Glass fiber reinforced plastic anti-corrosion template and preparation method thereof

By applying a special primer and pre-treated fiberglass cloth on the wooden building formwork and performing UV curing, the problem of easy weathering deformation and insufficient strength of the wooden formwork is solved, and the high impact resistance and long service life of the FRP anti-corrosion formwork are achieved.

CN118745815APending Publication Date: 2024-10-08GUANGXI BEIHAI YUEDA FRP PROD CO LTD
View PDF 5 Cites 0 Cited by

Patent Information

Application Number
CN202411025677.0
Authority / Receiving Office
CN · China
Patent Type
Applications(China)
Current Assignee / Owner
Filing Date
2024-07-30
Publication Date
2024-10-08

AI Technical Summary

Technical Problem

Existing wooden building formwork is prone to weathering and deformation, has low strength, is easily broken, and has poor finish, making it difficult to meet long-term use and high-strength requirements.

Method used

Using fiberglass anti-corrosion templates, a special primer and pre-treated fiberglass cloth are applied to the wooden template and cured under ultraviolet light radiation to form a template with high anti-corrosion performance, strength and pressure resistance.

Benefits of technology

It achieves multiple uses of the template, extends impact resistance and service life, prevents weathering deformation and moisture penetration, and has a smooth surface without bubbles, eliminating the need for frequent replacement.

✦ Generated by Eureka AI based on patent content.

Smart Images

  • Figure BDA0004968464970000051
    Figure BDA0004968464970000051
  • Figure BDA0004968464970000061
    Figure BDA0004968464970000061
Patent Text Reader

Abstract

The invention relates to the technical field of building templates, in particular to a glass fiber reinforced plastic anti-corrosion template which is a building template and comprises a wooden template, primer, glass fiber reinforced plastic cloth and a polyester film, and the primer, the glass fiber reinforced plastic cloth and the polyester film are used for processing the wooden template. The building formwork prepared through the method has the advantages of being good in corrosion resistance and high in strength and can be used repeatedly.
Need to check novelty before this filing date? Find Prior Art

Description

Technical Field

[0001] The invention relates to the technical field of building formwork, and in particular to a glass fiber reinforced plastic anti-corrosion formwork and a preparation method thereof. Background Art

[0002] Building formwork is often used in construction sites. It is a temporary support structure. The building formwork is made according to the design requirements, so that the concrete and components are formed according to the specified position and geometric size, and bear the weight of the building formwork and the external loads acting on it. On the one hand, the building formwork ensures that the concrete and components are formed and fixed according to the specified requirements, and on the other hand, it speeds up the construction progress and ensures construction safety. It is widely used in the field of construction technology.

[0003] In the prior art, in order to reduce the weight of the building formwork itself and facilitate the handling and transportation of the building formwork, the building formwork is made of wood material. Multiple formworks are spliced ​​together to allow concrete to solidify or components to be formed into specific shapes, which facilitates construction and improves construction efficiency and effects.

[0004] However, building formwork made of wooden materials is easily weathered and deformed, and has problems such as low strength, easy breakage and poor finish. Based on this, the present application proposes a fiberglass anti-corrosion formwork to solve the above problems. Summary of the invention

[0005] In view of the above, it is necessary to provide a glass fiber reinforced plastic anti-corrosion formwork and a preparation method thereof. The building formwork prepared by the method of the present application has the characteristics of good anti-corrosion performance and high strength, and can be used multiple times.

[0006] In order to achieve the above object, the technical solution adopted by the present invention is:

[0007] A glass fiber reinforced plastic anti-corrosion formwork, comprising a wooden formwork, a primer for treating the wooden formwork, a glass fiber reinforced plastic cloth and a polyester film;

[0008] The primer is prepared by mixing epoxy resin, bentonite, talcum powder and aromatic solvent in a mass ratio of 3-4:1:0.5-1:5-8 and then putting them into a reactor, then heating to 90-110°C, stirring and reacting for 0.5-1 hour to obtain a reactant, then adding pentaerythritol to the reactant, heating to 115-125°C, maintaining for 1-2 hours, then continuing to heat to 145-155°C for reaction for 2-3 hours, cooling to 50-60°C, then adding dibutyltin dilaurate, stirring evenly, finally cooling to room temperature, discharging, and obtaining the primer. Specifically, the epoxy resin is selected from bisphenol A diglycidyl ether.

[0009] Furthermore, the amount of pentaerythritol used is 0.1-0.2 times the total amount of reactants; the amount of dibutyltin dilaurate used is 0.2-0.4 times the total amount of reactants.

[0010] Furthermore, the fiberglass cloth is first treated as follows before use: the fiberglass cloth is soaked in deionized water at 5-8°C for 20-30 minutes, and then taken out and dried at 100-120°C.

[0011] Furthermore, the thickness of the fiberglass cloth is 0.2-0.4 mm.

[0012] The present application also provides a method for a glass fiber reinforced plastic anti-corrosion formwork, the method comprising the following steps:

[0013] (1) Primer: After sanding the wooden formwork, evenly apply primer on the wooden formwork;

[0014] (2) Adding fiberglass cloth: Lay fiberglass cloth on the wooden template in step (1), then lay polyester film, scrape it flat with a PVC scraper, and then use a roller to completely squeeze out the bubbles;

[0015] (3) Curing: The template treated in step (2) is cured, and then trimmed and inspected to obtain the finished FRP anti-corrosion template.

[0016] Furthermore, the step (3) is to cure by ultraviolet radiation.

[0017] The present invention has the following beneficial effects:

[0018] In the preparation process of the fiberglass anti-corrosion formwork of the present invention, first, it is polished and repaired and then painted with primer. The primer treatment gives the formwork good anti-corrosion performance. In addition, the primer prepared by the method of the present application has the characteristics of good fluidity. After multi-stage temperature rise and fall treatment, the wetting and dispersion effect of the primer can be improved. After use, the primer can penetrate various pores on the surface of the wooden formwork and close the pores on the surface. Then, a fiberglass cloth is further laid on the wooden formwork after the primer treatment. The used fiberglass cloth is pretreated in advance, cold soaked and then dried, and its molecular bonds are opened and covered on the wooden formwork painted with primer. There is good adhesion between the primer obtained by the treatment of the present application and the fiberglass cloth. The treated fiberglass cloth can allow the primer to penetrate into the fibers of the fiberglass cloth. The two have good compatibility, so that the fiberglass cloth can be effectively attached to the wooden formwork; the finally obtained fiberglass anti-corrosion formwork has the characteristics of low water permeability, smooth surface, high compressive strength, etc., can effectively isolate air and water from contact with the protected equipment materials, and has a long service life. DETAILED DESCRIPTION

[0019] All features disclosed in this specification, or steps in all methods or processes disclosed, except mutually exclusive features and / or steps, can be combined in any manner.

[0020] Any feature disclosed in this specification (including any appended claims and abstract), unless otherwise stated, is merely an example of a series of equivalent or similar features.

[0021] Embodiment 1:

[0022] The present embodiment provides a glass fiber reinforced plastic anti-corrosion formwork, which includes a wooden formwork and a primer for treating the wooden formwork, a glass fiber reinforced plastic cloth and a polyester film; the primer is prepared by mixing epoxy resin, bentonite, talcum powder and aromatic hydrocarbon solvent in a mass ratio of 3:1:0.5:5 and then putting the mixture into a reactor, then heating the mixture to 90°C and stirring the mixture for reaction for 0.5 hours to obtain a reactant, then adding pentaerythritol to the reactant, heating the mixture to 115°C and maintaining the mixture for 1 hour, then heating the mixture to 145°C and reacting the mixture for 2 hours, cooling the mixture to 50°C, then adding dibutyltin dilaurate and stirring the mixture, finally cooling the mixture to room temperature and discharging the mixture to obtain the primer; the amount of pentaerythritol is 0.1 times the total amount of the reactant; the amount of dibutyltin dilaurate is 0.2 times the total amount of the reactant; the thickness of the glass fiber reinforced plastic cloth is 0.2 mm.

[0023] Specifically, the preparation method is as follows:

[0024] (1) Primer: After sanding the wooden formwork, evenly apply primer on the wooden formwork;

[0025] (2) Pretreatment of FRP cloth: Soak the FRP cloth in deionized water at 5°C for 20 minutes, then take it out and dry it at 100°C;

[0026] (3) Adding fiberglass cloth: Lay 3 layers of fiberglass cloth on the wooden template in step (1), then lay polyester film, scrape it flat with a PVC scraper, and then use a roller to completely squeeze out the bubbles;

[0027] (4) Curing: The template treated in step (3) is cured by ultraviolet radiation, and then trimmed and inspected to obtain the finished fiberglass anti-corrosion template.

[0028] Embodiment 2:

[0029] The present embodiment provides a glass fiber reinforced plastic anti-corrosion formwork, which includes a wooden formwork and a primer for treating the wooden formwork, a glass fiber reinforced plastic cloth and a polyester film; the primer is prepared by mixing epoxy resin, bentonite, talcum powder and aromatic hydrocarbon solvent in a mass ratio of 3:1:1:6 and then putting the mixture into a reactor, then heating the mixture to 100°C, stirring and reacting the mixture for 0.7 hours to obtain a reactant, then adding pentaerythritol to the reactant, heating the mixture to 120°C, maintaining the temperature for 1.5 hours, then heating the mixture to 150°C and reacting the mixture for 2.5 hours, cooling the mixture to 55°C, then adding dibutyltin dilaurate, stirring the mixture evenly, finally cooling the mixture to room temperature, discharging the mixture, and obtaining the primer; the amount of pentaerythritol is 0.1 times the total amount of the reactants; the amount of dibutyltin dilaurate is 0.3 times the total amount of the reactants; the thickness of the glass fiber reinforced plastic cloth is 0.3 mm.

[0030] Specifically, the preparation method is as follows:

[0031] (1) Primer: After sanding the wooden formwork, evenly apply primer on the wooden formwork;

[0032] (2) Pretreatment of FRP cloth: soak the FRP cloth in deionized water at 6°C for 25 min, then take it out and dry it at 110°C;

[0033] (3) Adding fiberglass cloth: Lay 4 layers of fiberglass cloth on the wooden template in step (1), then lay polyester film, scrape it flat with a PVC scraper, and then use a roller to completely squeeze out the bubbles;

[0034] (4) Curing: The template treated in step (3) is cured by ultraviolet radiation, and then trimmed and inspected to obtain the finished fiberglass anti-corrosion template.

[0035] Embodiment 3:

[0036] The present embodiment provides a glass fiber reinforced plastic anti-corrosion formwork, which includes a wooden formwork and a primer for treating the wooden formwork, a glass fiber reinforced plastic cloth and a polyester film; the primer is prepared by mixing epoxy resin, bentonite, talcum powder and aromatic hydrocarbon solvent in a mass ratio of 4:1:1:8 and putting the mixture into a reactor, then heating the mixture to 110°C, stirring and reacting for 1 hour to obtain a reactant, then adding pentaerythritol to the reactant, heating the mixture to 125°C, maintaining the temperature for 2 hours, then continuing to heat the mixture to 155°C and reacting for 3 hours, cooling the mixture to 60°C, then adding dibutyltin dilaurate, stirring evenly, finally cooling the mixture to room temperature, discharging the mixture, and obtaining the primer; the amount of pentaerythritol is 0.2 times the total amount of the reactants; the amount of dibutyltin dilaurate is 0.4 times the total amount of the reactants; the thickness of the glass fiber reinforced plastic cloth is 0.4 mm.

[0037] Specifically, the preparation method is as follows:

[0038] (1) Primer: After sanding the wooden formwork, evenly apply primer on the wooden formwork;

[0039] (2) Pretreatment of FRP cloth: soak the FRP cloth in deionized water at 8°C for 30 min, then take it out and dry it at 120°C;

[0040] (3) Adding fiberglass cloth: Lay 5 layers of fiberglass cloth on the wooden template in step (1), then lay polyester film, scrape it flat with a PVC scraper, and then use a roller to completely squeeze out the bubbles;

[0041] (4) Curing: The template treated in step (3) is cured by ultraviolet radiation, and then trimmed and inspected to obtain the finished fiberglass anti-corrosion template.

[0042] Test example:

[0043] In order to illustrate the effect of this application, the applicant conducted the following comparative experiment to compare the quality of the FRP anti-corrosion formwork obtained by different treatment methods, and the groups are as follows:

[0044] The first group: the glass fiber reinforced plastic anti-corrosion formwork prepared in the manner described in Example 2 of the present application;

[0045] Group 2: The primer was prepared except for dibutyltin dilaurate, and the other methods were the same as those of Group 1;

[0046] Group 3: Remove the pretreatment of the fiberglass cloth, and other methods are the same as those of Group 1;

[0047] Group 4: The primer is prepared by mixing epoxy resin, bentonite, talcum powder and aromatic solvent in a mass ratio of 3:1:1:6 and then putting the mixture into a reactor, heating the mixture to 100°C and stirring the mixture for 0.7 hours. Other methods are the same as those of Group 1.

[0048] The fifth group: the primer is prepared by mixing epoxy resin, bentonite, talcum powder and aromatic solvent in a mass ratio of 3:1:1:6 and then putting them into a reactor, then heating to 100°C, stirring and reacting for 0.7 hours to obtain a reactant, then adding pentaerythritol into the reactant, cooling to 55°C, then adding dibutyltin dilaurate, stirring evenly, finally cooling to room temperature, discharging, and obtaining the primer; other methods are the same as the first group;

[0049] Group 6: No fiberglass sheet is added, other methods are the same as Group 1;

[0050] Group 7: Wooden formwork, no treatment is done.

[0051] Comparing the above groups of building formwork, the average impact resistance (GB / T 1732-2020), water absorption rate and number of uses after 10 tests, the recorded data are shown in Table 1:

[0052] Table 1

[0053]

[0054]

[0055] According to the data in Table 1, the building formwork prepared by the method of the present application has a longer service life and has excellent impact resistance, while the impact resistance of other groups is poor. The impact resistance of the second, fourth and fifth groups is good in the first 2-3 tests, but in the subsequent tests, the fiberglass cloth has poor adhesion and the impact resistance has decreased. It can also be seen from the table that the fiberglass anti-corrosion formwork prepared by the method of the present application will not mold after being stored for a long time. This is an effect that can only be achieved by using the primer in combination with the fiberglass anti-corrosion formwork; in addition, the method of the present application can extend the service life of the building formwork, from the original wooden board being scrapped after 30 uses to the fiberglass anti-corrosion formwork of the present application being used 80 times; and the applicant found that it is easy to demould during use, and the reinforced concrete surface is smooth, without bubbles or water lines.

[0056] The above-described embodiments only express several implementation methods of the present invention, and the description thereof is relatively specific and detailed, but it cannot be understood as limiting the scope of the present invention. It should be pointed out that, for a person of ordinary skill in the art, several modifications and improvements can be made without departing from the concept of the present invention, and these all belong to the protection scope of the present invention. Therefore, the protection scope of the present invention shall be subject to the attached claims.

Claims

1. A glass fiber reinforced plastic anti-corrosion formwork, characterized in that: The fiberglass anti-corrosion formwork comprises a wooden formwork and a primer, a fiberglass cloth and a polyester film for treating the wooden formwork; The primer is prepared by mixing epoxy resin, bentonite, talcum powder and aromatic hydrocarbon solvent in a mass ratio of 3-4:1:0.5-1:5-8 and then putting the mixture into a reactor, heating the mixture to 90-110°C, stirring the mixture for reaction for 0.5-1 hour to obtain a reactant, then adding pentaerythritol into the reactant, heating the mixture to 115-125°C, maintaining the mixture for 1-2 hours, then heating the mixture to 145-155°C for reaction for 2-3 hours, cooling the mixture to 50-60°C, then adding dibutyltin dilaurate, stirring the mixture evenly, finally cooling the mixture to room temperature, discharging the mixture, and obtaining the primer.

2. The glass fiber reinforced plastic anti-corrosion formwork according to claim 1, characterized in that: The amount of pentaerythritol used is 0.1-0.2 times the total amount of reactants; the amount of dibutyltin dilaurate used is 0.2-0.4 times the total amount of reactants.

3. According to the FRP anti-corrosion formwork described in claim 1, the FRP cloth is first treated as follows before use: the FRP cloth is soaked in deionized water at 5-8°C for 20-30 minutes, then taken out and dried at 100-120°C.

4. The glass fiber reinforced plastic anti-corrosion formwork according to claim 3 is characterized in that: The thickness of the fiberglass cloth is 0.2-0.4 mm.

5. A method for preparing the glass fiber reinforced plastic anticorrosive formwork according to any one of claims 1 to 4, characterized in that: The method comprises the following steps: (1) Primer: After sanding the wooden formwork, evenly apply primer on the wooden formwork; (2) Adding fiberglass cloth: Lay fiberglass cloth on the wooden template in step (1), then lay polyester film, scrape it flat with a PVC scraper, and then use a roller to completely squeeze out the bubbles; (3) Curing: The template treated in step (2) is cured, and then trimmed and inspected to obtain the finished FRP anti-corrosion template.

6. The method according to claim 5, characterized in that The step (3) is to cure by ultraviolet radiation.

Citation Information

Patent Citations

  • Novel safety glass decorative sheet and preparation method thereof

    CN103866939A

  • Varnish for wooden window frames, and preparation method thereof

    CN109111833A

  • Pump station runner construction method

    CN110952511A

  • High-solid low-viscosity universal primer and preparation method thereof

    CN116179081A

  • Glass fibre reinforced plastic multilayer wood forms

    CN2408175Y