Preparation method of multicolor electromagnetic wave absorption foam with adjustable absorption frequency

Through the chemical plating method and atomic layer deposition method of titanium oxide/nickel/porous foam materials, the problem of fixed absorption frequency of microwave absorbing materials is solved, multi-color adjustment and frequency control are realized, and it is suitable for intelligent electronic equipment and radar stealth fields. Excellent mechanical properties and environmentally friendly properties.

CN118745568APending Publication Date: 2024-10-08HAINAN UNIV
View PDF 0 Cites 0 Cited by

Patent Information

Application Number
CN202410040135.4
Authority / Receiving Office
CN · China
Patent Type
Applications(China)
Current Assignee / Owner
Filing Date
2024-01-11
Publication Date
2024-10-08

AI Technical Summary

Technical Problem

The absorption frequency of existing microwave absorbing materials is fixed and difficult to adjust, and traditional pigments are harmful to the environment and cannot meet the needs of multi-band communication and optical camouflage.

Method used

Titanium oxide/nickel/porous foam material is used, prepared by electroless plating and atomic layer deposition. The coating thickness and deposition cycle number of titanium oxide are adjusted to adjust the color and absorption frequency of the electromagnetic wave absorbing foam, using a three-dimensional cross-linked network. Structural porous foam material improves mechanical properties.

Benefits of technology

It realizes multi-color adjustment and frequency control of electromagnetic wave absorbing foam, has excellent mechanical properties and environmental protection characteristics, and is suitable for intelligent electronic equipment and radar stealth fields.

✦ Generated by Eureka AI based on patent content.

Smart Images

  • Figure CN118745568A_ABST
    Figure CN118745568A_ABST
Patent Text Reader

Abstract

The invention discloses a preparation method of multicolor electromagnetic wave absorption foam with adjustable absorption frequency, and the preparation method of the electromagnetic wave absorption foam comprises the following steps: firstly, growing a highly conductive nickel layer on the surface of porous melamine foam in situ through a chemical plating method, and then coating a titanium oxide film on the surface of the nickel layer through atomic layer deposition. The obtained composite foam has a three-dimensional interconnected porous structure, the preparation process is simple, the composite foam can present multiple colors by adjusting the thickness of the titanium oxide film, meanwhile, the electromagnetic parameters and the absorption frequency band of the composite foam can be effectively adjusted by changing the compression ratio, the defects that the traditional electromagnetic wave absorption frequency is fixed and single are overcome, and the electromagnetic wave absorption efficiency is improved. And wide frequency tuning range and absorption bandwidth are realized. The composite foam disclosed by the invention integrates colorful colors and an adjustable absorption frequency band, and provides precious insight for development of next-generation intelligent electromagnetic equipment crossing different fields.
Need to check novelty before this filing date? Find Prior Art

Description

Technical Field

[0001] The invention relates to a method for preparing an adjustable absorption frequency and multi-color electromagnetic wave absorbing foam. The electromagnetic wave absorbing foam of the invention can obtain a variety of colors by adjusting the preparation method, and the wave absorbing performance can be regulated by changing the compression ratio during actual use. The foam can be applied to multiple fields such as radar stealth, anti-electromagnetic interference and optical camouflage, and belongs to the technical field of nano material preparation and application. Background Art

[0002] Microwave absorbing materials play a vital role in mitigating electromagnetic pollution and improving military stealth capabilities, and are therefore widely used in fields such as portable electronic devices and stealth weapons. Inspired by the growing demand for coping with complex and changeable application environments, MXenes, graphene, carbon fiber, and carbonyl iron, as well as their composites, have been developed, and some of the outstanding representatives almost meet the multifunctional requirements, including strong adsorption, light weight, wide bandwidth, and high environmental stability. However, little attention has been paid to the regulation of their absorption frequency. The absorption frequency of all these materials is constant and limited to a specific frequency range due to their fixed electromagnetic parameters and fixed structural characteristics. At present, the application of multi-band cooperative communication technologies (such as 3G-5G) requires strategic and timely frequency adjustment of microwave absorbing materials. For stealth weapons, adjusting the absorption frequency to avoid multi-frequency radar detection is also a top priority. One feasible way to adjust the absorption frequency is to change the coating thickness of the absorption layer. According to the quarter-wavelength theory, the absorption frequency is inversely proportional to the coating thickness, so the absorption frequency can be adjusted to a lower frequency by increasing the coating thickness. However, this method is often complicated and cumbersome, making it inconvenient or even impossible to achieve during the operation stage of the equipment. Research has shown that reconfigurable metamaterial absorbers have better prospects for dynamic modulation of absorption frequency. Some metamaterials can be reversibly switched between different shapes by mechanical folding, compression, and stretching, thus providing the possibility of regulating the absorption frequency through structural transformation. However, the achievable structures are highly restricted by the prescribed design, which largely limits the tuning range of the absorption frequency. In addition, since the absorption capacity of metamaterials mainly depends on their intrinsic structure, their absorption bandwidth is generally narrow. Therefore, in practice, it remains a challenge to achieve tunable absorption frequency within a wide tuning range according to specific application requirements and real-time scenarios.

[0003] In addition to tunable absorption frequency in the microwave spectrum, optical camouflage in the visible light spectrum range is also considered to be one of the most critical strategic tasks. It mainly involves matching the color between the target and the surrounding environment to deceive enemy reconnaissance equipment, thereby improving the battlefield survivability of weapons. However, the significant wavelength difference between the microwave and visible light spectra is the main obstacle to the development of MAMs compatible with optical camouflage. Although traditional surface spraying dyes or coating treatments can obtain the desired color, the microwave absorption (MA) performance of the absorber is inevitably hindered due to impedance mismatch, but this method has serious limitations and disadvantages such as environmental harm, chemical instability, and easy degradation. Fortunately, structural colors provide a compelling choice due to the physical interaction between light and periodic nano- or microstructures. They show excellent anti-fading and environmental performance, and therefore have a wide range of uses in various fields, including anti-counterfeiting devices, colorimetric sensors, and visible camouflage. Structural colors with a wide spectral range offer hope for the construction of microwave absorbing materials that integrate tunable absorption frequency and optical camouflage, which, if realized, will undoubtedly promote the rapid development of advanced intelligent defense systems.

[0004] Colorful MAMs can provide optical camouflage by matching the color of the environment and making various camouflage patterns, which can further improve the safety of equipment and support complex application scenarios. For example, pure white, dark green, and khaki exterior walls are suitable for camouflaging military equipment in northern winter, southern summer, and desert areas, respectively. Their consistent color matching with the service environment can blend the two together and significantly extend the visual detection distance. Although traditional dyes and pigments are abundant, they are destructive to the environment, chemically unstable, easy to fall off, and may weaken MA due to additional coatings. Structural colors originate from the interaction between light and periodic nano- or microstructures. Structural colors have the advantages of overall structure, low toxicity, fading resistance, and environmental protection, and have been widely studied in anti-counterfeiting devices, colorimetric sensors, visible camouflage, and other fields. Microwave absorbers integrated with brilliant structural colors have not yet been reported. If realized, they will have great potential to build multifunctional intelligent MA systems. Summary of the invention

[0005] In view of the problems of single color and fixed wave absorption performance of traditional microwave absorbing materials, the present invention provides a method for preparing a foam with adjustable absorption frequency and multi-color electromagnetic wave absorption. The composition of the electromagnetic wave absorption foam is titanium oxide / nickel / porous foam material. The preparation process is simple, and the coating thickness of titanium oxide can be conveniently adjusted by adjusting the process parameters, thereby realizing the adjustment of the color of the electromagnetic wave absorption foam. At the same time, the composite material of the present invention uses a porous foam material with a three-dimensional cross-linked network structure as a skeleton, has excellent mechanical properties, and changes the thickness and electromagnetic parameters of the composite material by applying pressure, thereby realizing the adjustment of the absorption frequency and bandwidth, solving the disadvantage that the fixed absorption performance of traditional electromagnetic wave absorption materials cannot be adjusted in time with changes in the external environment.

[0006] The specific technical solutions of the present invention are as follows:

[0007] A method for preparing electromagnetic wave absorbing foam, characterized in that it comprises the following steps:

[0008] (1) coating a nickel layer on the surface of the foam material by chemical plating to obtain a nickel / porous foam material;

[0009] (2) A titanium oxide film is deposited on the nickel / porous foam material by atomic layer deposition to obtain a titanium oxide / nickel / porous foam material (TiO 2 / Ni / MF), that is, electromagnetic wave absorbing foam.

[0010] Furthermore, the porous foam material is a foam material with a three-dimensional cross-linked structure, which has elasticity and morphological plasticity, can be repeatedly compressed, and can adjust its thickness by controlling external pressure. The porous foam material used in the present invention is melamine foam, and the pore size is generally 50-300 μm. When melamine foam is used as the porous foam material, the obtained composite material can be expressed as TiO 2 / Ni / MF.

[0011] Furthermore, in step (1), the operation mode of the chemical plating method is: placing the porous foam in SnCl 2 / HCl aqueous solution for sensitization. Subsequently, the sensitized porous foam was placed in a solution of PdCl 2 Then, the activated porous foam was placed in a mixed solution of NaH 2 PO 2 ·H 2 O aqueous solution. Finally, the reduced porous foam was immersed in NiCl 2 and CH 3 In the aqueous dispersion of COONa, NaH 2 PO 2 ·H 2 O.C 6 H5 Na 3 O 7 and C 19 H 42 The aqueous dispersion of BrN is added to the above solution to carry out chemical plating reaction to obtain a nickel / porous foam material.

[0012] Furthermore, in step (1), SnCl 2 The mass ratio of PdCl to HCl is 2:1. 2 The concentration in 2.6% HCl aqueous dispersion is 2-3mmol / L, NaH 2 PO 2 ·H 2 The concentration of O in aqueous dispersion is 2-3 mol / L.

[0013] Further, in step (1), NiCl 2 , CH 3 COONa、NaH 2 PO 2 ·H 2 O.C 6 H 5 Na 3 O 7 and C 19 H 42 The concentrations of BrN aqueous dispersions are 26 g / L, 26 g / L, 36 g / L, 58 g / L, and 0.025 g / L, respectively.

[0014] Furthermore, in step (1), the chemical plating temperature is 45-55° C., preferably 50° C. The polymerization time is generally 10-40 min, preferably 30 min.

[0015] Furthermore, in step (2), the nickel / porous foam material is placed in an atomic layer deposition device for reaction. The method for preparing titanium oxide can be carried out with reference to the method disclosed in the prior art. Preferably, the precursors are tetraisopropyl titanium and water, respectively, the deposition temperature is 140-160°C, and the deposition cycle is 500-2500 cycles, for example, 500 cycles, 1000 cycles, 1500 cycles, 2000 cycles, and 2500 cycles. By adjusting the number of deposition cycles, the titanium oxide film with different thicknesses deposited on the surface of the nickel / porous foam material can be controllably regulated. Experiments have shown that the coating thickness of titanium oxide has a great influence on the morphology, color and performance of the final product, and is the key to the formation of the composition and morphology of the final product. Preferably, the deposition cycle is 2000 cycles.

[0016] The present invention first coats a magnetic nickel layer on the foam material by chemical plating, and then coats a uniform thickness of titanium oxide on the nickel / porous foam material by atomic layer deposition to obtain a brightly colored TiO2 / Ni / MF electromagnetic wave absorbing foam. In this composite material, the coating thickness of titanium oxide can be controlled by controlling the number of deposition cycles.

[0017] The present invention also provides a foam with adjustable absorption frequency and multi-color electromagnetic wave absorption, the raw materials of which include the above-mentioned TiO 2 / Ni / MF composite material. By adjusting the deposition cycle number of titanium oxide in the electromagnetic wave absorbing foam, the color of the electromagnetic wave absorbing foam can be controlled, and the electromagnetic wave absorbing performance can be adjusted by changing the radial compression ratio. It has a good application prospect.

[0018] The TiO obtained by the present invention 2 / Ni / MF composite materials have a variety of bright colors and can adjust the electromagnetic wave absorption performance in time according to changes in the external environment. They have excellent mechanical properties and stable structure. They can have good application prospects in the fields of smart electronic devices and radar stealth, overcoming the shortcomings of traditional electromagnetic wave absorption materials such as passive absorption and single color.

[0019] The present invention uses porous foam material as the skeleton and prepares TiO 2 / Ni / MF,TiO 2 / Ni grows evenly on the skeleton of melamine foam, which effectively solves the problem of single color, fixed absorption frequency and bandwidth of traditional absorbing materials, and greatly improves the electromagnetic wave absorption performance of melamine foam. Compared with the prior art, the advantages of the present invention are:

[0020] 1. The present invention combines chemical plating and atomic layer deposition technology to prepare TiO 2 / Ni / MF, the preparation process is simple and easy.

[0021] 2. The present invention prepares TiO with three-dimensional cross-linking 2 / Ni / MF, the thickness of titanium oxide can be precisely controlled through atomic layer deposition technology, which can well adjust the color of composite foam. And the coating of titanium oxide also effectively solves the shortcomings of Ni's easy shedding and oxidation.

[0022] 3. TiO prepared by the present invention 2 / Ni / MF has excellent mechanical properties and can effectively adjust the TiO 2 The electromagnetic wave absorption performance of / Ni / MF solves the shortcoming of fixed absorption performance of traditional electromagnetic wave absorption materials.

[0023] 4. TiO prepared by the present invention 2 / Ni / MF combines bright colors and adjustable absorption properties, is environmentally friendly and pollution-free, and has broad application prospects in smart electronic devices and radar stealth. BRIEF DESCRIPTION OF THE DRAWINGS

[0024] Figure 1 The scanning electron microscope images of the samples of the present invention are shown in Figure 1, where a. MF, b. Ni / MF, c. Ni / MF magnified image, d. TiO 2 / Ni / MF-2000 enlarged image.

[0025] Figure 2 This is the element distribution picture of the sample of the present invention.

[0026] Figure 3 (a) Transmission electron microscope image and (b) optical microscope image of the sample of the present invention, a. Transmission electron microscope image, b. Optical microscope image.

[0027] Figure 4 The TiO 2 Electromagnetic parameters of / Ni / MF at different compression ratios, a. real part of dielectric, b. imaginary part of dielectric, c. real part of magnetic permeability, d. imaginary part of magnetic permeability.

[0028] Figure 5 TiO 2 Reflection loss values ​​of / Ni / MF-2000 at different compression ratios. DETAILED DESCRIPTION

[0029] The present invention is described in detail below through specific examples, but the use and purpose of these exemplary embodiments are only used to explain and illustrate the present invention, and do not constitute any form of limitation on the actual protection scope of the present invention, nor limit the protection scope of the present invention to these.

[0030] Example 1 Preparation of PPy / MF

[0031] Ni / MF was synthesized by a simple chemical plating method. 2 (3.6 g) and concentrated hydrochloric acid (1.8 g) were dispersed in 100 mL of deionized water to obtain an aqueous dispersion.

[0032] Take a piece of MF (0.5cm×2cm×2cm), clean it thoroughly with ethanol and deionized water, and then dry it. Then immerse the MF completely in the mixed solution. Compress the MF foam fully to make the MF completely immersed in the mixed solution and fully contact with the components in the mixed solution. Sensitize for 20 minutes.

[0033] After the sensitization reaction is completed, rinse with deionized water and dry.

[0034] PdCl 2(50 mg) and HCl (7 mL) were dispersed in 100 mL of deionized water to obtain an aqueous dispersion. The dried MF was completely immersed in the mixed solution. The MF foam was fully compressed to make the MF completely immersed in the mixed solution and fully contact with the components in the mixed solution, and activated for 5 minutes.

[0035] NaH 2 PO 2 ·H 2 O (40g) was dispersed in 100mL deionized water to obtain an aqueous dispersion. The activated MF was completely immersed in the solution. The MF foam was fully compressed to make the MF completely immersed in the mixed solution and fully contact with the components in the mixed solution, and reduced for 1min. The obtained MF was rinsed with deionized water and dried.

[0036] NiCl 2 (2.6 g) CH 3 COONa (2.6 g) was dispersed in 50 mL of deionized water to obtain aqueous dispersion A. NaH 2 PO 2 ·H 2 O(3.6g), C 6 H 5 Na 3 O 7 (5.8 g) and C 19 H 42 BrN (2.5 mg) was dispersed in 50 mL of deionized water to obtain aqueous dispersion B.

[0037] Solutions A and B were placed in a magnetic stirring water bath at 50°C. The treated MF was immersed in the plating solution of solution A, and then solution B was added to the plating solution, and the reaction time was 30min.

[0038] After the reaction, Ni / MF was washed with distilled water and ethanol and dried in a vacuum oven at 60 °C.

[0039] MF has a unique three-dimensional interconnected macroporous structure ( Figure 1 a), is a good scaffold material for preparing Ni / MF. The morphology of the original MF and the Ni / MF prepared by chemical plating was characterized by scanning electron microscopy ( Figure 1 a, b). It can be observed from the figure that after chemical nickel plating, a Ni layer is formed on the surface of the MF skeleton, causing the surface to become rough ( Figure 1 b) The thickness of the Ni layer is 0.38 μm.

[0040] Example 2TiO 2 Preparation of / Ni / MF composites

[0041] By atomic layer deposition, the Ni / MF prepared in Example 1 is placed in an atomic layer deposition device to deposit titanium oxide. During atomic layer deposition, tetraisopropyl titanium and water are used as precursors. The deposition temperature is 150°C. The theoretical thickness of the titanium oxide molecular film obtained in a single cycle is about 0.083nm. Each cycle of atomic layer deposition is divided into two half reactions. In the first half reaction, the first precursor tetraisopropyl titanium is introduced with a pulse time of 2s, and nitrogen is passed to blow away the unreacted tetraisopropyl titanium and by-products, and the purge time is 15s; in the second half reaction, the second precursor water is introduced with a pulse time of 0.2s to react with the first half reaction, and nitrogen is passed to blow away the unreacted water and by-products, and the purge time is 15s to complete an atomic layer deposition process. The thickness of titanium oxide film can be precisely controlled by the number of atomic layer deposition cycles. In this experiment, a series of samples with different film thicknesses were prepared by adjusting the number of cycles, which were 500 cycles, 1000 cycles, 1500 cycles, 2000 cycles, and 2500 cycles, respectively. The obtained products were named TiO 2 / Ni / MF-n, where n is the number of cycles.

[0042] Energy dispersive X-ray spectroscopy of the obtained product revealed that the complementary profiles of Ti, O, Ni, and P converge specifically on the TiO 2 / Ni interface, thus providing additional evidence that the Ni-on-TiO 2 Uniformity and conformality of coating.

[0043] The obtained product was observed by transmission electron microscope. 2 TiO / Ni / MF-500 2 The thickness is about 45nm, TiO 2 The coating thickness can be precisely controlled by precisely controlling the number of atomic layer deposition cycles.

[0044] The obtained product was observed under an optical microscope. Figure 2 As shown, the TiO 2 / Ni / MF presents different colors. As the number of deposition cycles increases, a series of colors appear, such as light brown, gold, purple, blue, blue-white, and green. These gorgeous structural colors are the product of the synergistic effect of multiple optical phenomena, including light reflection, refraction, scattering, and thin film interference. It was observed that even the bone structure showed vibrant colors.

[0045] TiO 2 Application of Ni / MF composite materials in electromagnetic wave absorption

[0046] In order to obtain the microwave absorption performance of TiO2 / Ni / MF composite materials, the electromagnetic parameters of the composite materials in the frequency range of 2-18GHz were measured using Ceyear, 3672B-S network analyzer. ZnO / PPy / MF composite materials were formed after paraffin vacuum impregnation, and were compressed by 0%, 20%, 35%, 50%, and 70% in the radial direction, and then cut into rings with an outer diameter of 7.00mm and an inner diameter of 3.04mm (thickness of 2.00mm). Each ring was placed on a vector grid analyzer to measure the electromagnetic parameters of the composite materials.

[0047] TiO 2 The test results of / Ni / MF-2000 are as follows Figure 4 As shown in the figure, it can be seen that under different compression ratios, TiO 2 The dielectric real part ε′ and dielectric imaginary part ε" of / Ni / MF-2000 increase slightly with the increase of compression ratio, and decrease with the increase of frequency. This is mainly attributed to the insulating TiO 2 The formation of strong conductive pathways in the composite material is suppressed, so that its dielectric constant is maintained at an appropriate value, which is conducive to optimizing impedance matching, which is very beneficial for achieving wide-frequency tuned electromagnetic wave absorption performance.

[0048] The electromagnetic wave absorption performance of each sample was analyzed by transmission line theory.

[0049]

[0050] RL=20lg|(Z in -Z 0 ) / (Z in +Z 0 )| (Equation 2)

[0051] Where Z in is the input impedance of the absorber, Z 0 is the free space impedance, μ r is the relative complex permeability (μ r =μ′-iμ"), ε r is the complex dielectric constant (ε r =ε′-iε"), d is the thickness of the absorber, c and f are the speed and frequency of light respectively.

[0052] The reflection loss (RL) value should be less than -10dB, which means that 90% of electromagnetic waves can be absorbed, which can meet the usage requirements. Figure 5 TiO 2 / Ni / MF-2000 RL values ​​at different compression ratios. It can be seen from the figure that TiO 2 / Ni / MF-2000 can be adjusted by simple compression. The thickness of the electromagnetic wave absorbing foam is selected as 6mm, and by changing the ratio of radial compression, the electromagnetic wave absorption frequency can be effectively adjusted from C band (4-8GHz) to Ku band (12-18GHz).

Claims

1. A method for preparing an adjustable absorption frequency and multi-color electromagnetic wave absorbing foam, characterized in that: The following steps are involved: (1) coating the surface of the three-dimensionally interconnected foam with a nickel layer by chemical plating to obtain a nickel / foam material; (2) A titanium oxide layer is deposited on the nickel / foam material by an atomic layer deposition method to obtain a titanium oxide / nickel / foam material, namely, an electromagnetic wave absorbing foam material.

2. The preparation method according to claim 1, characterized in that: The porous foam material is melamine foam.

3. The preparation method according to claim 1, characterized in that: In step (1), the operation mode of the chemical plating method is as follows: the porous foam is placed in an aqueous solution of SnCl2 / HCl for sensitization treatment; then, the sensitized porous foam is placed in a mixed solution of PdCl2 and HCl for activation; then, the activated porous foam is placed in an aqueous solution of NaH2PO2·H2O for reduction; finally, the reduced porous foam is immersed in an aqueous dispersion of NiCl2 and CH3COONa, and NaH2PO2·H2O, C6H5Na3O7 and C 19 H 42 The aqueous dispersion of BrN is added to the above solution to carry out chemical plating reaction to obtain a nickel / porous foam material.

4. The preparation method according to claim 3, characterized in that: In step (1), the mass ratio of SnCl2 to HCl is 2:1, the concentration of PdCl2 in 2.6% HCl aqueous dispersion is 2-3 mmol / L, the concentration of NaH2PO2·H2O aqueous dispersion is 2-3 mol / L, and the concentration of NiCl 2、 CH3COONa, NaH2PO2·H2O, C6H5Na3O7 and C 19 H 42 The concentrations of BrN aqueous dispersions were 26 g / L, 26 g / L, 36 g / L, 58 g / L, and 0.025 g / L; Preferably, in step (1), the concentration of PdCl2 in 2.6% HCl aqueous dispersion is 2.9 mmol / L.

5. The preparation method according to claim 3, characterized in that: In step (1), the chemical plating temperature is 45-55°C, and the reaction time is 10-40 min; preferably, the chemical plating temperature is 50°C; preferably, the reaction time is 30 min.

6. The preparation method according to claim 1, characterized in that: In step (2), during the atomic layer deposition process, the precursors are tetraisopropyltitanium and water, the deposition temperature is 145-165° C., and the deposition period is 500-2500 cycles.

7. An electromagnetic wave absorbing composite material obtained by the preparation method of the electromagnetic wave absorbing foam according to any one of claims 1 to 6.

8. An electromagnetic wave absorbing foam with adjustable absorption frequency and multiple colors, characterized by: The raw materials include the electromagnetic wave absorbing composite material as described in claim 7.

9. A method for adjusting the color and frequency of electromagnetic wave absorbing foam, characterized by: The electromagnetic wave absorbing composite material described in claim 7 is used as the raw material of the electromagnetic wave absorber, the color of the composite foam is regulated by adjusting the thickness of the titanium oxide layer of the electromagnetic wave absorbing composite material, and the microwave absorption frequency and absorption bandwidth are adjusted by adjusting the thickness and radial compression ratio.

10. Use of the electromagnetic wave absorbing composite material according to claim 7 and the electromagnetic wave absorbing foam according to claim 8 in the fields of radar stealth equipment and civil electronic equipment.