Method for directly precipitating high-calcium rare earth chloride by sodium carbonate

By adding sodium bicarbonate to the sodium carbonate precipitation process and controlling the reaction conditions, the problem of difficult separation of calcium ions is solved, the calcium content is effectively reduced and the production cost is significantly reduced, meeting national standards and improving product quality.

CN118745534APending Publication Date: 2024-10-08中稀金龙(长汀)稀土有限公司
View PDF 0 Cites 0 Cited by

Patent Information

Application Number
CN202410918516.8
Authority / Receiving Office
CN · China
Patent Type
Applications(China)
Current Assignee / Owner
Filing Date
2024-07-10
Publication Date
2024-10-08

AI Technical Summary

Technical Problem

It is difficult to effectively separate calcium ions in the existing sodium carbonate precipitation process, resulting in excessive calcium content in the product and failure to meet national standards. Moreover, the extraction and separation method is costly and energy-intensive, affecting product quality and market competitiveness.

Method used

Using a mixed precipitant of sodium carbonate and sodium bicarbonate, by controlling the reaction conditions such as pH value, temperature and precipitant ratio, a calcium carbonate co-precipitate with a smaller content in lanthanum carbonate is generated to achieve effective separation and reduction of calcium ions.

Benefits of technology

The calcium content meets the national standard requirements, reducing production costs, especially the production costs of 4N lanthanum oxide, and improving product purity and market competitiveness.

✦ Generated by Eureka AI based on patent content.

Smart Images

  • Figure CN118745534A_ABST
    Figure CN118745534A_ABST
Patent Text Reader

Abstract

The invention discloses a method for directly precipitating high-calcium rare earth chloride by sodium carbonate, which comprises the following steps: (1) adding a proper amount of bottom water into a reaction kettle, and heating until the water temperature reaches 50 DEG C; (2) simultaneously adding a lanthanum-calcium material liquid and a sodium carbonate and sodium bicarbonate mixed solution into the reaction kettle in the step (1), controlling the pH value of the material liquid to be 4.0-4.5 in the adding process, heating to 58-60 DEG C after the adding is completed, and reacting until the pH value reaches 6-6.5; and (3) carrying out solid-liquid separation on the material obtained in the step (2), and washing the obtained solid with hot water at 50-55 DEG C to obtain the product. According to the method, a direct precipitation control method is adopted, and on the premise that calcium in the lanthanum calcium material is larger than 10000 mg / L, the content of calcium in the precipitate lanthanum carbonate meets the national standard requirement. According to the method, the production cost of 4N lanthanum oxide can be reduced by more than 0.70000 yuan / ton, and the method has a remarkable cost improvement effect on the premise that the total amount of rare earth and the precipitation yield are not influenced, and the content of calcium ions in the product is reduced.
Need to check novelty before this filing date? Find Prior Art

Description

Technical Field

[0001] The invention belongs to the technical field of rare earth chloride treatment, and in particular relates to a method for directly precipitating high-calcium rare earth chloride with sodium carbonate. Background Art

[0002] In the process of rare earth element extraction, the purity of lanthanum chloride is crucial. However, there is a significant technical problem in the current sodium carbonate precipitation process: the calcium ions in the raw materials are difficult to effectively separate, resulting in the final product failing to meet the strict requirements of national standards for calcium content. This problem not only affects the quality and application range of the product, but also brings huge economic pressure to the company.

[0003] First of all, the method of extracting and separating calcium is costly. In the process of refining rare earth elements, organic solvents are usually used as extractants, which are not only expensive but also may have adverse effects on the environment. In addition, the extraction process itself consumes a lot of energy and requires a lot of energy input, which undoubtedly increases production costs. Solvent recovery and waste disposal after extraction are also a major problem, which not only increases processing costs, but also poses a potential threat to the environment.

[0004] Secondly, the process of directly precipitating lanthanum calcium materials has technical defects. Due to the similarity in chemical properties between calcium ions and lanthanum ions, it is difficult to achieve effective separation of lanthanum and calcium through direct precipitation, resulting in the calcium content in the product generally exceeding the standard (greater than 1000μg / g). These products cannot meet the requirements of the national standard GB / T4154-2015 (Ca <500μg / g) and can only be downgraded or mixed with products of other specifications to meet the standard requirements. Although this approach can reduce costs in the short term, in the long run, it not only affects the market competitiveness of the product, but is also not conducive to the sustainable development of the enterprise.

[0005] In addition, the process of direct precipitation of lanthanum calcium materials also faces some operational problems. For example, improper control of conditions such as pH value, temperature, stirring speed, etc. during the precipitation process may lead to a decrease in the purity of the precipitate. Moreover, post-processing steps such as filtration, washing and drying after precipitation also have an important impact on the purity of the product. If these processes are not operated properly, the impurity content in the product will also increase. Summary of the invention

[0006] The present invention aims to overcome the defects of the prior art and provide a method for directly precipitating high calcium rare earth chloride with sodium carbonate.

[0007] The key control effect of the present invention is that the addition of the sodium carbonate / sodium bicarbonate mixed precipitant, due to the lack of power for sodium bicarbonate to react with calcium chloride in the lanthanum calcium material to form carbonate precipitation (the salt dilute solution and sodium bicarbonate react slightly), the content of calcium carbonate co-precipitate in the obtained reaction product lanthanum carbonate is relatively small (such asFigure 1 shown).

[0008] The reaction mechanism of the present invention is as follows:

[0009] The chemical reaction formula of sodium carbonate and rare earth chloride is as follows:

[0010] 2ReCl 3 +3Na 2 CO 3 +xH 2 O→Re 2 (CO 3 ) 3 xH 2 O↓+6NaCl

[0011] When the amount of sodium carbonate in the reaction system is large, rare earth sodium carbonate complex salt precipitation is produced. At the same time, since sodium carbonate is more alkaline than sodium bicarbonate, the following side reactions may also occur:

[0012] ReCl 3 +2Na 2 CO 3 +H 2 O→ReOHCO 3 ↓+3NaCl+NaHCO 3

[0013] The precipitate produced by the reaction has an abnormal crystal form, which easily encapsulates the free calcium in the solution and is not easy to separate the solid and the liquid. Therefore, the ratio of sodium bicarbonate to sodium carbonate is the key point of the present invention.

[0014] The technical solution of the present invention is as follows:

[0015] A method for directly precipitating high-calcium rare earth chloride with sodium carbonate comprises the following steps:

[0016] (1) Add an appropriate amount of bottom water to the reactor (the more bottom water, the lower the concentration of the precipitation system, which is beneficial to the effect of the present invention, but the cost should also be considered to add an appropriate amount), and heat the reactor until the water temperature reaches 50° C.;

[0017] (2) adding lanthanum calcium solution and sodium carbonate sodium bicarbonate mixed solution to the reaction kettle of step (1) at the same time, controlling the pH of the solution to be 4.0-4.5 during the addition process, heating the solution to 58-60° C. after the addition is completed to react until the pH reaches 6-6.5, wherein the mass percentage of sodium carbonate to sodium bicarbonate in the sodium carbonate sodium bicarbonate mixed solution is 20-80%:30-80%;

[0018] (3) The material obtained in step (2) is subjected to solid-liquid separation, and the obtained solid is washed with hot water at 50-55° C. to obtain the product.

[0019] In a preferred embodiment of the present invention, the concentration of the lanthanum calcium solution is 0.8-1.2 mol / L, and the total concentration of sodium carbonate and sodium bicarbonate in the sodium carbonate and sodium bicarbonate mixed solution is 0.8-1.2 mol / L.

[0020] Further preferably, the volume ratio of the lanthanum calcium solution to the sodium carbonate / sodium bicarbonate mixed solution is 4:5.6-5.9.

[0021] More preferably, the addition rate of the lanthanum calcium solution is 1.6-1.7m 3 / h, the addition rate of the sodium carbonate and sodium bicarbonate mixed solution is 2.1-2.3m 3 / h.

[0022] In a preferred embodiment of the present invention, in the sodium carbonate and sodium bicarbonate mixed solution, the mass percentage of sodium carbonate and sodium bicarbonate is 80%:20%.

[0023] The application of a sodium carbonate and sodium bicarbonate mixed solution in direct precipitation of high calcium rare earth chloride comprises the following steps:

[0024] (1) Add an appropriate amount of bottom water to the reactor and heat it to 50°C;

[0025] (2) adding lanthanum calcium solution and sodium carbonate sodium bicarbonate mixed solution to the reaction kettle of step (1) at the same time, controlling the pH of the solution to be 4.0-4.5 during the addition process, heating the solution to 58-60° C. after the addition is completed to react until the pH reaches 6-6.5, wherein the mass percentage of sodium carbonate to sodium bicarbonate in the sodium carbonate sodium bicarbonate mixed solution is 20-80%:30-80%;

[0026] (3) The material obtained in step (2) is subjected to solid-liquid separation, and the obtained solid is washed with hot water at 50-55° C. to obtain the product.

[0027] In a preferred embodiment of the present invention, the concentration of the lanthanum calcium solution is 0.8-1.2 mol / L, and the total concentration of sodium carbonate and sodium bicarbonate in the sodium carbonate and sodium bicarbonate mixed solution is 0.8-1.2 mol / L.

[0028] Further preferably, the volume ratio of the lanthanum calcium solution to the sodium carbonate / sodium bicarbonate mixed solution is 4:5.6-5.9.

[0029] More preferably, the addition rate of the lanthanum calcium solution is 1.6-1.7m 3 / h, the addition rate of the sodium carbonate and sodium bicarbonate mixed solution is 2.1-2.3m 3 / h.

[0030] In a preferred embodiment of the present invention, in the sodium carbonate and sodium bicarbonate mixed solution, the mass percentage of sodium carbonate and sodium bicarbonate is 80%:20%.

[0031] The beneficial effect of the present invention is that the present invention adopts a direct precipitation control method, and on the premise that the calcium in the lanthanum calcium material is greater than 10000 mg / L, the calcium content in the precipitate lanthanum carbonate meets the national standard requirements. This method can reduce the production cost of 4N lanthanum oxide by more than 7,000 yuan / ton, and has a significant cost effect of improving the total amount of rare earths, and reducing the content of calcium ions in the product on the premise that the precipitation yield is not affected. BRIEF DESCRIPTION OF THE DRAWINGS

[0032] Figure 1 This is the carbonate solubility curve.

[0033] Figure 2 This is a diagram of the experimental results of Example 1 of the present invention. DETAILED DESCRIPTION

[0034] The technical solution of the present invention is further illustrated and described below through specific implementation modes in combination with the accompanying drawings.

[0035] Example 1

[0036] In the precipitation workshop of Zhongxi Jinlong (Changting) Rare Earth Co., Ltd., the lanthanum calcium material used was prepared by the extraction workshop to a CaO>10000mg / L, and was precipitated in three 25 cubic meter reactors (hereinafter referred to as 1# pot, 2# pot, 3# pot) in sequence according to the following steps:

[0037] 1# Pot: Preparation of precipitant (100% sodium carbonate, mass percentage, the same below)

[0038] Pot 2#: precipitant preparation (50% sodium carbonate + 50% sodium bicarbonate)

[0039] Pot 3#: precipitant preparation (20% sodium carbonate + 80% sodium bicarbonate)

[0040] 1# Pot:

[0041] (1) Add an appropriate amount of bottom water to the reactor and heat it to 50°C;

[0042] (2) Add 4m 3 Lanthanum calcium solution (concentration 1mol / L, feed rate 1.65m 3 / h) and 5.75m 3 Sodium carbonate and sodium bicarbonate mixed solution (the total concentration of sodium carbonate and sodium bicarbonate is 1 mol / L, the feed rate is 2.18m 3 / h), during the addition process, the pH of the feed solution was controlled to be 4.0-4.5, and after the addition was completed, the temperature was raised to 58-60°C for reaction until the pH reached 6.5, and the rare earth concentration of the supernatant was measured to be <0.01 mol / L;

[0043] (3) The material obtained in step (2) was aged and then subjected to solid-liquid separation. The obtained solid was washed 8 times with hot water at 53° C., and after being drained, carbonate was taken for detection: CaO: 919 μg / g, Cl: 468 μg / g, REO%. Total oxide content: >99.0%.

[0044] 2# Pot:

[0045] (1) Add an appropriate amount of bottom water to the reactor and heat it to 50°C;

[0046] (2) Add 4m 3 Lanthanum calcium solution (concentration 1mol / L, feed rate 1.65m 3 / h) and 5.83m 3 Sodium carbonate and sodium bicarbonate mixed solution (the total concentration of sodium carbonate and sodium bicarbonate is 1 mol / L, the feed rate is 2.22m 3 / h), during the addition process, the pH of the feed solution was controlled to be 4.0-4.5, and after the addition was completed, the temperature was raised to 59-60°C for reaction until the pH reached 6.5, and the rare earth concentration of the supernatant was measured to be <0.008 mol / L;

[0047] (3) The material obtained in step (2) was aged and then subjected to solid-liquid separation. The obtained solid was washed 8 times with hot water at 53° C., and after being drained, carbonate was taken for detection: CaO: 407 μg / g, Cl: 322 μg / g, REO%. Total oxide content: >99.50%.

[0048] 3# Pot:

[0049] (1) Add an appropriate amount of bottom water to the reactor and heat it to 50°C;

[0050] (2) Add 4m 3 Lanthanum calcium solution (concentration 1mol / L, feed rate 1.65m 3 / h) and 5.65m 3 Sodium carbonate and sodium bicarbonate mixed solution (the total concentration of sodium carbonate and sodium bicarbonate is 1 mol / L, the feed rate is 2.14m 3 / h), during the addition process, the pH of the feed solution was controlled to be 4.0-4.5, and after the addition was completed, the temperature was raised to 59-60°C for reaction until the pH reached 6.5, and the rare earth concentration of the supernatant was measured to be <0.01 mol / L;

[0051] (3) The material obtained in step (2) was aged and then subjected to solid-liquid separation. The obtained solid was washed 8 times with hot water at 53° C., and after being drained, carbonate was taken for detection: CaO: 421 μg / g, Cl: 295 μg / g, REO%. Total oxide content: >99.5.

[0052] As can be seen from the above, the addition of sodium bicarbonate can significantly improve the effect of carbon precipitation of lanthanum calcium materials, but the higher the ratio, the better the effect. The market price of sodium bicarbonate is also much higher than that of sodium carbonate. Therefore, the appropriate ratio has obvious advantages in terms of calcium removal effect and cost saving. The experiment was carried out with 50% sodium carbonate + 50% sodium bicarbonate as the control, and the following three sets of data were obtained (the specific process parameters are the same as above):

[0053] 1# pot: precipitant preparation (90% sodium carbonate + 10% sodium bicarbonate), CaO: 579μg / g, Cl: 331μg / g

[0054] 2# pot: precipitant preparation (80% sodium carbonate + 20% sodium bicarbonate), CaO: 523μg / g, Cl: 370μg / g

[0055] Pot 3#: precipitant preparation (70% sodium carbonate + 30% sodium bicarbonate), CaO: 466μg / g, Cl: 305μg / g

[0056] like Figure 2 As shown, it can be seen that the best effect is achieved when the ratio is 80% sodium carbonate + 20% sodium bicarbonate, and the product quality meets the national standard requirements.

[0057] The above description is only a preferred embodiment of the present invention, and therefore cannot be used to limit the scope of the present invention. That is, equivalent changes and modifications made according to the patent scope of the present invention and the contents of the specification should still fall within the scope of the present invention.

Claims

1. A method for directly precipitating high calcium rare earth chloride with sodium carbonate, Features: The steps include: (1) Add an appropriate amount of bottom water to the reactor and heat it to 50°C; (2) adding lanthanum calcium solution and sodium carbonate sodium bicarbonate mixed solution to the reaction kettle of step (1) at the same time, controlling the pH of the solution to be 4.0-4.5 during the addition process, heating the solution to 58-60° C. after the addition is completed to react until the pH reaches 6-6.5, wherein the mass percentage of sodium carbonate to sodium bicarbonate in the sodium carbonate sodium bicarbonate mixed solution is 20-80%:30-80%; (3) The material obtained in step (2) is subjected to solid-liquid separation, and the obtained solid is washed with hot water at 50-55° C. to obtain the product.

2. The method according to claim 1, Features: The concentration of the lanthanum-calcium solution is 0.8-1.2 mol / L, and the total concentration of sodium carbonate and sodium bicarbonate in the sodium carbonate-sodium bicarbonate mixed solution is 0.8-1.2 mol / L.

3. The method according to claim 2, Features: The volume ratio of the lanthanum calcium solution to the sodium carbonate and sodium bicarbonate mixed solution is 4:5.6-5.

9.

4. The method according to claim 3, Features: The addition rate of the lanthanum calcium solution is 1.6-1.7m 3 / h, the addition rate of the sodium carbonate and sodium bicarbonate mixed solution is 2.1-2.3m 3 / h.

5. The method according to any one of claims 1 to 4, Features: In the sodium carbonate and sodium bicarbonate mixed solution, the mass percentage of sodium carbonate and sodium bicarbonate is 80%:20%.

6. Application of sodium carbonate and sodium bicarbonate mixed solution in direct precipitation of high calcium rare earth chloride, Features: The steps include: (1) Add an appropriate amount of bottom water to the reactor and heat it to 50°C; (2) adding lanthanum calcium solution and sodium carbonate sodium bicarbonate mixed solution to the reaction kettle of step (1) at the same time, controlling the pH of the solution to be 4.0-4.5 during the addition process, heating the solution to 58-60° C. after the addition is completed to react until the pH reaches 6-6.5, wherein the mass percentage of sodium carbonate to sodium bicarbonate in the sodium carbonate sodium bicarbonate mixed solution is 20-80%:30-80%; (3) The material obtained in step (2) is subjected to solid-liquid separation, and the obtained solid is washed with hot water at 50-55° C. to obtain the product.

7. The use according to claim 6, Features: The concentration of the lanthanum-calcium solution is 0.8-1.2 mol / L, and the total concentration of sodium carbonate and sodium bicarbonate in the sodium carbonate-sodium bicarbonate mixed solution is 0.8-1.2 mol / L.

8. The use according to claim 7, Features: The volume ratio of the lanthanum calcium solution to the sodium carbonate and sodium bicarbonate mixed solution is 4:5.6-5.

9.

9. The method according to claim 8, Features: The addition rate of the lanthanum calcium solution is 1.6-1.7m 3 / h, the addition rate of the sodium carbonate and sodium bicarbonate mixed solution is 2.1-2.3m 3 / h.

10. The use according to any one of claims 6 to 9, Features: In the sodium carbonate and sodium bicarbonate mixed solution, the mass percentage of sodium carbonate and sodium bicarbonate is 80%:20%.