A fully quantified cementitious composite material based on red mud and its preparation method
By modifying the red mud, Si-O-Al grid structure and three-dimensional network structure are generated, and cross-linking of silicone resin and silica, the problem of dissolution of high alkaline substances and heavy metals in red mud is solved. The mechanical properties and water permeability of semi-flexible pavement materials are improved, and the effective utilization of red mud and the long-term stability of pavement materials are achieved.
Patent Information
- Application Number
- CN202410741671.7
- Authority / Receiving Office
- CN · China
- Patent Type
- Patents(China)
- Current Assignee / Owner
- Filing Date
- 2024-06-11
- Publication Date
- 2024-12-03
- Estimated Expiration
- 2044-06-11
AI Technical Summary
The dissolution problem of high alkaline substances and heavy metal elements in red mud limits its large-scale utilization in engineering materials, and the existing technology is difficult to effectively solve the crack resistance, water damage resistance and water stability of semi-flexible road surfaces in rainy and high temperature areas. Sexual problems.
Using a gelled composite material based on red mud, the Si-O-Al grid structure is generated to seal the heavy metal by modification of sodium metasilicate, silica and ore powder, and the silicone resin and silica are used. The crosslinked matrix forms a three-dimensional network structure to improve the mechanical properties and water resistance of the material. At the same time, the addition of lipophilic calcium-based montmorillonite is added to enhance water permeability and water purification function.
The gelled composite material with high permeability and low shrinkage in red mud has been achieved, which significantly improves the mechanical properties and service life of semi-flexible pavement materials, avoids the dissolution of high alkali substances and heavy metals, and improves water permeability and water resistance. Solve the brittleness and water absorption of pavement materials.
Smart Images

Figure CN118745103B_ABST
Abstract
Description
Technical Field
[0001] The invention relates to the technical field of building materials, and in particular to a red mud-based gelled composite material and a preparation method thereof. Background Art
[0002] Red mud is an insoluble residue with the main chemical components of Al2O3, Fe2O3, SiO2, CaO, Na2O, TiO2, etc. It is the largest waste generated in the production process of alumina and the largest source of pollution in alumina plants. my country's red mud emissions in 2021 are about 120 million tons, and the total red mud emissions have reached 800 million tons. However, the current treatment methods are mostly to transport red mud to the landfill, build dams for wet storage, and rely on natural sedimentation to separate the solution for reuse. Every year, a lot of costs are spent on the construction and maintenance of red mud landfills. Such a large amount of red mud has not been effectively and fully utilized, causing serious harm to the social environment: occupying large tracts of land and increasing infrastructure investment. Moreover, the pH of red mud is between 12 and 14. Long-term stacking will break the pH balance of the soil and damage the ecological environment. If its filtrate seeps, it will also cause changes in groundwater hardness. In addition, red mud also contains a small amount of heavy metals. The loss of these components will cause great harm to the health of humans and other animals.
[0003] Resource utilization is the best way to achieve red mud disposal, especially in building materials, which can achieve large-scale disposal of red mud and significantly improve the comprehensive utilization level of red mud. In recent years, domestic and foreign scholars have conducted a series of studies on the complete set of resource utilization technologies of red mud in the fields of cementitious materials, pavement water-stabilizing materials, building blocks, ceramsite and polymer materials.
[0004] A Chinese patent with publication number CN107986739B discloses a red mud slag building material and a preparation method thereof. Red mud slag is used to prepare raw material powder for red mud slag building materials, thereby improving the strength of the red mud slag building materials and reducing the production cost and difficulty of red mud slag resource utilization. However, it does not involve the problem of dissolution of heavy metals and high alkalinity substances in red mud, as well as the problem of water stability.
[0005] The Chinese patent with publication number CN108774043B discloses a high-mix red mud building material, which is to mix the red mud raw material and chromium slag evenly, mix the light-burned magnesium powder with the red mud and chromium slag premix evenly, add it to the magnesium chloride brine, stir for 2 to 5 minutes, add the modifier, continue stirring for 3 minutes, and add the water reducer; add water to the red mud and chromium slag composite material raw material powder, stir well to obtain the red mud magnesium gel composite material slurry, pour the red mud magnesium gel composite material slurry into a mold, demould to obtain the high-mix red mud building material, which has excellent flexural strength, compressive strength, and softening coefficient, and is suitable for most building environments. However, it does not involve the problem of high alkalinity and heavy metal dissolution in the red mud of the high-mix red mud building material.
[0006] However, the dissolution of high alkaline substances and heavy metal elements in red mud has always been a bottleneck restricting the large-scale use of red mud in engineering materials. Bayer red mud is more difficult to use due to its high alkalinity content and weak activity. However, 95% of red mud in industry is Bayer red mud. Therefore, how to efficiently and reasonably utilize red mud and solidify the high alkaline substances and heavy metals in it without dissolving has become a technical problem in this field.
[0007] On the other hand, the surface of modern cities is increasingly covered by buildings and concrete. The densification of this surface material makes it difficult for atmospheric precipitation to penetrate into the ground in time, increasing surface runoff and insufficient drainage, causing environmental problems such as waterlogging and urban surface subsidence, especially in rainy cities in the south. The semi-flexible pavement is a pavement formed by pouring cement mortar into a large-pore (void ratio of 20% to 25%) asphalt mixture matrix pavement and curing for a period of time. It has both higher flexibility than cement concrete and higher rigidity than asphalt concrete. Among them, the grouting material is generally composed of cement, water, fine sand and additives. During the hardening process, the hydrated cement interacts with the porous asphalt mixture, and the skeleton is added by connecting the voids in the porous asphalt mixture, thereby increasing the strength of the overall composite material. This kind of building composite material is in large demand, so how to use red mud as a raw material to prepare a good permeable cementitious composite material with good performance as a grouting material provides a new way for the comprehensive utilization of red mud. Therefore, how to efficiently and reasonably utilize red mud and solidify the highly alkaline substances and heavy metal elements therein without dissolving has become a technical problem that needs to be solved urgently. Summary of the invention
[0008] At present, there is not much research on the application of red mud-based cementitious composite materials and their application in semi-flexible pavement mixed slurries, especially in rainy and high-temperature areas, where there is a coupling effect between water and temperature, which puts higher requirements on the crack resistance, water damage resistance and water stability of semi-flexible pavements.
[0009] Therefore, in order to solve the above problems, the purpose of the present invention is to provide a red mud-based cementitious composite material, which has high permeability and low shrinkage, adjustable strength and low cost, can be poured into the base asphalt mixture, significantly improve the injection rate of the semi-flexible pavement material, and at the same time take into account the shrinkage characteristics of cement mortar, improve the mechanical properties and road performance of the semi-flexible pavement material, and extend the service life of the semi-flexible pavement.
[0010] To achieve the above object, the present invention provides a red mud-based cementitious composite material, wherein the addition amount of each component is calculated by weight: 60-80 parts of red mud, 8-10 parts of silicon dioxide, 8-15 parts of montmorillonite, 8-12 parts of mineral powder, 8-15 parts of cement, 1-2 parts of water reducer, and 7-15 parts of water;
[0011] The water reducer is a polycarboxylate water reducer or a naphthalene water reducer; the particle size of the silicon dioxide is 30 to 50 μm; the mineral powder is of S105 grade; and the cement is ordinary Portland cement or early strength Portland cement with a strength grade of 42.5 or 52.5.
[0012] According to the above weight ratio, the cementitious composite material obtained by directly mixing with red mud as the matrix cannot meet the corresponding requirements in terms of compression resistance, flexural resistance and other parameters. In addition, after being soaked in water, high alkaline substances and heavy metal ions will be dissolved, resulting in poor water stability.
[0013] This is because red mud itself has a high alkalinity, and because caustic soda solution is used to dissolve bauxite during the extraction of alumina, red mud is rich in Na alkali. The pH value of the alkaline solution is high and contains free heavy metal ions. At the same time, because red mud particles are fine, the specific surface area is large, and it has the same viscosity as clay soil, red mud has good plasticity, and because of its high compaction degree and stable crystal phase composition. It has low activity and is not easy to decompose at room temperature. Therefore, the use of red mud in roadbed fillers can ensure the stability of the structure. Therefore, we designed to modify red mud with sodium metasilicate, silicon dioxide and mineral powder, specifically:
[0014] S001, dissolve sodium metasilicate in water, heat to 40-60°C, add mineral powder, stir evenly to obtain slurry.
[0015] S002, adding silicon dioxide and red mud to the slurry, heating to 80°C, reacting for 3 to 4 hours, and obtaining a solid mixture, namely the red mud-based gelling material. The modified red mud-based gelling composite material generates a grid structure due to the polymerization reaction, so that the heavy metals in the red mud are sealed in the components of the red mud to a certain extent.
[0016] This is because the alkalinity in red mud can promote polymerization and activate the polymerization reaction between red mud and mineral powder. Mineral powder is both an activator and a matrix material for the reaction. Red mud contains a large amount of silicon and aluminum compounds. The mineral powder is composed of aluminosilicates and has high activity. Therefore, under the stimulation of strong alkalinity, the mineral powder can be polymerized with red mud to obtain a modified red mud component with high strength development and high resistance to chemical erosion. Alkali silicates react chemically with aluminosilicate precursors to form polymerized Si-O-Al bonds. The Si-O bonds and Al-O bonds in the raw materials are broken and reorganized under the action of alkaline catalysts. First, [SiO4] and [AlO4] in the aluminosilicate raw materials in the mineral powder are dissolved in an alkaline solution, and then under the action of an alkaline activator, they react with red mud to form a polymerization reaction. The monomers are dehydrated and condensed into aluminosilicate oligomers to form a Si-O-Al grid structure. However, when it is used as a pavement material, it is found that there are some shortcomings similar to ordinary concrete, such as high brittleness, poor toughness, and poor crack resistance. At the same time, due to the structure of red mud, the obtained red mud-based gelled composite material easily absorbs moisture, which makes the material's water resistance poor. After long-term immersion, the enclosed heavy metals are no longer stable to a certain extent and dissolution occurs.
[0017] In order to solve the problems of high brittleness, poor toughness, poor crack resistance, water absorption and slow dissolution, red mud is further modified as follows:
[0018] S101, in a reaction kettle equipped with a stirring blade, a thermometer, and a condenser, vinyl trimethoxysiloxane, dimethyl dimethoxysiloxane and aniline methyl triethyl siloxane are mixed with ethanol, stirred evenly, deionized water is added as a reaction solvent, stirred at room temperature for 1 hour until the solution is clear, and then diluted phosphoric acid is added dropwise, and the temperature is raised to 30-40°C for reaction for 18-20 hours. After the reaction stops, the acid-water layer is separated by standing for 60-80 minutes, and the acid-water layer is washed with water several times until it is neutral, and the small molecules and other substances remaining in the reaction system are removed, so as to obtain a polymer matrix with a molecular weight of 10,000-20,000; the mass ratio of the vinyl trimethoxysiloxane, dimethyl dimethoxysiloxane and aniline methyl triethyl siloxane is 1:1:2.
[0019] The first polymer with a molecular weight of 10,000 to 20,000 is preferably used as the matrix. The main reason is that if the molecular weight of such a high molecular weight polymer matrix is too small, the cross-linking network is insufficient, and the porosity is small, so that it cannot load too many small molecular substances, it will lead to its loading rate being too low, and the obtained matrix is too dense, further making the gel composite material insufficient in expansion performance and water permeability due to insufficient loading rate, while the molecular weight is too large, too many holes are formed, and the porosity is too high, so that the strength and compressive resistance of the formed gel composite material are insufficient. The first polymer directly connects the alkyl and phenyl groups to the same silicon atom during synthesis, and this molecular weight range makes the cross-linking network more and denser. At the same time, when it is combined with the inorganic layer at high temperature, there is still a certain porosity, so that the large particles can effectively combine with silicon oxygen. The porosity of the gel composite material is further changed by filling with large and small particles, and the mechanical strength of the gel composite material is enhanced, and its toughness is significantly improved, and the crack resistance is enhanced.
[0020] S102, blending silica and a first polymer matrix with a molecular weight of 10,000 to 20,000 in an alcohol ether solution by a solution blending method, stirring at high speed for 60 to 90 minutes, so that the silica is also fully cross-linked in the polymer matrix. Calcining it at a high temperature of 300° C. for 2 to 3 hours to obtain a second polymer matrix, wherein the mass ratio of the silica to the first polymer matrix is 1:8 to 10;
[0021] The introduction of silica is to introduce small particles into the matrix of the first polymer and fill them into the cavities of the cross-linked polymer. After high-temperature calcination, when the lattice transformation of silica occurs, it can fuse with the elements of the inorganic layer.
[0022] Silicone resin is a semi-inorganic and semi-organic polymer with -Si-O-Si- as the main chain. Under certain conditions, it will undergo a cross-linking reaction to form a three-dimensional network structure. When mixed with silica powder, this three-dimensional network structure will encapsulate the powder particles, forming a layered structure with a certain shape and strength. When the temperature rises to 300℃ for sintering, the added silicone resin main chain will decompose and remain in the form of -Si-OC-. The side chain groups of silicone resin are oxidized and decomposed into CO2 and H2O small molecular gases. The continuous overflow of these gases causes the sintered sample to expand in volume. Si-OH reacts nucleophilically with the Si atoms on the main chain, and pyrolysis obtains linear and annular skeletons, while the side chains form many hole structures.
[0023] Further, the red mud is activated and reacted with the second polymer, specifically:
[0024] S103, calcining the red mud at 300° C. for 1 to 2 hours, controlling its moisture content to 15 to 20%, and then crushing it with a solid crusher, passing it through a vibrating sieve with a mesh size of 1 mm, to obtain activated red mud;
[0025] The purpose of activating and crushing red mud is not only to ensure that the red mud can be evenly mixed with the additives and have the same reaction degree during the sample preparation process, but also to reduce the error caused by the non-uniform red mud particle size. The structure of the aluminosilicate crystals in the activated red mud changes, making the active silicon and aluminum substances easier to depolymerize, so that more active substances in the red mud can undergo hydration reactions, thereby improving the mechanical properties of the polymer obtained by the polymerization reaction.
[0026] S104, after dissolving sodium metasilicate in water, heat it to 40-60°C, add mineral powder, stir evenly, and obtain slurry. Add the second polymer and red mud to the slurry, heat it to 80°C, react for 3-4 hours, obtain a solid mixture, heat it to 150-200°C, stir, and continue to react for 1-2 hours to obtain red mud agglomerates. Red mud agglomerates generate a cross-linked three-dimensional grid structure due to the polymerization reaction, so that the metal elements in the red mud are firmly solidified in the three-dimensional grid structure, so that it changes from a free state to a stable state.
[0027] The mass ratio of the second polymer matrix, mineral powder and red mud is (10-15):
[0028] (8-12): (60-80), the mass concentration of the sodium metasilicate solution is 5%, and the mass of the sodium metasilicate solution accounts for 8% of the total mass of the solid matter.
[0029] Under the stimulation of a strong alkaline environment, the organic functional groups in the mineral powder and polymer and the red mud undergo a cross-linking reaction to generate a large number of Si-O-Al grid structures. The three-dimensional network structure formed by the second polymer continues to break as the reaction proceeds, resulting in an increase in the metal diffusion rate of the inorganic layer sandwiched in the middle, which promotes the continuous transformation between particles. And as the reaction proceeds, the particles fit into the three-dimensional grid structure, making the combination between the inorganic layer particles and the organic bottom layer more dense. And because the red mud microstructure is relatively loose, there are many gaps between the particles, and it has a cemented pore frame structure. Therefore, the loose porous structure can absorb a large number of siloxane groups, thereby intensifying cross-linking, and then reorganizing into a cross-linked dense Si-O-Al grid structure.
[0030] The untreated red mud sample has a loose microstructure, showing blocky and flaky particle structures, with many holes and cracks. The sample structure is loose and not dense, forming voids in aggregates, voids in aggregates and voids in agglomerates. Figure 2 This is consistent with the poor mechanical properties of the untreated red mud sample. As for the modified red mud powder sample with S105 mineral powder added, it can be seen that the microstructure of the sample is still basically blocky and flake particles, but some parts of the structure are connected by agglomerates, and it can be seen that polymers are produced. Figure 3As for the red mud agglomerate sample modified by adding mineral powder and a first polymer with a molecular weight of 10,000 to 20,000 polymerized with silicone resin as the matrix and cross-linking silica to obtain a second polymer matrix, the sample has almost no block and flaky structure, the pores and cracks are closely connected by the agglomerates, the sample structure is dense, and there are many micropores. Figure 1 This is also consistent with the results that the specimens exhibit good strength and other mechanical properties.
[0031] The Si-O-Al or Si-O-Si structure in the red mud agglomerates is due to the addition of the second polymer matrix cross-linked by S105 mineral powder and silica, which changes or activates the charge distribution in the red mud-mineral powder and forms a stable bond. With the increase of Si-O-Al grid content, the yield stress of red mud-based composite materials increases. The continuously enhanced red mud-based polymer materials all show a higher elastic modulus and a lower porosity ratio. There is an effective interfacial bonding between Si-O-Si and the siloxane organic skeleton. This makes the red mud agglomerates have higher toughness, indicating that under the action of the second polymer matrix, the red mud agglomerates have higher stability and durability, and the improvement effect on the brittleness of the red mud agglomerates is more significant.
[0032] The main reason is that the second polymer matrix reinforces the red mud and mineral powder in the process of fracture and re-bridging, and the formation of active functional clusters of the second polymer leads to the emergence of a bridging mechanism in the red mud and mineral powder composite material, which acts as a bridge to cross the microcracks caused by stress and prevent them from expanding in the matrix. The debonding, sliding and pulling out of the second polymer consumes a lot of energy, which could have been used to generate cracks. Therefore, the addition of siloxane polymer significantly improves the toughness of red mud aggregates.
[0033] In addition, red mud is easy to agglomerate, and fine particles agglomerate with each other to form coarse particles. In fact, fine particles make it easier for Si4+ in red mud to leach out, forming more gel materials. At the same time, fine particles also have a filling effect; while coarse particles are more likely to play a cementing role in cementitious materials. Moreover, the presence of iron oxide and titanium dioxide in red mud will also promote the formation of hydration products under alkaline conditions, densify the microscopic cross-linked grid structure, and thus improve the mechanical properties of red mud aggregates.
[0034] At this time, according to the chemical composition, mineral composition and physical properties of red mud, the compatibility of organic and inorganic compounds in the synthesis process makes the red mud activated into an active filler. Its surface is covered with an organic long-chain molecular layer due to physical and chemical effects, and it changes from hydrophilic to organic. Improve processing performance, improve the physical properties, mechanical strength, light resistance and aging resistance of synthetic materials. At the same time, because of the change from hydrophilic to organic, the red mud agglomerates change from water-absorbing to water-permeable gelling materials with excellent water resistance. In order to further improve the overall water resistance of the composite material.
[0035] Further, the montmorillonite is modified, specifically:
[0036] Calcium-based montmorillonite is selected, and deionized water is added to the calcium-based montmorillonite. Dilute phosphoric acid is added and stirred evenly to make the calcium-based montmorillonite fully dispersed in the dilute phosphoric acid solution. The temperature is raised to 80°C, octadecylamine polyoxyalkylene ether diquaternary ammonium salt is added, the mixture is fully stirred, and the mixture is reacted for 1 to 2 hours to obtain a suspension of the calcium-based montmorillonite. The suspension is taken out and centrifuged at a speed of 3000 rpm, and the suspension is washed with deionized water for 2 to 3 times to remove the phosphoric acid. The mixture is centrifuged again, and a solid mixture at the bottom is taken out, dried and ground at 80°C, and then sieved to obtain an oleophilic calcium-based montmorillonite with a particle size of 0.3 to 0.5 μm. The mass ratio of the octadecylamine polyoxyalkylene ether diquaternary ammonium salt to the calcium-based montmorillonite is 1:3 to 4.
[0037] The modified oleophilic calcium-based montmorillonite no longer swells when it meets water, improves the water absorption of the composite material, and becomes more stable to water. In addition, due to the microporous structure of montmorillonite, the formed gel has tortuous three-dimensional micropores. This structure allows the water to seep out through the microporous structure of the gel when water accumulates, thereby making the gel highly permeable and greatly enhancing the water resistance of the composite material. At the same time, the diquaternary ammonium salt will also be loaded in the interlayer structure of montmorillonite, which can play a role in adsorbing heavy metals. It can stimulate the alkaline substances in red mud and promote the adsorption of red mud particles. It can promote the change of heavy metals from an effective state to a stable state, effectively reducing the effectiveness and dissolution concentration of heavy metals. The combination of red mud aggregates and organic matter can play a role in adsorbing heavy metal ions in the soil. In addition to being able to solidify heavy metals, the ability to adsorb heavy metal ions is significantly enhanced. The synergistic effect of red mud aggregates and their synergy can play a role in permeability and water purification, but will not cause pollution to the environment.
[0038] Finally, the addition amount of each component is calculated by weight: 60-80 parts of red mud agglomerates, 8-15 parts of oleophilic calcium-based montmorillonite, 8-15 parts of cement, 1-2 parts of water reducer, and 7-15 parts of water;
[0039] S201, mixing: adding oleophilic calcium-based montmorillonite and cement to red mud agglomerates cooled to 30-40° C., stirring and mixing thoroughly, adding water, and continuing to stir for 5 minutes to fully mix the materials to obtain a red mud-based gelled composite material slurry;
[0040] S202, molding: pouring the red mud-based cementitious composite material slurry into a 40×40×160 mm standard test mold, fully shaking and molding, curing for 24 hours and then demolding, and naturally curing after demolding to obtain a fully quantified cementitious composite material based on red mud;
[0041] Furthermore, a semi-flexible pavement material with good water permeability is also provided, specifically:
[0042] S203, adding fine sand and water to the red mud-based cementitious composite material slurry; stirring to obtain a uniform slurry, that is, obtaining the slurry material for semi-flexible pavement; pouring it into a porous asphalt mixture, and finally obtaining a semi-flexible pavement material with good water permeability; the fine sand is yellow sand, river sand or quartz sand, and its maximum particle size is 0.4 mm, and its fineness modulus is 1.4-0.8. The slurry material for semi-flexible pavement is obtained, and it is poured into a porous asphalt mixture, and finally obtaining a semi-flexible pavement material with good water permeability.
[0043] In the prior art, red mud is used together with lime and cement, which cannot effectively lock the alkaline substances in red mud or saponified residue, resulting in the dissolution of calcium hydroxide and heavy metal ions, which creates environmental hazards. Compared with the prior art, the invention has the following beneficial effects:
[0044] 1. The present invention provides a fully quantitative treatment method for red mud, which can consume a large amount of red mud waste to prepare a cementitious composite material, which can be directly used for paving roads, or made into a slurry material for semi-flexible pavement, which is poured into a porous asphalt mixture and finally made into a semi-flexible pavement material with good water permeability. The method is safe, environmentally friendly, and has a large consumption.
[0045] 2. The present invention prepares a fully quantified gelled composite material based on red mud. First, the red mud is activated at high temperature, and then a first polymer with a molecular weight of 10,000 to 20,000 is polymerized with a silicone resin as a matrix and a second polymer matrix is obtained by cross-linking silica. The activated red mud is modified to prepare red mud agglomerates. Through holes are formed inside the red mud agglomerates, and the polymer matrix polymerized with silicone resin can promote the cross-linking of inorganic metal elements in the red mud agglomerates, forming an organic long-chain molecular layer on the surface of the red mud, changing from hydrophilic to organic, on the one hand, avoiding impurities from clogging the through holes in the red mud during the mixing process, and on the other hand, converting the heavy metal elements in the red mud from a free state to a fixed state, firmly locking the metal elements, and during the soaking process, no high-alkali substances and heavy metals will be dissolved. The surface of red mud polymer has hydroxyl, amine and epoxy groups. These oxygen-containing groups form a cage-like organic film, which wraps the red mud particles and makes them water-resistant, thereby locking the metal elements. During use, it can prevent the overflow of water-soluble alkaline substances and heavy metal ions in red mud or saponified residue. Because the silicone resin polymer cross-links silica and releases small molecular gases on the polymer matrix due to cracking, a large number of through holes are formed in the system, thereby improving the water permeability of the product; at the same time, silica undergoes crystal transformation at high temperature, further improving the shrinkage problem of the slurry, and can improve compressive strength, impact resistance and seismic resistance, reducing the shrinkage rate of the gel composite material; at the same time, it changes the hydrophilicity of the contact angle of the capillary wall, thereby increasing the permeability of the composite material, and at the same time, it can increase the amount of red mud, improve processing performance, and improve the physical properties, mechanical strength and water resistance of the composite material. It changes the shortcomings of traditional inorganic gelling materials such as poor mechanical properties, water resistance, and poor toughness.
[0046] 3. The fully quantified red mud-based gelled composite material prepared by the present invention not only does not cause the dissolution of high-alkali substances and heavy metals, but also can play the role of water permeability and water purification because of its dense three-dimensional network structure with a certain porosity and the synergistic effect of the oleophilic calcium-based montmorillonite.
[0047] 4. Through the cross-linked matrix of siloxane resin and silicon dioxide, the mineral powder acts synergistically to increase the yield stress and apparent viscosity of the material, so that a three-dimensional network structure is formed between the prepared red mud agglomerates, the workability, compatibility and dispersibility of the material are improved, and the physical and mechanical properties of the material are not affected at the same time, and the high temperature stability, low temperature crack resistance, fatigue resistance and water stability of the semi-flexible pavement material are improved. Compared with the prior art, the modulus of cement mortar can be greatly reduced, the cement mortar can be made soft, the flexural strength can be improved, and the compression-folding ratio can be reduced. Not only does the semi-flexible pavement cement-based mortar have good fluidity, the rheological properties of the entire system are good, the mechanical properties are good, it has good high temperature rutting resistance, low temperature crack resistance, water damage resistance, and fatigue resistance, and can extend the service life of the pavement. The cementitious composite material of the present invention has considerable flexural tensile strength and compressive strength, its flexural strength can reach more than 5.0MPa, and the corresponding compressive strength can reach 45MPa, has good matching, good uniformity, no stratification and segregation phenomenon, can ensure that the base slurry is uniform and stable during the construction time, so as to play a coordinated role. BRIEF DESCRIPTION OF THE DRAWINGS
[0048] Figure 1 , a 3000-fold magnified electron microscope scanning image of the red mud agglomerates prepared in Example 1;
[0049] Figure 2 , 3000 times magnified electron microscope scanning image of red mud;
[0050] Figure 3 , an electron microscope scan of the gelled material obtained by mixing red mud and mineral powder at 3000 times magnification. DETAILED DESCRIPTION
[0051] The present invention will be further described below in conjunction with specific embodiments. It should be understood that these embodiments are only used to illustrate the present invention and are not intended to limit the scope of the present invention. In addition, it should be understood that after reading the content described in the present invention, those skilled in the art may make various changes or modifications to the present invention, and these equivalent forms fall within the scope limited by the appended claims of the application equally.
[0052] Example 1
[0053] A fully quantified cementitious composite material based on red mud must first be modified by:
[0054] In a reaction kettle equipped with a stirring paddle, a thermometer, and a condenser, 4 parts of vinyl trimethoxysiloxane, 4 parts of dimethyl dimethoxysiloxane, and 8 parts of aniline methyl triethylsiloxane are mixed with an appropriate amount of ethanol, stirred evenly, a certain mass of deionized water is added as a reaction solvent, stirred at room temperature for 1 hour until the solution is clear, and then 1 part of dilute phosphoric acid is added dropwise, and the temperature is raised to 40°C for reaction for 20 hours; after the reaction stops, the acid and water layers are separated by standing for 60 minutes, and the acid and water layers are washed with water several times until neutral, and small molecules and other substances remaining in the reaction system are removed, so as to obtain a first polymer matrix with a molecular weight of 18129; further, 2 parts of silica and 16 parts of the first polymer matrix are mixed in an alcohol ether solution by a solution blending method, and stirred at high speed for 90 minutes, so that the silica is also fully cross-linked in the polymer matrix; it is calcined at a high temperature of 300°C for 3 hours to obtain a second polymer matrix;
[0055] 80 parts of red mud were calcined at 300°C for 2 hours, with a water content of 18%, and then crushed with a solid crusher and passed through a 1mm mesh vibrating sieve to obtain activated red mud; sodium metasilicate was dissolved in water to obtain 6.2 parts of a 5% sodium metasilicate solution, which was heated to 60°C, and 8 parts of mineral powder were added and stirred to obtain a slurry; 10 parts of a second polymer matrix and 60 parts of red mud were added to the slurry, heated to 80°C, reacted for 4 hours, and obtained a solid mixture, which was heated to 150°C and continued to react for 2 hours to obtain red mud agglomerates;
[0056] Further, oleophilic calcium-based montmorillonite is prepared, specifically:
[0057] 10 parts of calcium montmorillonite are selected, the calcium montmorillonite is added to 50 parts of deionized water, 1 part of dilute phosphoric acid is added and stirred evenly, so that the calcium montmorillonite is fully dispersed in the dilute phosphoric acid solution, the temperature is raised to 80° C., 2.5 parts of octadecylamine polyoxyalkylene ether diquaternary ammonium salt are added, the mixture is fully stirred, and the mixture is reacted for 2 hours to obtain a suspension of calcium montmorillonite, the suspension is taken out and centrifuged at a speed of 3000 rpm, the suspension is washed with deionized water for 3 times to remove the phosphoric acid, and the mixture is centrifuged again, the solid mixture at the bottom is taken out, dried and ground at 80° C., and then sieved to obtain an oleophilic calcium montmorillonite with a particle size of 0.3 to 0.5 μm;
[0058] Finally, a fully quantified cementitious composite material based on red mud was prepared, specifically: the addition amount of each component was calculated by weight: 70 parts of red mud aggregates, 10 parts of oleophilic calcium-based montmorillonite, 8 parts of ordinary Portland cement, 1 part of polycarboxylate water reducer, and 12 parts of water;
[0059] Add oleophilic calcium-montmorillonite and ordinary Portland cement to red mud agglomerates cooled to 30°C and mix them thoroughly, add polycarboxylic acid water reducer and water, and continue stirring for 5 minutes to fully mix the materials to obtain red mud-based cementitious composite material slurry; pour the red mud-based cementitious composite material slurry into a 40×40×160mm standard test mold, fully shake to form, demold after curing for 24 hours, and naturally cure after demolding to obtain a fully quantified cementitious composite material based on red mud.
[0060] A semi-flexible pavement material with good water permeability is also provided, specifically:
[0061] Add fine sand and water to the red mud-based gel composite material slurry; stir to obtain a uniform slurry, that is, the slurry material for the semi-flexible pavement; pour the slurry into a porous asphalt mixture, and finally obtain a semi-flexible pavement material with good water permeability.
[0062] Example 2
[0063] A fully quantified cementitious composite material based on red mud must first be modified by:
[0064] In a reaction kettle equipped with a stirring paddle, a thermometer, and a condenser, 4 parts of vinyl trimethoxysiloxane, 4 parts of dimethyl dimethoxysiloxane, and 8 parts of aniline methyl triethylsiloxane are mixed with an appropriate amount of ethanol, stirred evenly, a certain mass of deionized water is added as a reaction solvent, stirred at room temperature for 1 hour until the solution is clear, and then 1 part of dilute phosphoric acid is added dropwise, and the temperature is raised to 40°C for reaction for 20 hours; after the reaction stops, the acid and water layers are separated by standing for 60 minutes, and the acid and water layers are washed with water several times until neutral, and small molecules and other substances remaining in the reaction system are removed, so as to obtain a first polymer matrix with a molecular weight of 15862; further, 2 parts of silica and 16 parts of the first polymer matrix are mixed in an alcohol ether solution by a solution blending method, and stirred at high speed for 90 minutes, so that the silica is also fully cross-linked in the polymer matrix; it is calcined at a high temperature of 300°C for 2 hours to obtain a second polymer matrix;
[0065] 60 parts of red mud were calcined at 300°C for 2 hours, with a water content of 16%, and then crushed with a solid crusher and passed through a vibrating sieve with a mesh diameter of 1 mm to obtain activated red mud; 100 parts of 5% sodium metasilicate solution were obtained by dissolving sodium metasilicate in water, heated to 60°C, added with 12 parts of mineral powder, and stirred evenly to obtain a suspension; 15 parts of a second polymer matrix and 60 parts of red mud were added to the suspension, heated to 80°C, reacted for 4 hours, and the reaction product was taken out for solid-liquid separation to obtain a solid mixture, heated to 180°C, and continued to react for 2 hours to obtain red mud agglomerates;
[0066] Further, oleophilic calcium-based montmorillonite is prepared, specifically:
[0067] 9 parts of calcium montmorillonite are selected, the calcium montmorillonite is added to 50 parts of deionized water, 1 part of dilute phosphoric acid is added and stirred evenly, so that the calcium montmorillonite is fully dispersed in the dilute phosphoric acid solution, the temperature is raised to 80° C., 3 parts of octadecylamine polyoxyalkylene ether diquaternary ammonium salt are added, the mixture is fully stirred, and the reaction is performed for 2 hours to obtain a suspension of calcium montmorillonite, the suspension is taken out and centrifuged at a speed of 3000 rpm, the suspension is washed with deionized water for 3 times to remove the phosphoric acid, and the mixture is centrifuged again, the solid mixture at the bottom is taken out, dried and ground at 80° C., and then sieved to obtain an oleophilic calcium montmorillonite with a particle size of 0.3 to 0.5 μm;
[0068] Finally, a fully quantified cementitious composite material based on red mud was prepared, specifically, according to the addition amount of each component in parts by weight: 75 parts of red mud aggregates, 8 parts of oleophilic calcium-based montmorillonite, 8 parts of early strength silicate cement, 1 part of polycarboxylate water reducer, and 8 parts of water;
[0069] Add oleophilic calcium-based montmorillonite and early-strength silicate cement to red mud agglomerates cooled to 30°C and mix them thoroughly, add polycarboxylic acid water-reducing agent and water, and continue stirring for 5 minutes to fully mix the materials to obtain red mud-based cementitious composite material slurry; pour the red mud-based cementitious composite material slurry into a 40×40×160mm standard test mold, fully shake to form, demold after curing for 24 hours, and naturally cure after demolding to obtain a fully quantified cementitious composite material based on red mud.
[0070] A semi-flexible pavement material with good water permeability is also provided, specifically:
[0071] Add fine sand and water to the red mud-based gel composite material slurry; stir to obtain a uniform slurry, that is, the slurry material for the semi-flexible pavement; pour the slurry into a porous asphalt mixture, and finally obtain a semi-flexible pavement material with good water permeability.
[0072] Example 3
[0073] A fully quantified cementitious composite material based on red mud must first be modified by:
[0074] In a reaction kettle equipped with a stirring paddle, a thermometer, and a condenser, 4 parts of vinyl trimethoxysiloxane, 4 parts of dimethyl dimethoxysiloxane, and 8 parts of aniline methyl triethylsiloxane are mixed with an appropriate amount of ethanol, stirred evenly, a certain mass of deionized water is added as a reaction solvent, stirred at room temperature for 1 hour until the solution is clear, and then 1 part of dilute phosphoric acid is added dropwise, and the temperature is raised to 40°C for reaction for 20 hours; after the reaction stops, the acid and water layers are separated by standing for 60 minutes, and the acid and water layers are washed with water several times until neutral, and small molecules and other substances remaining in the reaction system are removed, so as to obtain a first polymer matrix with a molecular weight of 12074; further, 2 parts of silica and 16 parts of the first polymer matrix are mixed in an alcohol ether solution by a solution blending method, and stirred at high speed for 90 minutes, so that the silica is also fully cross-linked in the polymer matrix; it is calcined at a high temperature of 300°C for 3 hours to obtain a second polymer matrix;
[0075] 65 parts of red mud were calcined at 300°C for 2 hours, with a water content of 20%, and then crushed with a solid crusher, and passed through a vibrating sieve with a mesh diameter of 1 mm to obtain activated red mud; sodium metasilicate was dissolved in water to obtain 100 parts of a 5% sodium metasilicate solution, which was heated to 60°C, and 9 parts of mineral powder were added and stirred to obtain a suspension; 10 parts of a second polymer matrix and 70 parts of red mud were added to the suspension, heated to 80°C, reacted for 4 hours, and the reaction product was taken out for solid-liquid separation to obtain a solid mixture, which was heated to 150°C and continued to react for 2 hours to obtain red mud agglomerates;
[0076] Further, oleophilic calcium-based montmorillonite is prepared, specifically:
[0077] 9 parts of calcium montmorillonite are selected, the calcium montmorillonite is added to 50 parts of deionized water, 1 part of dilute phosphoric acid is added and stirred evenly, so that the calcium montmorillonite is fully dispersed in the dilute phosphoric acid solution, the temperature is raised to 80° C., 3 parts of octadecylamine polyoxyalkylene ether diquaternary ammonium salt are added, the mixture is fully stirred, and the reaction is performed for 2 hours to obtain a suspension of calcium montmorillonite, the suspension is taken out and centrifuged at a speed of 3000 rpm, the suspension is washed with deionized water for 3 times to remove the phosphoric acid, and the mixture is centrifuged again, the solid mixture at the bottom is taken out, dried and ground at 80° C., and then sieved to obtain an oleophilic calcium montmorillonite with a particle size of 0.3 to 0.5 μm;
[0078] Finally, a fully quantified cementitious composite material based on red mud was prepared, specifically, according to the addition amount of each component in parts by weight: 60 parts of red mud aggregates, 15 parts of oleophilic calcium-based montmorillonite, 15 parts of early strength silicate cement, 2 parts of naphthalene-based water reducer, and 8 parts of water;
[0079] Add oleophilic calcium-based montmorillonite and early-strength silicate cement to red mud agglomerates cooled to 30°C and mix them thoroughly, add a naphthalene-based water reducer, add water, and continue stirring for 5 minutes to fully mix the materials to obtain a red mud-based cementitious composite material slurry; pour the red mud-based cementitious composite material slurry into a 40×40×160mm standard test mold, fully shake it to form, demold it after curing for 24 hours, and naturally cure it after demolding to obtain a fully quantified cementitious composite material based on red mud.
[0080] A semi-flexible pavement material with good water permeability is also provided, specifically:
[0081] Add fine sand and water to the red mud-based gel composite material slurry; stir to obtain a uniform slurry, that is, the slurry material for the semi-flexible pavement; pour the slurry into a porous asphalt mixture, and finally obtain a semi-flexible pavement material with good water permeability.
[0082] Comparative Example 1: red mud, silicon dioxide, montmorillonite and mineral powder were not modified, and the amounts used were the same as in Example 1, and the others were the same as in Example 1;
[0083] Comparative Example 2: Red mud, silicon dioxide and mineral powder were not modified, and the amounts used were the same as in Example 1, and the others were the same as in Example 1;
[0084] Comparative Example 3: The grouting material involved in Example 2 of the grouting material for semi-flexible pavement disclosed in the Chinese invention patent with publication number CN111943614B.
[0085] Experimental effect comparison data
[0086] 1. Scanning electron microscopy
[0087] The morphology of the samples was observed using a field emission scanning electron microscope of the FEI Nova NanoSEM450. Before the test, the red mud aggregates in Example 1 were placed for 1 day and then the samples were evenly dispersed on the conductive glue. The parameters of the scanning electron microscope were adjusted, and the acceleration voltage, detection current of 10mA, resolution of 1.7nm, and magnification of 3000 times were set. The morphology is shown in Figure 1 .
[0088] The untreated red mud was dried to a moisture content of 15%, crushed and evenly dispersed on the conductive glue, and the parameters of the scanning electron microscope were adjusted to set the acceleration voltage, detection current 10mA, resolution 1.7nm, and magnification 3000 times; the morphology is shown in Figure 2
[0089] 8 parts of mineral powder, 60 parts of red mud dried to 15% moisture content, and crushed red mud were mixed with 5.4 parts of 5% sodium metasilicate solution to form a gelled substance. After drying for 1 day, the gelled substance was evenly dispersed on the conductive glue. The parameters of the scanning electron microscope were adjusted, and the acceleration voltage, detection current 10mA, resolution 1.7nm, and magnification 3000 times were set. The morphology is shown in Figure 3 .
[0090] from Figure 2 It can be seen that the untreated red mud sample has a loose microstructure, showing a block and flaky particle structure, with many holes and cracks. The sample structure is loose and not dense, forming multiple large agglomerate voids, aggregate voids and agglomerate voids. Therefore, it can be seen that the untreated red mud has strong water absorption and poor water stability. As for the gelled material obtained by adding the modified red mud powder with S105 mineral powder, it can be seen that the microstructure of the sample is still basically block and flaky particles, but some of the structures are connected by agglomerates, and it can be seen that polymers are produced. Figure 3 .
[0091] As for the red mud agglomerate sample modified by adding mineral powder and a first polymer with a molecular weight of 10,000 to 20,000 polymerized with silicone resin as the matrix and cross-linking silica to obtain a second polymer matrix, the sample has almost no block and flaky structure, the pores and cracks are closely connected by the agglomerates, the sample structure is dense and uniform, the spatial structure is more complex, and there are many uniformly distributed micropores, as shown in Fig. Figure 1 Therefore, the modified red mud aggregates have better water permeability and better mechanical properties.
[0092] 2. Heavy metal element dissolution test
[0093] 100 g of red mud agglomerates were crushed and placed in 500 mL of 10% dilute hydrochloric acid, heated to 80 ° C, and soaked for 90 days. The supernatant was filtered and placed in an ICPMS inductively coupled plasma mass spectrometer for detection of the contents of five heavy metal elements, Cd, Cr, Mo, Pb and Zn. See Table 1. The inductively coupled plasma mass spectrometer was NexION 300X, with an ion emission power of 1300 W, a plasma flow rate of 15 L / min, an auxiliary gas flow rate of 0.5 L / min, a nebulizer flow rate of 0.9 L / min, an injection volume of 15 mL / min, and a pulse stage voltage of 1000 V.
[0094] 100 g of red mud aggregates were crushed and placed in 500 mL of deionized water, heated to 80 °C, and soaked for 2 days. The supernatant was filtered and the alkali content and pH value were measured, as shown in Table 1.
[0095] It can be seen from Table 1 that the dissolution amount of the five heavy metals in Examples 1-3 is much lower than that in Comparative Examples 1-2, and no dissolution of the two heavy metals Mo and Pb was detected. This is because the red mud agglomerates in Examples 1-3 are compatible with organic and inorganic compounds during the synthesis process, which activates the red mud into an active filler. Its surface is coated with an organic long-chain molecular layer due to physical and chemical effects, and changes from hydrophilic to organic, and forms a tightly cross-linked three-dimensional grid structure, so that the metal ions fit into the three-dimensional grid structure, making the combination between the particles of the inorganic layer and the organic bottom layer more dense, so that the free metal elements form a stable solidified structure and are almost not dissolved. The metal ions in the red mud in Comparative Examples 1-2 are not completely solidified, and are easily dissolved after high-temperature immersion. Therefore, when the gelled composite material made of red mud agglomerates is used in large quantities as a pavement material, it will not cause secondary pollution to the surrounding water environment.
[0096] Table 1 Red mud aggregate heavy metal dissolution and alkali content test record (mg / kg)
[0097] Sample Cd element Cr element Mo element Pb element Zn element Alkali content pH Example 1 0.04 0.01 - - 0.17 249,7 7.3 Example 2 0.05 0.03 - - 0.19 258.9 7.9 Example 3 0.03 0.02 - - 0.23 241.5 7.6 Comparative Example 1 71.63 601.81 78.08 120.19 318.84 1985.7 13.2 Comparative Example 2 65.19 529.15 61.19 113.73 258.91 1754.6 12.5
[0098] 3. Water permeability and water absorption test of cementitious composite materials based on full quantification of red mud
[0099] The products obtained in Examples 1 to 3 and Comparative Examples 1-3 were tested for water permeability, wherein Comparative Example 3 was to pour the grouting material involved in Example 2 of the semi-flexible pavement grouting material with the publication number CN111943614B into a 40×40×160mm standard test mold, fully shake it into shape, demould it after curing for 24 hours, and naturally cure it after demoulding. The obtained material was tested for water permeability and water absorption. The specific detection method is as follows: The water permeability coefficient test is carried out in accordance with the provisions of JC / T945, and the test water is deionized water. The water absorption rate is the water absorption after the obtained cementitious composite material is completely immersed in tap water for 24 hours. The test results are shown in Table 2. It can be seen from Table 2 that the cementitious composite material prepared in Examples 1-3 is not easy to absorb water, and has a strong water permeability function and a large number of connecting holes. Even if it rains heavily, rainwater can quickly penetrate the surface into the ground, which can effectively reduce the burden of the drainage system in rainy cities in the south. Although Comparative Example 3 also has good water resistance and very low water absorption, its water permeability is very poor, which easily causes rainwater retention and imposes a serious burden on the drainage system of rainy cities in the south.
[0100] Table 2 Water permeability test data record
[0101]
[0102] 4. Overall performance test of the fully quantified cementitious composite material based on red mud
[0103] Compressive strength test method: Refer to the T0506 method in the "Test Procedure for Cement and Cement Concrete for Highway Engineering" JTG3420-2020 to measure the compressive strength of the cementitious composite materials obtained in Examples 1-3 and Comparative Examples 1-3 at the corresponding ages. Prepare a 40mm×40mm×40mm cementitious material specimen block, cure it to the specified age of 3 hours and 7 days under standard curing conditions, and use a pressure testing machine to measure its compressive strength. The test data is shown in Table 3; it can be seen from the data records in Table 3 that the compressive strength growth rate of the cementitious composite materials in Examples 1-3 is relatively large, and its 3h compressive strength has reached 80% of the 1d compressive strength, which can effectively ensure the strength of the cementitious composite material and achieve the goal of early strength. Its final performance far exceeds the technical requirements of the T0506 method in JTG3420-2020. This is because it can be seen from Table 3 that the strength of the cementitious composite material made of unmodified red mud is far from enough, while Comparative Example 3 is a cementitious material made of ordinary materials without red mud, and its compressive strength is only about 70% of the strength of red mud agglomerates.
[0104] Flexural strength test method: Refer to the T0506 method in the "Test Procedure for Cement and Cement Concrete for Highway Engineering" JTG3420-2020 to measure the flexural strength of the cementitious composite materials obtained in Examples 1-3 and Comparative Examples 1-3. Prepare 40mm×40mm×160mm red mud-based cementitious material specimens, cure them to the specified age of 3 hours and 7 days under standard curing conditions, put them into the flexural fixture of a lever-type electric flexural testing machine, and measure the flexural strength. The test data is shown in Table 3; it can be seen from the data records in Table 3 that the flexural strength of the cementitious composite materials in Examples 1-3 is significantly higher than that of Comparative Example 3. This is because the organic polymer resin, as a collective, greatly improves the toughness of the cementitious material.
[0105] Shrinkage rate, pour the cementitious material into a test mold with staples installed at both ends, the size of the test mold is 25mm×25mm×280mm, and use a knife to scrape the surface, put it into a shrinkage curing box and cure it to the test age of 7 days, take it out and use a comparator to measure the length of the specimen, calculate the shrinkage rate, see Table 3; this is because the more cement is used, the more cement stone content, the greater the drying shrinkage. Therefore, the addition of red mud can reduce the amount of cement used, so that the shrinkage deformation of the cementitious material is reduced. Compared with comparative example 3, it has a better shrinkage rate, which further improves the mechanical properties of the cementitious material.
[0106] It can be seen from Table 3 that the fully quantified cementitious composite material based on red mud prepared by the present invention has good mechanical properties and durability. This is because the mineral powder acts synergistically to increase the yield stress and apparent viscosity of the material through the cross-linked matrix of silicone resin and silica, so that a three-dimensional network structure is formed between the prepared red mud agglomerates, which improves the workability and compatibility of the material. Its porous and dense structure will not only not affect the physical and mechanical properties of the material, but also enhance the flexural strength, compressive strength and water stability of the cementitious composite material. The red mud agglomerates obtained by cross-linking red mud with silica and high molecular polymer materials have a promoting effect on the mechanical properties and durability of the mortar, and have a coordinated and synergistic effect.
[0107] Table 3 Overall performance test of cementitious composite materials based on red mud full quantification
[0108]
[0109] In order to verify the performance of the fully-quantified cementitious composite material slurry based on red mud of the present invention, the inventors used the fully-quantified cementitious composite material slurry based on red mud prepared in Example 2 of the present invention, poured it into a large-void asphalt mixture, and carried out Marshall stability, high-temperature rutting resistance, flexural strength, and bending failure strain tests of the asphalt mixture in accordance with the requirements of the Technical Specifications for Highway Asphalt Pavement Construction (JTG F40-2004) of the Ministry of Transport. The test results show that the semi-flexible pavement with good water permeability formed by using the fully-quantified cementitious composite material slurry based on red mud of the present invention poured into a large-void asphalt mixture has good road performance. The main performance indicators are shown in Table 4. Its performance far exceeds the technical requirements of the semi-flexible pavement and can be used in a large number of pavement construction materials.
[0110] Table 4 Performance test results of semi-flexible pavement with good permeability
[0111]
[0112] The above description is only used to illustrate the technical solution of the present invention rather than to limit it. Any equal modifications and changes made to the technical solution of the present invention by ordinary persons in the art, as long as they do not deviate from the overall concept of the present invention, are still within the scope of the present invention.
Claims
1. A fully quantified cementitious composite material based on red mud, characterized by: The red mud-based fully quantified cementitious composite material comprises the following components in weight: 60 to 80 parts of red mud aggregates, 8 to 15 parts of oleophilic calcium-based montmorillonite, 8 to 15 parts of cement, 1 to 2 parts of water reducer, and 7 to 15 parts of water. The red mud agglomerates, wherein the red mud is high temperature activated red mud, are polymerized with silicone resin to form a first polymer with a molecular weight of 10,000 to 20,000 as a matrix and a second polymer matrix obtained by cross-linking silicon dioxide, and the activated red mud is modified to prepare red mud agglomerates; specifically: S101, in a reaction kettle equipped with a stirring blade, a thermometer, and a condenser, vinyl trimethoxysiloxane, dimethyl dimethoxysiloxane and aniline methyl triethylsiloxane are mixed with ethanol, stirred evenly, deionized water is added as a reaction solvent, stirred at room temperature for 1 hour until the solution is clear, and then diluted phosphoric acid is added dropwise, and the temperature is raised to 30-40° C. to react for 18-20 hours; after the reaction stops, the acid-water layer is allowed to stand for 60-80 minutes to separate the acid-water layer, and the small molecular substances remaining in the reaction system are removed after multiple water washing until neutral, so as to obtain a first polymer matrix with a molecular weight of 10,000-20,000; S102, blending silica and a first polymer matrix with a molecular weight of 10,000 to 20,000 in an alcohol ether solution by a solution blending method, stirring at high speed for 60 to 90 minutes, so that the silica is also fully cross-linked in the first polymer matrix; calcining the first polymer matrix at a high temperature of 300° C. for 2 to 3 hours to obtain a second polymer matrix; S103, calcining the red mud at 300° C. for 1 to 2 hours, controlling its moisture content to 15 to 20%, and then crushing it with a solid crusher, passing it through a vibrating sieve with a mesh size of 1 mm, to obtain activated red mud; S104, dissolving sodium metasilicate in water, heating to 40-60°C, adding mineral powder, stirring evenly to obtain slurry; adding the second polymer and red mud to the slurry, heating to 80°C, reacting for 3-4 hours to obtain a solid mixture, heating to 150-200°C, stirring, and continuing to react for 1-2 hours to obtain red mud agglomerates, wherein the mass concentration of the sodium metasilicate solution is 5%.
2. The fully quantified cementitious composite material based on red mud according to claim 1, characterized in that: The montmorillonite is a modified montmorillonite, specifically: Calcium-based montmorillonite is selected, and deionized water is added to the calcium-based montmorillonite. Dilute phosphoric acid is added and stirred evenly to make the calcium-based montmorillonite fully dispersed in the dilute phosphoric acid solution. The temperature is raised to 80°C, octadecylamine polyoxyalkylene ether diquaternary ammonium salt is added, the mixture is fully stirred, and the mixture is reacted for 1 to 2 hours to obtain a suspension of the calcium-based montmorillonite. The suspension is taken out and centrifuged at a speed of 3000 rpm, and the suspension is washed with deionized water for 2 to 3 times to remove the phosphoric acid. The mixture is centrifuged again, and a solid mixture at the bottom is taken out, dried and ground at 80°C, and then sieved to obtain an oleophilic calcium-based montmorillonite with a particle size of 0.3 to 0.5 μm. The mass ratio of the octadecylamine polyoxyalkylene ether diquaternary ammonium salt to the calcium-based montmorillonite is 1:3 to 4.
3. The fully quantified cementitious composite material based on red mud according to any one of claims 1 to 2, characterized in that: The preparation method of the fully quantified cementitious composite material based on red mud is as follows: the addition amount of each component is calculated by weight: 60-80 parts of red mud aggregates, 8-15 parts of oleophilic calcium-based montmorillonite, 8-15 parts of cement, 1-2 parts of water reducer, and 7-15 parts of water; S201, mixing: fully mixing red mud aggregates, oleophilic calcium-based montmorillonite, and cement to obtain raw material powder, adding water, and continuing to stir for 5 minutes to fully mix the materials to obtain red mud-based gelled composite material slurry; S202, molding: pour the red mud-based cementitious composite material slurry into a 40×40×160mm standard test mold, fully shake it to form, demould it after curing for 24 hours, and naturally cure it after demoulding to obtain a fully quantified cementitious composite material based on red mud.
4. The fully quantified cementitious composite material based on red mud according to claim 3, characterized in that: A semi-flexible pavement material with good water permeability is also provided, specifically: S203, adding fine sand and water to the red mud-based cementitious composite material slurry; stirring to obtain a uniform slurry, namely the slurry material for the semi-flexible pavement; pouring the slurry into a porous asphalt mixture, and finally obtaining a semi-flexible pavement material with good water permeability; the fine sand is yellow sand, river sand or quartz sand, with a maximum particle size of 0.4 mm and a fineness modulus of 1.4 to 0.
8.
5. The fully quantified cementitious composite material based on red mud according to claim 1, characterized in that: The water reducer is a polycarboxylate water reducer or a naphthalene water reducer; the particle size of the silicon dioxide is 30 to 50 μm; the mineral powder is of S105 grade; and the cement is ordinary Portland cement or early strength Portland cement with a strength grade of 42.5 or 52.
5.
6. The fully quantified cementitious composite material based on red mud according to claim 1, characterized in that: The mass ratio of the vinyl trimethoxysiloxane, dimethyl dimethoxysiloxane and aniline methyl triethylsiloxane is 1:1:
2.
7. The fully quantified cementitious composite material based on red mud according to claim 1, characterized in that: The mass ratio of the silicon dioxide to the first polymer matrix is 1:8-10; the mass ratio of the second polymer matrix, mineral powder and red mud is (10-15):(8-12):(60-80), and the mass of the sodium metasilicate solution accounts for 8% of the total mass of the solid matter.