Preparation method and application of asphalt-based hard carbon material
Through fractionation and multi-step processing of petroleum asphalt, high-quality pitch-based hard carbon materials are prepared, which solves the problems of low oxidation degree and low sodium storage capacity in the existing technology, and achieves high sodium storage capacity and high first-time efficiency. Effect.
Patent Information
- Application Number
- CN202410841978.4
- Authority / Receiving Office
- CN · China
- Patent Type
- Applications(China)
- Current Assignee / Owner
- Filing Date
- 2024-06-27
- Publication Date
- 2024-10-11
- Estimated Expiration
- 2044-06-27
AI Technical Summary
Existing asphalt-based hard carbon materials have problems such as low oxidation degree, uneven oxidation, and low sodium storage capacity during the preparation process, resulting in low sodium storage capacity and low first-time efficiency.
The petroleum asphalt is divided into light and heavy asphalt by vacuum distillation, which are subjected to cooling, crushing, oxidation and high-temperature carbonization respectively. After the light asphalt is melted, carbonized materials and organic sodium salts are added for stirring and oxidation, and then high-temperature carbonization is performed. , forming high-quality pitch-based hard carbon materials.
The quality of the pitch-based hard carbon material is stable and uniform, the sodium storage capacity and first efficiency are improved, a disordered structure and a rich pore structure are formed, and the electrochemical performance is enhanced.
Smart Images

Figure CN118754094A_ABST
Abstract
Description
Technical Field
[0001] The present invention relates to the technical field of preparation of asphalt-based hard carbon materials, and in particular to a preparation method and application of asphalt-based hard carbon materials. Background Art
[0002] As we all know, in recent years, with the rise of lithium-ion batteries in electric vehicles and energy storage, the demand for lithium-ion batteries has skyrocketed. The limited supply of lithium resources has become a constraint on the development of new energy. Sodium-ion batteries, as an electrochemical power source similar to lithium-ion batteries, have received more and more attention due to the abundance of sodium resources and almost no restrictions. Hard carbon is currently the most preferred negative electrode material for sodium-ion batteries. To facilitate the preparation of asphalt-based hard carbon materials, we propose a preparation method and application of asphalt-based hard carbon materials.
[0003] From the perspective of hard carbon precursor materials, there are currently three main types: bio-based, polymer resin-based and asphalt-based. Bio-based hard carbon is prepared from raw materials such as coconut shells, straws, and sugars, and has been commercialized as a negative electrode material for sodium batteries. However, the source of biomass raw materials is unstable and the carbon yield is low, which limits its large-scale application. Polymer resin-based hard carbon is prepared from polymer materials such as phenolic resin to prepare hard carbon negative electrode materials, which also shows good electrical properties, but has the problem of high raw material costs. Asphalt raw materials have a stable source, low cost, and high carbon yield, and are a very cost-effective raw material.
[0004] At present, asphalt-based hard carbon materials have low sodium storage capacity due to the fact that they easily form a highly ordered graphite-like structure. Current research shows that pre-oxidation, cross-linking agents, and heteroatom doping can effectively increase the disorder of the asphalt-based hard carbon material structure and increase the interlayer spacing of the carbon layers, thereby greatly improving the sodium storage capacity. Most of the existing pre-oxidation methods for preparing asphalt-based hard carbon materials have low oxidation degrees and uneven oxidation, and the obtained asphalt hard carbon materials generally have low first efficiency. Summary of the invention
[0005] 1. Technical issues to be resolved
[0006] In view of the shortcomings of the prior art, the present invention provides a preparation method and application of a pitch-based hard carbon material, which not only obtains a pitch-based hard carbon material with stable and uniform quality, but also has a high sodium storage capacity and high initial efficiency.
[0007] (II) Technical solution
[0008] To achieve the above object, the present invention provides the following technical solution: a method for preparing a pitch-based hard carbon material, comprising the following steps:
[0009] (1) subjecting petroleum asphalt to vacuum distillation, and taking light asphalt of the fraction at about 200°C to 350°C and heavy asphalt of the fraction above 500°C as carbon source precursors;
[0010] (2) cooling and crushing the heavy asphalt fraction, and introducing air into the fraction for oxidation treatment to obtain an oxidation product A;
[0011] (3) The pre-oxidized material A is subjected to high-temperature carbonization treatment in an inert gas atmosphere to obtain a carbonized material B;
[0012] (4) melting the light asphalt at high temperature, then adding carbonized material B and a certain amount of organic sodium salt, stirring and mixing, and then introducing air for oxidation treatment to obtain an oxidation product C;
[0013] (5) The oxidation product C is subjected to high-temperature carbonization treatment in an inert gas atmosphere to obtain a pitch-based hard carbon material.
[0014] Preferably, the petroleum asphalt is one or more of ethylene tar rich in aromatic components, catalytic oil slurry and the like.
[0015] Furthermore, the specific method of introducing air for oxidation treatment in step (2) is: the asphalt solid particles are 100-1000um, the air flow rate is 1-20L / min per 1kg of asphalt, the oxidation temperature is 300-400°C, and the time is 2-6h. The specific method of introducing air for oxidation treatment in step (4) is: the asphalt mixture is in a liquid molten state and is in a stirring state for the first hour, the air flow rate is 1-20L / min per 1kg of the mixture, the temperature is 200-300°C, and the time is 2-6h.
[0016] Preferably, the carbonization treatment method in step (3) and step (5) is: under nitrogen atmosphere, the carbonization temperature is 1100-1500° C., and the time is 1-10 h.
[0017] Furthermore, the high-temperature melting temperature in step (4) is 200-300°C, the added amounts of carbonized material B and organic sodium salt are in a mass ratio of light asphalt: carbonized material B: organic sodium salt = 40-50: 50-60: 1-10, and the types of organic sodium salt are organic sodium alcohol, sodium phenol and sodium acid such as sodium ethanol.
[0018] Preferably, the asphalt-based hard carbon material obtained in step (5) is used as the negative electrode material of a sodium ion battery.
[0019] An application process of a pitch-based hard carbon material comprises the following steps:
[0020] S1. The prepared asphalt-based hard carbon material was ground and slurried with acetylene black and sodium alginate in a mass ratio of 8:1:1;
[0021] S2. The prepared slurry was evenly coated on the surface of the copper foil and dried in vacuum at 100°C for 12 h to obtain a coated electrode, which was cut into small discs with a diameter of 12 mm, and then the CR2430 half-cell was assembled in an argon glove box;
[0022] S3. Sodium metal sheet was used as the counter electrode, the diaphragm was glass fiber, the electrolyte was 1 mol / L NaPF6 / DME, and the Blue Power CT2001A battery test system was used for charge and discharge tests with a voltage range of 0.01 to 2.5 V.
[0023] (III) Beneficial effects
[0024] Compared with the prior art, the present invention provides a preparation method and application of a pitch-based hard carbon material, which has the following beneficial effects:
[0025] 1. In the present invention, petroleum asphalt is selected from ethylene tar or catalytic oil slurry rich in aromatic components with high oxidation reaction activity and the asphalt is pretreated. The asphalt is divided into light asphalt with a low softening point and heavy asphalt with a high softening point according to the distillation range. Different oxidation and carbonization methods are adopted according to the characteristics of the two components. The heavy asphalt with a high softening point has a large molecular weight and is not easy to liquefy, so it is suitable for high-temperature gas-solid oxidation and is simple to operate. The heavy asphalt with a high softening point is crushed and then subjected to gas-solid contact oxidation in an air flow. The light asphalt with a low softening point has a small molecular weight and is easy to melt and liquefy and has a high oxidation reaction activity, so that the asphalt is fully and evenly oxidized, and the quality of the product after carbonization is more stable and uniform, and the interlayer spacing after carbonization is large, and the sodium storage capacity is high.
[0026] 2. In the present invention, low softening point light asphalt is melted and mixed into asphalt-based hard carbon material. The asphalt-based hard carbon material acts as a spatial barrier, making it difficult for light asphalt to form large streamlined structures during carbonization, preventing graphite crystals from growing and tending to form an overall disordered structure. The asphalt-based hard carbon material formed by the two fraction asphalts has different structures. The asphalt-based hard carbon material finally formed has a richer pore structure, thereby increasing the sodium storage space.
[0027] 3. In the present invention, sodium salt is mixed into the melted low-softening-point light asphalt. Since light asphalt is rich in polycyclic aromatic hydrocarbons such as naphthalene and phenanthrene, sodium phenolate and sodium alcoholate are easily formed. During carbonization in an inert atmosphere, a certain amount of chemical pre-sodiumization agent effect is formed under a reducing atmosphere, thereby improving the initial efficiency. BRIEF DESCRIPTION OF THE DRAWINGS
[0028] Figure 1 The present invention is a flow chart of the method for preparing the pitch-based hard carbon material. DETAILED DESCRIPTION
[0029] The following will be combined with the drawings in the embodiments of the present invention to clearly and completely describe the technical solutions in the embodiments of the present invention. Obviously, the described embodiments are only part of the embodiments of the present invention, not all of the embodiments. Based on the embodiments of the present invention, all other embodiments obtained by ordinary technicians in this field without creative work are within the scope of protection of the present invention.
[0030] Example 1
[0031] (1) subjecting ethylene tar to vacuum distillation, and taking light asphalt of the fraction at about 200°C to 350°C and heavy asphalt of the fraction above 500°C as carbon source precursors;
[0032] (2) 500 g of the heavy asphalt fraction above 500° C. was cooled and crushed, and the particle size of the asphalt particles after crushing was about 500 μm. The asphalt particles were placed in a high-temperature furnace at 350° C. and oxidized by passing air at 2 L / min for 4 hours to obtain an oxidized product A;
[0033] (3) The oxidized material A obtained in step (2) is subjected to high-temperature carbonization treatment at 1100° C. in a nitrogen atmosphere for 3 hours to obtain a carbonized material B;
[0034] (4) heating 500 g of the light asphalt to 200° C. for melting and liquefaction, then adding 400 g of the carbonized material B obtained in step (3) and 100 g of sodium phenolate and stirring and mixing for 1 hour, introducing 5 L / min of air during stirring for oxidation treatment for 4 hours to obtain an oxidation product C;
[0035] (5) subjecting the oxidized material C obtained in step (4) to a high-temperature carbonization treatment at 1200° C. in a nitrogen atmosphere for 3 hours to obtain a final pitch-based hard carbon material;
[0036] (6) The obtained pitch-based hard carbon material has a discharge specific capacity of 345.2 mAh / g and a first efficiency of 92.1%.
[0037] Example 2
[0038] (1) subjecting the catalytic oil slurry to vacuum distillation, and taking the light asphalt of the fraction at about 200° C. to 350° C. and the heavy asphalt of the fraction at above 500° C. as carbon source precursors;
[0039] (2) 500 g of the heavy asphalt fraction above 500° C. was cooled and crushed, and the particle size of the asphalt particles after crushing was about 600 μm. The asphalt particles were placed in a high-temperature furnace at 350° C. and oxidized by passing air at 2 L / min for 4 hours to obtain an oxidized product A;
[0040] (3) The oxidized material A obtained in step (2) is subjected to high-temperature carbonization treatment at 1100° C. in a nitrogen atmosphere for 3 hours to obtain a carbonized material B;
[0041] (4) heating 600 g of the light asphalt to 200° C. for melting and liquefaction, then adding 350 g of the carbonized material B obtained in step (3) and 50 g of sodium ethoxide and stirring and mixing for 1 hour, introducing 5 L / min of air during stirring for oxidation treatment for 4 hours to obtain an oxidation product C;
[0042] (5) subjecting the oxidized material C obtained in step (4) to a high-temperature carbonization treatment at 1200° C. in a nitrogen atmosphere for 3 hours to obtain a final pitch-based hard carbon material;
[0043] (6) The obtained pitch-based hard carbon material has a discharge specific capacity of 343.6 mAh / g and a first efficiency of 91.6%.
[0044] Comparative Example 1
[0045] (1) Using catalytic oil slurry as a carbon source precursor;
[0046] (2) cooling and crushing the catalytic oil slurry, the asphalt particles after crushing have a particle size of about 500 μm, placing it in a high-temperature furnace at 350° C. and introducing air at 2 L / min for oxidation treatment for 4 hours to obtain an oxidation product;
[0047] (3) The oxidized material obtained in step (2) is subjected to high-temperature carbonization treatment at 1100° C. in a nitrogen atmosphere for 3 hours to obtain a pitch-based hard carbon material;
[0048] (4) The obtained pitch-based hard carbon material has a discharge specific capacity of 305.2 mAh / g and a first efficiency of 78.1%.
[0049] Comparative Example 2
[0050] (1) subjecting the catalytic oil slurry to vacuum distillation, and taking the light asphalt of the fraction at about 200° C. to 350° C. and the heavy asphalt of the fraction at above 500° C. as carbon source precursors;
[0051] (2) mixing light asphalt and heavy asphalt in a mass ratio of 1:1, cooling and crushing, the asphalt particles after crushing have a particle size of about 600 μm, placing them in a 350° C. high-temperature furnace and passing 2 L / min of air for oxidation treatment for 4 hours to obtain an oxidation product;
[0052] (3) The oxidized material obtained in step (2) is subjected to high-temperature carbonization treatment at 1100° C. in a nitrogen atmosphere for 3 hours to obtain a pitch-based hard carbon material;
[0053] (4) The obtained pitch-based hard carbon material has a discharge specific capacity of 336.4 mAh / g and a first efficiency of 85.1%.
[0054] Performance Testing
[0055] Among them, the battery performance test: the prepared asphalt-based hard carbon material is used as the negative electrode, sodium is used as the positive electrode, NaPF6 with a concentration of 1 mol / L is dissolved in EC:DMC:PC=1:1:1, and 1% FEC is used as the electrolyte additive, the diaphragm is glass fiber (GF / A), the battery is assembled in a glove box filled with argon, and charge and discharge tests are carried out.
[0056] Although embodiments of the present invention have been shown and described, it will be appreciated by those skilled in the art that various changes, modifications, substitutions and variations may be made to the embodiments without departing from the principles and spirit of the present invention, and that the scope of the present invention is defined by the appended claims and their equivalents.
Claims
1. A method for preparing a pitch-based hard carbon material, characterized in that: The following steps are involved: (1) subjecting petroleum asphalt to vacuum distillation, and taking light asphalt of the fraction at about 200°C to 350°C and heavy asphalt of the fraction above 500°C as carbon source precursors; (2) cooling and crushing the heavy asphalt fraction, and introducing air into the fraction for oxidation treatment to obtain an oxidation product A; (3) The pre-oxidized material A is subjected to high-temperature carbonization treatment in an inert gas atmosphere to obtain a carbonized material B; (4) melting the light asphalt at high temperature, then adding carbonized material B and a certain amount of organic sodium salt, stirring and mixing, and then introducing air for oxidation treatment to obtain an oxidation product C; (5) The oxidation product C is subjected to high-temperature carbonization treatment in an inert gas atmosphere to obtain a pitch-based hard carbon material.
2. The method for preparing a pitch-based hard carbon material according to claim 1, characterized in that: The petroleum asphalt is a mixed product of ethylene tar rich in aromatic components and catalytic oil slurry.
3. The method for preparing a pitch-based hard carbon material according to claim 2, characterized in that: The specific method of introducing air for oxidation treatment in step (2) is: the asphalt solid particles are 100-1000um, the air flow rate is 1-20L / min per 1kg of asphalt, the oxidation temperature is 300-400°C, and the time is 2-6h. The specific method of introducing air for oxidation treatment in step (4) is: the asphalt mixture is in a liquid molten state, is in a stirring state for the first hour, the air flow rate is 1-20L / min per 1kg of the mixture, the temperature is 200-300°C, and the time is 2-6h.
4. The method for preparing a pitch-based hard carbon material according to claim 3, characterized in that: The carbonization treatment method in step (3) and step (5) is: under nitrogen atmosphere, the carbonization temperature is 1100-1500° C. and the time is 1-10 hours.
5. The method for preparing a pitch-based hard carbon material according to claim 4, characterized in that: The high temperature melting temperature in step (4) is 200-300°C, the added amount of carbonized material B and organic sodium salt is the mass ratio of light asphalt: carbonized material B: organic sodium salt = 40-50: 50-60: 1-10, and the types of organic sodium salt are organic sodium alcohol, sodium phenol and sodium acid such as sodium ethanol.
6. The method for preparing a pitch-based hard carbon material according to claim 5, characterized in that: The asphalt-based hard carbon material obtained in step (5) is used as the negative electrode material of the sodium ion battery.
7. An application process of a pitch-based hard carbon material, characterized in that: The pitch-based hard carbon material obtained by the method for preparing a pitch-based hard carbon material according to claims 1 to 6 comprises the following steps: S1. The prepared asphalt-based hard carbon material was ground and slurried with acetylene black and sodium alginate in a mass ratio of 8:1:1; S2. The prepared slurry was evenly coated on the surface of the copper foil and dried in vacuum at 100°C for 12 h to obtain a coated electrode, which was cut into small discs with a diameter of 12 mm, and then the CR2430 half-cell was assembled in an argon glove box; S3. Sodium metal sheet was used as the counter electrode, the diaphragm was glass fiber, the electrolyte was 1 mol / L NaPF6 / DME, and the Blue Power CT2001A battery test system was used for charge and discharge tests with a voltage range of 0.01 to 2.5 V.
Citation Information
Patent Citations
Preparation method of asphalt-based hard carbon material as well as obtained product and application of asphalt-based hard carbon material
CN117361500A
Carbonaceous negative electrode material for sodium secondary battery and method for producing the same
JP2014203530A
An improved carbon precursor material