Solvent violet 59 and preparation method thereof

Through three-stage stirring and liquid caustic soda dripping technology, combined with nano-silica powder and other additives, the difficulty in temperature rise and material flushing during the condensation stage in the production of Solvent Violet 59 has been solved, and the coloring rate and purity have been improved.

CN118745290APending Publication Date: 2024-10-08ANHUI QINGKERUIJIE NEW MATERIALS CO LTD
View PDF 0 Cites 2 Cited by

Patent Information

Application Number
CN202410729303.0
Authority / Receiving Office
CN · China
Patent Type
Applications(China)
Current Assignee / Owner
Filing Date
2024-06-06
Publication Date
2024-10-08

AI Technical Summary

Technical Problem

In the production process of Solvent Violet 59, there is difficulty in heating up during the condensation stage, which leads to the problem of excessive punching or phenol water, and the coloring rate and purity are low.

Method used

Three-stage stirring is used to control heat diffusion, and the stability of the dye is improved by gradually raising the temperature in the reaction kettle and dripping liquid caustic soda into the crystallization kettle, combined with additives such as nano-silica powder, polyvinylpyrrolidone and xylitol. and dispersion effects.

Benefits of technology

It achieves efficient heating during the condensation stage, avoids the problem of excessive punching and phenol water, improves the coloring rate of Solvent Violet 59 to more than 98%, and the product purity reaches more than 99%.

✦ Generated by Eureka AI based on patent content.

Smart Images

  • Figure BDA0004879722160000011
    Figure BDA0004879722160000011
Patent Text Reader

Abstract

The invention discloses solvent violet 59 and a preparation method thereof. The solvent violet 59 is prepared from the following raw materials in parts by weight: 45-60 parts of a 59 # violet crude product, 1-10 parts of an auxiliary agent and 40-60 parts of deionized water, the 59 # purple crude product is prepared from the following raw materials in parts by weight: 70 to 85 parts of phenol, 10 to 25 parts of 1, 4-diamino-2, 3-dichloroanthraquinone, 10 to 15 parts of potassium carbonate, 25 to 35 parts of liquid caustic soda and 20 to 35 parts of deionized water. In the preparation process, by adding the auxiliary agent compounded from the nano organic silicon powder, the polyvinylpyrrolidone and the xylitol, better thickening and dispersing effects can be achieved in dye dispersion, the stability and the optical performance of the dye are improved, the polyvinylpyrrolidone can enhance the binding power and the durability of the dye, and the dye has the advantages that the adhesion force of the dye can be improved, and the service life of the dye is prolonged. And the natural colloidal xylitol can be used as a thickening agent and a dispersing agent, so that the rheological property and the stability of the dye can be improved.
Need to check novelty before this filing date? Find Prior Art

Description

Technical Field

[0001] The invention relates to the technical field of dye production, and in particular to solvent violet 59 and a preparation method thereof. Background Art

[0002] Solvent Violet 59, also known as 1,4-diamino-2,3-diphenoxyanthraquinone, has a molecular formula of C 14 H8Cl2N2O2, with a molecular weight of 307.1315, is an important high-grade solvent dye used for ink and plastic coloring, and can also be used for transfer printing. It is also a disperse dye. After being commercialized by sand grinding with auxiliaries, it can be used for dyeing polyester and its blended fabrics. With the help of dispersants, it is uniformly dispersed in the dye liquor for dyeing, and can be used for coloring a variety of plastics and polyesters. Its structural formula is shown in (I):

[0003]

[0004] At present, the production process of solvent violet 59 has the problem of difficulty in heating up the condensation stage. Due to the excessively high alkali addition temperature or the excessively fast alkali addition speed, the problem of excessive material or phenol water is prone to occur in the production process. The coloring rate of solvent violet 59 on the market is generally 90-95%, the main content of the product is 80-90%, and the purity is average. Therefore, it is very necessary to develop a colorant solvent violet 59 that can increase the heating rate in the condensation stage, overcome the problem of excessive material or phenol water in the production process, and prepare a solvent violet 59 with high coloring rate and high purity and a preparation method thereof. Summary of the invention

[0005] In order to solve the problems mentioned in the above background technology, the present invention provides a solvent violet 59 and a preparation method thereof.

[0006] In order to achieve the above object, the present invention adopts the following technical solutions:

[0007] A solvent violet 59, which is made from the following raw materials in parts by weight:

[0008] 45-60 parts of 59# purple crude product, 1-10 parts of auxiliary agent and 40-60 parts of deionized water;

[0009] The 59# purple crude product is made from the following raw materials in parts by weight:

[0010] 70-85 parts of phenol, 10-25 parts of 1,4-diamino-2,3-dichloroanthraquinone, 10-15 parts of potassium carbonate, 25-35 parts of liquid caustic soda and 20-35 parts of deionized water.

[0011] Preferably, the preparation method of the 59# purple crude product comprises the following steps:

[0012] S1. Add phenol and 1,4-diamino-2,3-dichloroanthraquinone into a reaction kettle, and control the stirring speed to 75-80 r / min and the stirring time to 8-10 min;

[0013] S2, add potassium carbonate to the reactor, increase the stirring speed to 80-85r / min, stir for 10-12min, and heat to 180-200°C, then reduce the stirring speed to 60-65r / min, continue stirring for 5-8min, and keep warm for 2-3 hours;

[0014] S3, then transfer to the crystallization kettle, add liquid alkali dropwise, control the amount of liquid alkali added to 50-80g / min, add water, cool to 75-90℃ after the addition is completed, keep warm for 0.5-1.5 hours, discharge the material and filter by pressure to obtain 59# purple crude product.

[0015] Preferably, the liquid alkali is a 25%-35% sodium hydroxide solution.

[0016] Preferably, the auxiliary agent is prepared by compounding nano-organic silicon powder, polyvinyl pyrrolidone and xylitol in a mass ratio of 1.5:2-3:1.

[0017] Preferably, the method for preparing the nano-organic silicon powder comprises the following steps:

[0018] S1. Prepare a mixture of herbs, cellulase, ammonium nitrate, salt and water, ferment in a fermenter to prepare a fermentation mixture, add a 20-25% sodium carbonate solution to the fermentation mixture, continue soaking for 4-6 hours, control the temperature at 110-115° C., filter and purify after the soaking to obtain a mixed extract;

[0019] S2, the mixed extract is calcined and compounded in a sintering furnace with nitrogen as protective gas and oxygen-free environment to obtain porous organosilicon powder;

[0020] S3, crush the porous silicone powder to nanometer scale, with a particle size of 30-50nm and a specific surface area of ​​90-95m 2 / g.

[0021] Preferably, the herb is selected from mugwort or foxtail grass.

[0022] A method for preparing solvent violet 59 comprises the following steps:

[0023] According to the weight portions, 59# violet crude product, 50%-70% of the additives and 60%-75% of the deionized water were added into a grinding pot and ground to a powder particle size of 85-100 mesh. The powder was then transferred into an adjusting pot, and the remaining additives and deionized water were added into the adjusting pot. The product solvent violet 59 was then transferred into a drying tower for drying to obtain the product solvent violet 59.

[0024] Preferably, the temperature of the drying tower is controlled at 95-110° C. for 0.5-2 h.

[0025] Compared with the prior art, the present invention has the following beneficial effects:

[0026] 1. The present invention extracts organosilicon components from herbs and adds cellulase and the like for fermentation, wherein the cellulase can help the herbs release more organosilicon components, thereby improving the extraction efficiency and shortening the extraction time. The prepared porous organosilicon powder has a large specific surface area and pore volume, and can adsorb more functional substances, such as antibacterial active components, thereby enhancing its effect in functional applications.

[0027] 2. The present invention adopts three-stage stirring in the condensation stage. By controlling the stirring speed and time, the heat diffusion is uniform and rapid, which solves the problem of difficulty in heating up in the condensation stage in the current production process of solvent violet 59; at the same time, the speed of dripping liquid alkali is controlled to avoid the problem of excessive material or excessive phenol water in the production process due to too high alkali addition temperature or too fast alkali addition speed; the coloring rate of solvent violet 59 prepared according to the present invention reaches more than 98%, which is greater than the 90-95% coloring rate on the market, and the main content of the product obtained by high performance liquid chromatography reaches more than 99%, indicating that the product purity is high.

[0028] 3. In the preparation process of the present invention, by adding nano-organic silicon powder, polyvinyl pyrrolidone and xylitol as a compound auxiliary agent, it can achieve better thickening and dispersing effects in dye dispersion, and improve the stability and optical properties of the dye. Among them, polyvinyl pyrrolidone can enhance the adhesion and durability of the dye, and improve its performance in coatings or inks. As a natural colloid, xylitol can be used as a thickener and dispersant, which can improve the rheology and stability of the dye. DETAILED DESCRIPTION

[0029] The technical solution of the present invention will be clearly and completely described below in conjunction with the embodiments of the present invention. Obviously, the described embodiments are part of the embodiments of the present invention, not all of the embodiments. Based on the embodiments of the present invention, all other embodiments obtained by ordinary technicians in this field without creative work are within the scope of protection of the present invention.

[0030] Unless otherwise specified, the raw materials used in the present invention are all from conventional products purchased on the market. Among them, phenol, 1,4-diamino-2,3-dichloroanthraquinone, potassium carbonate, liquid caustic soda, cellulase, ammonium nitrate, polyvinyl pyrrolidone and xylitol are all purchased from Aladdin;

[0031] Preparation Example 1

[0032] The preparation method of the 59# purple crude product comprises the following steps:

[0033] S1. Add 70 g of phenol and 15 g of 1,4-diamino-2,3-dichloroanthraquinone into a reaction kettle, and control the stirring speed to 75 r / min and the stirring time to 8 min.

[0034] S2, add 12g potassium carbonate to the reactor, increase the stirring speed to 80r / min, stir for 10min, and heat to 180°C, then reduce the stirring speed to 60r / min, continue stirring for 6min and keep warm for 2 hours;

[0035] S3, transfer to the crystallization kettle, add 25g of 25% sodium hydroxide solution, control the amount of sodium hydroxide solution added to 50g / min, first fast and then slow, add 25g of deionized water, cool to 75℃ after the addition is completed, keep warm for 1 hour, discharge the material and filter, and obtain 59# purple crude product.

[0036] Preparation Example 2

[0037] The preparation method of the 59# purple crude product comprises the following steps:

[0038] S1. Add 80 g of phenol and 20 g of 1,4-diamino-2,3-dichloroanthraquinone into a reaction kettle, and control the stirring speed to 78 r / min and the stirring time to 9 min.

[0039] S2, add 12g potassium carbonate to the reactor, increase the stirring speed to 82r / min, stir for 11min, and heat to 190°C, then reduce the stirring speed to 65r / min, continue stirring for 8min and keep warm for 3 hours;

[0040] S3, transfer to the crystallization kettle, add 30g of 35% sodium hydroxide solution, control the amount of sodium hydroxide solution added to 65g / min, first fast and then slow, add 30g of deionized water, cool to 85℃ after the addition is completed, keep warm for 1.5 hours, discharge the material and filter, and obtain 59# purple crude product.

[0041] Preparation Example 3

[0042] The preparation method of the 59# purple crude product comprises the following steps:

[0043] S1. Add 85 g of phenol and 25 g of 1,4-diamino-2,3-dichloroanthraquinone into a reaction kettle, and control the stirring speed to 75 r / min and the stirring time to 10 min.

[0044] S2, add 15g potassium carbonate to the reactor, increase the stirring speed to 85r / min, stir for 12min, and heat to 200°C, then reduce the stirring speed to 65r / min, continue stirring for 8min and keep warm for 3 hours;

[0045] S3, transfer to the crystallization kettle, add 35g of 30% sodium hydroxide solution, control the amount of sodium hydroxide solution added to 80g / min, add 30g of deionized water, cool to 90℃ after the addition is completed, keep warm for 1.5 hours, discharge the material and filter, and obtain 59# purple crude product.

[0046] Preparation Example 4

[0047] The auxiliary agent is prepared by compounding 150g of nano-organic silicon powder, 200g of polyvinyl pyrrolidone and 100g of xylitol.

[0048] The preparation method of the nano-organic silicon powder comprises the following steps:

[0049] 100 g of foxtail grass, 55 g of cellulase, 10 g of ammonium nitrate, 20 g of salt and 60 g of water are prepared into a mixture, and fermented in a fermentation tank to prepare a fermentation mixture, 21 g of a 20% sodium carbonate solution is added to the fermentation mixture, and the mixture is soaked for 4 hours at a temperature of 110° C. After the soaking, the mixture is filtered and purified to obtain a mixed extract;

[0050] S2, the mixed extract is calcined and compounded in a sintering furnace with nitrogen as protective gas and oxygen-free environment to obtain porous organosilicon powder;

[0051] S3, crush the porous silicone powder to nanometer scale, with a particle size of 30nm and a specific surface area of ​​95m 2 / g.

[0052] Preparation Example 5

[0053] The auxiliary agent is prepared by compounding 150g of nano-organic silicon powder, 250g of polyvinyl pyrrolidone and 100g of xylitol.

[0054] The preparation method of the nano-organic silicon powder comprises the following steps:

[0055] 150g of wormwood, 60g of cellulase, 15g of ammonium nitrate, 25g of salt and 70g of water are prepared into a mixture, and fermented in a fermentation tank to prepare a fermentation mixture, 25g of a 25% sodium carbonate solution is added to the fermentation mixture, and the mixture is soaked for 5 hours at a temperature of 112°C. After the soaking is completed, the mixture is filtered and purified to obtain a mixed extract;

[0056] S2, the mixed extract is calcined and compounded in a sintering furnace with nitrogen as protective gas and oxygen-free environment to obtain porous organosilicon powder;

[0057] S3, crush the porous silicone powder to nanometer scale, with a particle size of 40nm and a specific surface area of ​​92m 2 / g.

[0058] Preparation Example 6

[0059] The auxiliary agent is prepared by compounding 150g of nano-organic silicon powder, 300g of polyvinyl pyrrolidone and 100g of xylitol.

[0060] The preparation method of the nano-organic silicon powder comprises the following steps:

[0061] 180g of wormwood, 65g of cellulase, 18g of ammonium nitrate, 28g of salt and 75g of water are prepared into a mixture, and fermented in a fermentation tank to prepare a fermentation mixture, 25g of a 20% sodium carbonate solution is added to the fermentation mixture, and the mixture is soaked for 6 hours at a temperature of 115°C. After the soaking is completed, the mixture is filtered and purified to obtain a mixed extract;

[0062] S2, the mixed extract is calcined and compounded in a sintering furnace with nitrogen as protective gas and oxygen-free environment to obtain porous organosilicon powder;

[0063] S3, crush the porous silicone powder to nanometer scale, with a particle size of 50nm and a specific surface area of ​​90m 2 / g.

[0064] Example 1

[0065] Add 45g of the 59# violet crude product prepared in Preparation Example 1, 5g of the auxiliary agent prepared in Preparation Example 4 and 30g of deionized water into a grinding pot and grind them to a powder particle size of 85 mesh. Then transfer them into an adjusting pot, add the remaining 5g of the auxiliary agent and 35g of deionized water into the adjusting pot, and then transfer them into a drying tower for drying. The temperature of the drying tower is controlled at 95°C for 1 hour to obtain the product solvent violet 59.

[0066] Example 2

[0067] Add 55g of the 59# violet crude product prepared in Preparation Example 1, 8g of the auxiliary agent prepared in Preparation Example 5 and 30g of deionized water into a grinding pot and grind them to a powder particle size of 100 mesh. Transfer them into an adjusting pot, add the remaining 6g of the auxiliary agent and 25g of deionized water into the adjusting pot, and then transfer them into a drying tower for drying. The temperature of the drying tower is controlled at 100°C for 1.5h to obtain the product solvent violet 59.

[0068] Example 3

[0069] Add 60g of the 59# violet crude product prepared in Preparation Example 1, 6g of the auxiliary agent prepared in Preparation Example 6 and 25g of deionized water into a grinding pot and grind them to a powder particle size of 100 mesh. Then transfer them into an adjusting pot, add the remaining 6g of the auxiliary agent and 25g of deionized water into the adjusting pot, and then transfer them into a drying tower for drying. The temperature of the drying tower is controlled at 105°C for 2h to obtain the product solvent violet 59.

[0070] Example 4

[0071] Add 60g of the 59# violet crude product prepared in Preparation Example 2, 6g of the auxiliary agent prepared in Preparation Example 4 and 25g of deionized water into a grinding pot and grind them to a powder particle size of 100 mesh. Then transfer them into an adjusting pot, add the remaining 6g of the auxiliary agent and 25g of deionized water into the adjusting pot, and then transfer them into a drying tower for drying. The temperature of the drying tower is controlled at 105°C for 2h to obtain the product solvent violet 59.

[0072] Example 5

[0073] Add 60g of the 59# violet crude product prepared in Preparation Example 3, 6g of the auxiliary agent prepared in Preparation Example 5 and 25g of deionized water into a grinding pot and grind them to a powder particle size of 100 mesh. Then transfer them into an adjusting pot, add the remaining 6g of the auxiliary agent and 25g of deionized water into the adjusting pot, and then transfer them into a drying tower for drying. The temperature of the drying tower is controlled at 105°C for 2h to obtain the product solvent violet 59.

[0074] Example 6

[0075] Add 60g of the 59# violet crude product prepared in Preparation Example 3, 6g of the auxiliary agent prepared in Preparation Example 6 and 25g of deionized water into a grinding pot and grind them to a powder particle size of 100 mesh. Then transfer them into an adjusting pot, add the remaining 6g of the auxiliary agent and 25g of deionized water into the adjusting pot, and then transfer them into a drying tower for drying. The temperature of the drying tower is controlled at 105°C for 2h to obtain the product solvent violet 59.

[0076] Comparative Example

[0077] The difference between this comparative example and Example 1 is that the auxiliary agent prepared in Preparation Example 4 is replaced by disodium hydrogen phosphate purchased from Aladdin, CAS No.: 7558-79-4.

[0078] 1. Performance Testing

[0079] The performance test and HPLC related data of the solvent violet 59 obtained in Examples 1-6 are shown in Table 1 below.

[0080] GB / T3920 is used to measure its rubbing fastness, GB / T8426 is used to measure its sunlight fastness, and GB / T9337-2001 is used to measure its high temperature dyeing rate.

[0081] Table 1

[0082] Test items Abrasion resistance Light fastness Coloring rate Main content of the product Example 1 5 5 99.4% 99.2% Example 2 5 5 99.3% 99.4% Example 3 5 5 99.3% 99.5% Example 4 5 5 99.1% 99.3% Example 5 5 5 99.2% 99.4% Example 6 5 5 99.3% 99.3% Comparative Example 4 4 96.9% 97.2%

[0083] As can be seen from Table 1, through the above embodiments and comparative examples, it is concluded that the color uptake rate (130°C, 60min) (mass fraction of dyeing amount) of solvent violet 59 prepared by the method of the present invention reaches more than 99%, wherein the optimal color uptake rate is 99.4%, which is higher than the quality specifications and industry standards; the main content of the product obtained by high performance liquid chromatography reaches more than 99%, wherein the optimal main content of the product is 99.5%, indicating that the product has high purity.

[0084] The above description is only a preferred specific implementation manner of the present invention, but the protection scope of the present invention is not limited thereto. Any technician familiar with the technical field can make equivalent replacements or changes according to the technical scheme and inventive concept of the present invention within the technical scope disclosed by the present invention, which should be covered by the protection scope of the present invention.

Claims

1. A solvent violet 59, characterized in that The solvent violet 59 is made from the following raw materials in parts by weight: 45-60 parts of 59# purple crude product, 1-10 parts of auxiliary agent and 40-60 parts of deionized water; The 59# purple crude product is made from the following raw materials in parts by weight: 70-85 parts of phenol, 10-25 parts of 1,4-diamino-2,3-dichloroanthraquinone, 10-15 parts of potassium carbonate, 25-35 parts of liquid caustic soda and 20-35 parts of deionized water.

2. A solvent violet 59 according to claim 1, characterized in that, The preparation method of the 59# purple crude product comprises the following steps: S1. Add phenol and 1,4-diamino-2,3-dichloroanthraquinone into a reaction kettle, and control the stirring speed to 75-80 r / min and the stirring time to 8-10 min; S2, add potassium carbonate to the reactor, increase the stirring speed to 80-85r / min, stir for 10-12min, and heat to 180-200°C, then reduce the stirring speed to 60-65r / min, continue stirring for 5-8min, and keep warm for 2-3 hours; S3, then transfer to the crystallization kettle, add liquid alkali dropwise, control the amount of liquid alkali added to 50-80g / min, add deionized water, cool to 75-90℃ after the addition is completed, keep warm for 0.5-1.5 hours, discharge the material and filter by pressure to obtain 59# purple crude product.

3. A solvent violet 59 according to claim 2, characterized in that, The liquid alkali is selected from 25%-35% sodium hydroxide solution.

4. A solvent violet 59 according to claim 1, characterized in that, The auxiliary agent is prepared by compounding nano-organic silicon powder, polyvinyl pyrrolidone and xylitol in a mass ratio of 1.5:2-3:

1.

5. A solvent violet 59 according to claim 4, characterized in that, The preparation method of the nano-organic silicon powder comprises the following steps: Prepare a mixture of herbaceous plants, cellulase, ammonium nitrate, salt and water, ferment in a fermentation tank to prepare a fermentation mixture, add a sodium carbonate solution with a concentration of 20-25% to the fermentation mixture, continue soaking for 4-6 hours, control the temperature at 110-115° C., filter and purify after the soaking to obtain a mixed extract; S2, the mixed extract is calcined and compounded in a sintering furnace with nitrogen as protective gas and oxygen-free environment to obtain porous organosilicon powder; S3, crush the porous silicone powder to nanometer scale, with a particle size of 30-50nm and a specific surface area of ​​90-95m 2 / g.

6. A solvent violet 59 according to claim 5, characterized in that, The herbaceous plant is selected from mugwort or foxtail grass.

7. A method for preparing solvent violet 59, comprising preparing the solvent violet 59 as claimed in any one of claims 1 to 6, characterized in that: The following steps are involved: According to the weight portions, 59# violet crude product, 50%-70% of the additives and 60%-75% of the deionized water were added into a grinding pot and ground to a powder particle size of 85-100 mesh. The powder was then transferred into an adjusting pot, and the remaining additives and deionized water were added into the adjusting pot. The product solvent violet 59 was then transferred into a drying tower for drying to obtain the product solvent violet 59.

8. The method for preparing solvent violet 59 according to claim 7, characterized in that: The temperature of the drying tower is controlled at 95-110° C. for 0.5-2 h.

Citation Information

Cited By

  • High-dispersion type solvent dye and preparation method thereof

    CN119463528A

  • Preparation process of light-cured organic silicon release film

    CN119798753A