance improvement and frequency band Matching feature optimization.

CN118745007APending Publication Date: 2024-10-08GUANGDONG UNIV OF TECH
View PDF 2 Cites 0 Cited by

Patent Information

Application Number
CN202410914490.X
Authority / Receiving Office
CN · China
Patent Type
Applications(China)
Current Assignee / Owner
Filing Date
2024-07-09
Publication Date
2024-10-08

Smart Images

  • Figure HDA0004934699990000011
    Figure HDA0004934699990000011
  • Figure HDA0004934699990000012
    Figure HDA0004934699990000012
  • Figure HDA0004934699990000021
    Figure HDA0004934699990000021
Patent Text Reader

Abstract

The invention belongs to the technical field of electromagnetic wave absorption, and discloses a heterostructure electromagnetic wave absorbent composed of multiple layers of titanium carbide (Ti3C2Tx) and cobalt ferrite nanosheets as well as a preparation method and application of the heterostructure electromagnetic wave absorbent. The material is prepared by adopting a quaternary ammonium salt oriented in-situ growth method and a high-temperature cracking method, and the ferrocobalt layered double hydroxide can be converted into a magnetic component cobalt ferrite nanosheet after being subjected to high-temperature cracking, so that the impedance matching of the composite material can be effectively adjusted and an additional electromagnetic wave loss mechanism can be increased due to the introduction of the component; and the multi-reflection behavior of incident electromagnetic waves can be further promoted. According to the method, electromagnetic parameters are regulated and controlled by changing the content of multi-layer Ti < 3 > C < 2 > T < x >, so that the composite material obtains the optimal performance; cobalt ferrite vertically grows on multiple layers of Ti3C2Tx in situ in the form of nanosheets, so that the adverse agglomeration behavior of magnetic component nanoparticles is effectively avoided, and the magnetic loss capacity of magnetic components is fully exerted.
Need to check novelty before this filing date? Find Prior Art

Description

Technical Field

[0001] The present invention belongs to the field of electromagnetic wave absorption technology, and particularly relates to a multi-layer titanium carbide (Ti3C2T x ) and cobalt ferrite nanosheets, and its preparation method and application. Background Art

[0002] At present, the electromagnetic waves from the widespread use of electronic devices (such as smartphones and household devices) have posed a certain degree of threat to the environment and human health. In particular, with the vigorous development of 5G communication technology, the service frequencies of more and more electronic devices are gradually moving towards high-frequency bands. Therefore, it is very important to explore electromagnetic wave absorbing materials with strong electromagnetic wave energy absorption and wide-band effective absorption characteristics to alleviate the increasingly serious electromagnetic wave pollution problem.

[0003] As a representative member of the emerging MXene material family, Ti3C2T x Due to its unique multilayer structure, large specific surface area, rich surface functional groups and high electrical conductivity, it has attracted great attention in the field of electromagnetic wave absorption in recent years. x It can only show relatively poor microwave absorption performance. Cobalt ferrite is a spinel ferrite with the advantages of low price, abundant raw materials and high magnetic permeability in the GHz band. x is an improved Ti3C2T x An effective method to improve microwave absorption performance. x In the system composed of Ti3C2T x The agglomeration is not conducive to the full play of magnetic loss, which results in little improvement in the electromagnetic wave absorption performance of the composite system. Summary of the invention

[0004] In order to solve the above-mentioned shortcomings and deficiencies in the prior art, the primary purpose of the present invention is to provide a multilayer titanium carbide (Ti3C2T x ) and a method for preparing an electromagnetic wave absorber with a house of cards heterostructure composed of cobalt ferrite nanosheets.

[0005] Another object of the present invention is to provide a multilayer titanium carbide (Ti3C2T x ) and cobalt ferrite nanosheets; the unique house-of-cards heterostructure of this material can effectively promote the multiple reflection loss of the incident electromagnetic wave. xThe relative content in the composite material achieves simultaneous optimization of impedance matching and attenuation constant to demonstrate a wide effective absorption bandwidth and strong electromagnetic wave loss capability.

[0006] Another object of the present invention is to provide the above-mentioned multilayer titanium carbide (Ti3C2T x ) and cobalt ferrite nanosheets composed of a house of cards heterostructure electromagnetic wave absorber.

[0007] The purpose of the present invention is achieved through the following technical solutions:

[0008] A multilayer titanium carbide (Ti3C2T x ) and cobalt ferrite nanosheets, comprising the following steps:

[0009] (1) adding iron salt, cobalt salt and quaternary ammonium salt to deionized water, and continuously stirring to obtain solution A;

[0010] (2) Multilayer Ti3C2T x Add to deionized water and treat with ultrasound to obtain suspension B;

[0011] (3) Pour suspension B into solution A and continue stirring to obtain solution C;

[0012] (4) adding hydroxide and borohydride to deionized water, and continuously stirring to obtain solution D;

[0013] (5) Solution D was added dropwise to solution C by a peristaltic pump to obtain solution E, and solution E was continuously stirred at room temperature to obtain a multilayer Ti3C2T x and composite materials with house-of-cards heterostructures composed of cobalt-iron layered double hydroxide nanosheets;

[0014] (6) The multilayer Ti3C2T x The composite material with a house of cards heterostructure composed of cobalt-iron layered double hydroxide nanosheets was pyrolyzed at high temperature to obtain a multilayer Ti3C2T x Heterostructure electromagnetic wave absorber composed of cobalt ferrite nanosheets.

[0015] In step (1), the iron salt is ferric nitrate nonahydrate, the cobalt salt is cobalt sulfate heptahydrate, the quaternary ammonium salt is hexadecyltrimethylammonium bromide, and the continuous stirring time is 15 minutes.

[0016] The ultrasonic treatment time in step (2) is 15 minutes.

[0017] The continuous stirring time in step (3) is 15 minutes.

[0018] In step (4), the hydroxide is sodium hydroxide, the borohydride is sodium borohydride, and the continuous stirring time is 5 minutes.

[0019] In step (5), the flow rate of the peristaltic pump is 2 mL / s, the room temperature is 30° C., and the continuous stirring time is 30 min.

[0020] The high temperature cracking in step (6) is carried out by heating the temperature to 500°C at a heating rate of 2°C / min and then keeping the temperature for 2h.

[0021] The mass ratio of the iron salt, cobalt salt, quaternary ammonium salt in step (1) and the hydroxide and borohydride in step (4) is 2.78:1.41:1:0.4:0.3.

[0022] Ti3C2T in step (2) x The dosage is ≥50mg and <160mg.

[0023] A multilayer titanium carbide (Ti3C2T x ) and cobalt ferrite nanosheets.

[0024] The electromagnetic wave absorber is a multilayer titanium carbide (Ti3C2T x ) were in situ vertically grown on the surface of the nanostructured material to form a unique house-of-cards heterostructure.

[0025] The above-mentioned multilayer titanium carbide (Ti3C2T x ) and cobalt ferrite nanosheets in the field of electromagnetic wave absorption.

[0026] Principle of the present invention:

[0027] The present invention prepares a multilayer Ti3C2T3O3 heterostructure with a house of cards structure by a simple quaternary ammonium salt-guided in-situ growth method and a high-temperature pyrolysis method. x and cobalt ferrite nanosheets. x The in-situ vertically grown cobalt ferrite nanosheets not only add an additional magnetic loss mechanism to the composite system, strengthening the loss of incident electromagnetic waves, but also achieve a synergistic effect of dielectric-magnetic properties and improve the impedance matching of the composite material. In addition, the vertical arrangement of cobalt ferrite nanosheets further promotes the multiple reflection behavior of the incident electromagnetic waves.

[0028] Compared with the prior art, the present invention has the following advantages and effects:

[0029] (1) The present invention introduces a multilayer Ti3C2T xThe vertically grown cobalt ferrite nanosheets can effectively avoid the agglomeration phenomenon of cobalt ferrite nanoparticles commonly found in the prior art, so as to better exert the geomagnetic loss capacity of the magnetic component of cobalt ferrite; on the other hand, the vertical arrangement of cobalt ferrite nanosheets can further promote the multiple reflection behavior of the incident electromagnetic wave, making the multilayer Ti3C2T3 with a unique house of cards heterostructure x The composite absorber composed of cobalt ferrite nanosheets has achieved commendable reflection loss (-49.4dB, f=29.0GHz, d=3.0mm) and excellent effective absorption bandwidth (10.8GHz, d=2.3mm) in the frequency range of 2-40GHz, showing great potential in the field of electromagnetic wave absorption and has broad application prospects.

[0030] (2) The preparation method of the present invention can be achieved by changing the Ti3C2T x The content of dielectric constant is adjusted to obtain the best impedance matching characteristics in different frequency bands.

[0031] (3) The preparation method of the present invention has few steps, short time, large output, is simple and convenient, and can obtain a multilayer Ti3C2T3O ... x A composite electromagnetic wave absorber with a house of cards heterostructure composed of cobalt ferrite nanosheets. BRIEF DESCRIPTION OF THE DRAWINGS

[0032] Figure 1 The multilayer Ti3C2T prepared in Examples 1 to 3 x Scanning electron microscope images (a, b, c) of the composite electromagnetic wave absorber with a house of cards heterostructure composed of cobalt ferrite nanosheets.

[0033] Figure 2 The multilayer Ti3C2T prepared in Example 1 x X-ray diffraction patterns of the composite electromagnetic wave absorber with a house of cards heterostructure composed of cobalt ferrite nanosheets before and after high-temperature pyrolysis.

[0034] Figure 3 The multilayer Ti3C2T prepared in Examples 1 to 3 x Three-dimensional graph of the electromagnetic wave absorption performance of the composite electromagnetic wave absorber with a house of cards heterostructure composed of cobalt ferrite nanosheets in the frequency range of 2–40 GHz (a–i).

[0035] Figure 4 The multilayer Ti3C2T prepared in Examples 1 to 3 xThe maximum effective absorption bandwidth (a1–c3) of the composite electromagnetic wave absorber with a house-of-cards heterostructure composed of cobalt ferrite nanosheets in the frequency range of 2–40 GHz.

[0036] Figure 5 The multilayer Ti3C2T prepared in Examples 1 to 3 x Electromagnetic wave impedance matching diagram (a1–c3) of the composite electromagnetic wave absorber with a house of cards heterostructure composed of cobalt ferrite nanosheets in the frequency range of 2–40 GHz.

[0037] Figure 6 The multilayer Ti3C2T prepared in Examples 1 to 3 x Graph (a–c) of the electromagnetic wave attenuation constants of a composite electromagnetic wave absorber with a house of cards heterostructure composed of cobalt ferrite nanosheets in the frequency range of 2–40 GHz. DETAILED DESCRIPTION

[0038] The present invention is further described below with reference to specific embodiments, but they should not be construed as limiting the present invention.

[0039] Example 1: Preparation of TCF-0.5-500 composite material

[0040] (1) Add 2.78 g of ferric nitrate nonahydrate, 1.41 g of cobalt sulfate heptahydrate and 1 g of hexadecyltrimethylammonium bromide to 300 ml of deionized water and stir for 15 min to obtain solution A; add 50 mg of multilayer Ti3C2T x Add to 20 ml of deionized water and ultrasonically treat for 15 min to obtain suspension B; pour suspension B into solution A and continue stirring for 15 min to obtain solution C;

[0041] (2) 0.4 g of sodium hydroxide and 0.3 g of sodium borohydride were added to 60 ml of deionized water and stirred for 5 min to obtain solution D. Solution D was added dropwise to solution C at a flow rate of 2 mL / s through a peristaltic pump to obtain solution E. Solution E was then stirred for 30 min at room temperature to obtain a multilayer Ti3C2T x and composite materials with house-of-cards heterostructures composed of cobalt-iron layered double hydroxide nanosheets;

[0042] (3) Multilayer Ti3C2T x The composite material with a house of cards heterostructure composed of cobalt-iron layered double hydroxide nanosheets was pyrolyzed at 500℃ in N2 atmosphere with a holding time of 2h and a heating rate of 2℃ / min to obtain a multilayer Ti3C2T xThe composite electromagnetic wave absorber with a house of cards heterostructure composed of cobalt ferrite nanosheets is named TCF-0.5-500.

[0043] Example 2: Preparation of TCF-0.75-500 composite material

[0044] (1) Add 2.78 g of ferric nitrate nonahydrate, 1.41 g of cobalt sulfate heptahydrate and 1 g of hexadecyltrimethylammonium bromide to 300 ml of deionized water and stir for 15 min to obtain solution A; add 100 mg of the raw material multilayer Ti3C2T x Add to 20 ml of deionized water and ultrasonically treat for 15 min to obtain suspension B; pour suspension B into solution A and continue stirring for 15 min to obtain solution C;

[0045] (2) 0.4 g of sodium hydroxide and 0.3 g of sodium borohydride were added to 60 ml of deionized water and stirred for 5 min to obtain solution D. Solution D was added dropwise to solution C at a flow rate of 2 mL / s through a peristaltic pump to obtain solution E. Solution E was then stirred for 30 min at room temperature to obtain a multilayer Ti3C2T x and composite materials with house-of-cards heterostructures composed of cobalt-iron layered double hydroxide nanosheets;

[0046] (3) Multilayer Ti3C2T x The composite material with a house of cards heterostructure composed of cobalt-iron layered double hydroxide nanosheets was pyrolyzed at 500℃ in N2 atmosphere with a holding time of 2h and a heating rate of 2℃ / min to obtain a multilayer Ti3C2T x The composite electromagnetic wave absorber with a house of cards heterostructure composed of cobalt ferrite nanosheets is named TCF-0.75-500.

[0047] Example 3: Preparation of TCF-1.5-500 composite material

[0048] (1) Add 2.78 g of ferric nitrate nonahydrate, 1.41 g of cobalt sulfate heptahydrate and 1 g of hexadecyltrimethylammonium bromide to 300 ml of deionized water and stir for 15 min to obtain solution A; add 150 mg of multilayer Ti3C2T x Add to 20 ml of deionized water and ultrasonically treat for 15 min to obtain suspension B; pour suspension B into solution A and continue stirring for 15 min to obtain solution C;

[0049] (2) 0.4 g of sodium hydroxide and 0.3 g of sodium borohydride were added to 60 ml of deionized water and stirred for 5 min to obtain solution D. Solution D was added dropwise to solution C at a flow rate of 2 mL / s through a peristaltic pump to obtain solution E. Solution E was then stirred for 30 min at room temperature to obtain a multilayer Ti3C2T x and composite materials with house-of-cards heterostructures composed of cobalt-iron layered double hydroxide nanosheets;

[0050] (3) Multilayer Ti3C2T x The composite material with a house of cards heterostructure composed of cobalt-iron layered double hydroxide nanosheets was pyrolyzed at 500℃ in N2 atmosphere with a holding time of 2h and a heating rate of 2℃ / min to obtain a multilayer Ti3C2T x The composite electromagnetic wave absorber with a house of cards heterostructure composed of cobalt ferrite nanosheets is named TCF-1.5-500.

[0051] Embodiment 4 (Effect Embodiment):

[0052] Made of multilayer Ti3C2T x Structural characterization and performance testing of composite materials with house-of-cards heterostructure composed of cobalt ferrite nanosheets:

[0053] (1) Composite material structure characterization:

[0054] The multilayer Ti3C2T obtained in Examples 1-3 x The surface morphology of the composite electromagnetic wave absorber with a house of cards heterostructure composed of cobalt ferrite nanosheets is as follows Figure 1 As shown in a, b, and c. Regardless of the multilayer Ti3C2T x Regardless of the amount of addition, the obtained composite materials all exhibit a unique house of cards heterostructure, with cobalt ferrite nanosheets in situ vertically grown on the multilayer Ti3C2T x A large number of heterogeneous interfaces are formed, which significantly enhances the interface polarization loss of the composite material. At the same time, it can further promote the multiple reflection loss of the incident electromagnetic wave and improve the attenuation ability of the electromagnetic wave energy.

[0055] In order to characterize the x The crystal structure and phase composition of the composite material with a house of cards heterostructure composed of cobalt ferrite nanosheets before and after high temperature pyrolysis are compared with the multilayer Ti3C2T prepared in Example 1. x X-ray diffraction analysis was performed on the composite electromagnetic wave absorber sample with a house of cards heterostructure composed of cobalt ferrite nanosheets. Figure 2As shown, for the sample that was not subjected to high temperature cracking, several peaks corresponding to cobalt-iron layered double hydroxides appeared. In contrast, the peaks corresponding to multilayer Ti3C2T x The peak of (002) crystal plane disappears, which can be attributed to the cobalt-iron layered double hydroxide on the multilayer Ti3C2T x The in-situ vertical growth on the Ti3C2T x After high temperature pyrolysis, it corresponds to the ordered stacking of multilayer Ti3C2T x The peak of the (002) crystal plane reappears, and this peak is larger than that of pure multilayer Ti3C2T x The peak of the (002) crystal plane shifts to a lower angle, which means that the multilayer Ti3C2T x The interlayer spacing has changed. In addition, the peaks corresponding to the cobalt-iron layered double hydroxide have all disappeared. The peaks at 30.1°, 35.4°, 43.5°, 57.2° and 62.7° correspond to the (220), (311), (400), (511) and (440) crystal planes of cobalt ferrite, respectively. It is worth noting that several diffraction peaks corresponding to the metal cobalt element with a face-centered cubic structure appear at 44.2°, 51.5° and 75.9°, indicating that after high-temperature pyrolysis, the cobalt-iron layered double hydroxide has been transformed into cobalt ferrite and elemental cobalt. According to the intensity of the peaks, it can be determined that cobalt ferrite is the main phase and elemental cobalt is the secondary phase. The appearance of elemental cobalt can be attributed to the decomposition of the residual sodium borohydride at 500°C, which has a reducing effect on the hydrogen, so that part of the cobalt ions in the cobalt ferrite are reduced to elemental cobalt.

[0056] (2) Performance characterization:

[0057] like Figure 3 and 4 As shown, the electromagnetic wave absorption performance of TCF-0.5-500, TCF-0.75-500, and TCF-1.5-500 was tested in the frequency range of 2–40 GHz and the thickness range of 1.5–4.0 mm. Figure 3 From a–c, we can find that in the frequency range of 2–18 GHz, TCF-1.5-500 exhibits the best electromagnetic wave loss intensity compared to other samples, achieving a reflection loss of -40.4 dB at a matching thickness of 1.7 mm. Figure 3 d–f, in the frequency range of 18–26.5 GHz, TCF-1.5-500 once again exhibits the best electromagnetic wave loss strength, achieving a reflection loss of -44.1 dB at a matching thickness of 2.5 mm; Figure 3In the frequency range of 26.5–40 GHz, TCF-1.5-500 also exhibits the best electromagnetic wave loss strength, achieving a reflection loss of -49.4 dB at a matching thickness of 3.0 mm. Figure 4 From a1–c3, we can find that TCF-1.5-500 has a wider effective absorption bandwidth in the frequency range of 2–40 GHz compared to other samples, and its maximum effective absorption bandwidth can reach 10.8 GHz when the matching thickness is 2.3 mm. In summary, TCF-1.5-500 has the best electromagnetic wave absorption performance among the three composite materials.

[0058] like Figure 5 As shown, a1–c1 is the impedance matching diagram of TCF-0.5-500 in the frequency range of 2–40 GHz, a2–c2 is the impedance matching diagram of TCF-0.75-500 in the frequency range of 2–40 GHz, and a3–c3 is the impedance matching diagram of TCF-0.75-500 in the frequency range of 2–40 GHz. Generally speaking, the closer the impedance matching value is to 1, the more electromagnetic waves will enter the material, and the fewer electromagnetic waves will be reflected in the air and the upper surface of the material. By fixing the impedance matching values ​​to 0.8 and 1.2 respectively, the impedance matching value corresponding to the red dotted line part is 0.8, and the impedance matching value corresponding to the black dotted line part is 1.2. In the frequency range of 2–18 GHz, as Figure 5 As shown in a1–a3, TCF-0.75-500 has the largest area enclosed by the red dotted line and the black dotted line, indicating that it has better impedance matching characteristics than the other two composite materials in this band; in the frequency range of 18–26.5 GHz, Figure 5 As shown in b1–b3, TCF-0.5-500 has the largest area enclosed by the red dotted line and the black dotted line, indicating that it has better impedance matching characteristics than the other two composite materials in this band; in the frequency range of 26.5–40 GHz, Figure 5 TCF-1.5-500 shown in c1–c3 has the largest area enclosed by the red dotted line and the black dotted line, indicating that it has better impedance matching characteristics than the other two composite materials in this band. In summary, this type of composite material can be easily controlled by multilayer Ti3C2T x The added amount can achieve the best impedance matching characteristics in different frequency bands.

[0059] like Figure 6As shown in a-c, in the frequency range of 2-18 GHz, the attenuation constant of TCF-1.5-500 is more prominent than that of other samples. In particular, when the frequency of the electromagnetic field increases to 18 GHz, its attenuation constant can reach 600; on the contrary, in the frequency range of 26.5-40 GHz, the attenuation constant of TCF-1.5-500 is not as good as that of other samples, indicating that this band is not conducive to TCF-1.5-500 showing a significant attenuation ability of incident electromagnetic waves; in the frequency range of 26.5-40 GHz, the attenuation constant of TCF-1.5-500 is the largest among these samples.

[0060] The above is a simple quaternary ammonium salt-guided in-situ growth method and high-temperature pyrolysis method to prepare a multilayer Ti3C2T with a house of cards heterostructure. x A detailed description of the composite materials (TCF-0.5-500, TCF-0.75-500 and TCF-1.5-500) composed of cobalt ferrite nanosheets.

[0061] The above embodiments are preferred implementation modes of the present invention, but the implementation modes of the present invention are not limited to the above embodiments. Any other changes, modifications, substitutions, combinations, and simplifications that do not deviate from the spirit and principles of the present invention should be equivalent replacement methods and are included in the protection scope of the present invention.

Claims

1. A method for preparing a heterostructured electromagnetic wave absorber composed of multilayer titanium carbide and cobalt ferrite nanosheets, Features The steps include: (1) adding iron salt, cobalt salt and quaternary ammonium salt to deionized water, and continuously stirring to obtain solution A; (2) Multilayer Ti 3 C 2 T x Add to deionized water and treat with ultrasound to obtain suspension B; (3) Pour suspension B into solution A and continue stirring to obtain solution C; (4) adding hydroxide and borohydride to deionized water, and continuously stirring to obtain solution D; (5) Solution D is added dropwise to solution C by a peristaltic pump to obtain solution E, and solution E is continuously stirred at room temperature to obtain a multilayer Ti 3 C 2 T x and composite materials with house-of-cards heterostructures composed of cobalt-iron layered double hydroxide nanosheets; (6) The multi-layer Ti 3 C 2 T x A composite material with a house of cards heterostructure composed of cobalt-iron layered double hydroxide nanosheets is subjected to high-temperature pyrolysis to obtain a heterostructure electromagnetic wave absorber composed of multilayer titanium carbide and cobalt ferrite nanosheets.

2. The preparation method according to claim 1, Features: In step (1), the iron salt is ferric nitrate nonahydrate, the cobalt salt is cobalt sulfate heptahydrate, the quaternary ammonium salt is hexadecyltrimethylammonium bromide, and the continuous stirring time is 15 minutes; and in step (2), the ultrasonic treatment time is 15 minutes.

3. The preparation method according to claim 1, Features: The continuous stirring time in step (3) is 15 minutes; the hydroxide in step (4) is sodium hydroxide, the borohydride is sodium borohydride, and the continuous stirring time is 5 minutes.

4. The preparation method according to claim 1, Features: In step (5), the flow rate of the peristaltic pump is 2 ml / s, the room temperature is 30° C., and the continuous stirring time is 30 min. In step (6), the high temperature pyrolysis is heated to 500° C. at a heating rate of 2° C. / min and then kept warm for 2 h.

5. The preparation method according to claim 1, Features: The mass ratio of the iron salt, cobalt salt, quaternary ammonium salt in step (1) to the hydroxide and borohydride in step (4) is 2.78:1.41:1:0.4:0.3; the Ti in step (2) 3 C 2 T x The dosage is ≥50mg and <160mg.

6. A heterostructure electromagnetic wave absorber composed of multilayer titanium carbide and cobalt ferrite nanosheets prepared by the preparation method according to any one of claims 1 to 5.

7. The heterostructure electromagnetic wave absorber composed of multilayer titanium carbide and cobalt ferrite nanosheets according to claim 6, Features: The electromagnetic wave absorber is formed by in-situ vertical growth of cobalt ferrite nanosheets on multilayer titanium carbide to form a unique house of cards heterostructure.

8. Use of the heterostructure electromagnetic wave absorber composed of multilayer titanium carbide and cobalt ferrite nanosheets according to claim 6 in the field of electromagnetic wave absorption.

Citation Information

Patent Citations

  • Layered MXene loaded cobalt ferrite composite wave-absorbing material and preparation method thereof

    CN110290691A

  • Hierarchical porous cobalt / iron bimetallic oxide nanosheet catalyst with rich oxygen vacancies, and preparation method and application thereof

    CN110548514A