Cu2 (CdxZn1-x) SnS4 film with component gradient as well as preparation method and application of Cu2 (CdxZn1-x) SnS4 film
Cu2(CdxZn1-x)SnS4 thin films were prepared through microwave liquid phase synthesis and spin coating methods, which solved the problems of element diffusion and high cost, achieved Cd gradient distribution and improved performance, and was suitable for industrial production.
Patent Information
- Application Number
- CN202410942957.1
- Authority / Receiving Office
- CN · China
- Patent Type
- Applications(China)
- Current Assignee / Owner
- Filing Date
- 2024-07-15
- Publication Date
- 2024-10-11
- Estimated Expiration
- 2044-07-15
AI Technical Summary
The existing technology has element diffusion problems when preparing Cu2ZnSnS4 thin films. It is difficult to form a Cd gradient, which affects the performance of the thin film. Moreover, the preparation process requires vacuum equipment, which is high in cost and has poor suitability.
Cu2ZnSnS4 and Cu2CdSnS4 nanoparticles are prepared using a microwave liquid phase synthesis method, nano-ink is formed by spin coating, a stacked structure is formed on the substrate, and a Cu2(CdxZn1-x)SnS4 film with a composition gradient is prepared by annealing without vacuum equipment. , reduce production costs.
The gradient distribution of Cd elements is achieved, which improves the performance of solar cells and photodetectors, reduces production costs, and is suitable for industrial mass production.
Smart Images

Figure CN118754190A_ABST
Abstract
Description
Technical Field
[0001] The present invention belongs to the field of photoelectric functional materials, and specifically relates to a Cu2(Cd x Zn 1-x )SnS4 thin film and its preparation method and application. Background Art
[0002] With the rapid development of science and technology, people's demand for energy is increasing, non-renewable energy is on the verge of exhaustion, and rising energy prices have become an important factor restricting the country's economic development; on the other hand, the concept of environmental protection is becoming more and more popular, and people are more concerned about a series of problems caused by greenhouse gases. my country has clearly put forward the goals of "carbon peak" in 2030 and "carbon neutrality" in 2060. Environmental protection has become another hot topic on the diplomatic negotiation table of various countries. Therefore, it is necessary to find a clean, green and cheap renewable energy. Solar energy has attracted widespread attention because of its huge reserves, green and pollution-free, and almost no geographical restrictions. Solar cells can directly convert solar energy into electrical energy, which has become a research hotspot in today's scientific community.
[0003] Cu2ZnSnS4 (CZTS) is regarded as an absorber material with great potential due to its abundant reserves, low cost and excellent photoelectric performance. CZTS is a group I-II-IV-VI quaternary semiconductor compound with a crystal structure similar to CIGS. Depending on the arrangement order of Cu and Zn inside it, there are two crystal structures: kesterite and stannitite (Solar RRL, 2023, 7(24): 2300670). However, due to its narrow single-phase region, pure CZTS material is prone to the appearance of other impurities during the reaction process, resulting in unsatisfactory film quality, which in turn limits device performance. On the other hand, there are interface defects at the CZTS / CdS interface, forming a "Cliff" band structure that reduces the carrier recombination barrier at the interface and affects carrier collection (Journal of Alloys and Compounds, 2020, 817:153329). Doping is a common strategy for regulating semiconductor performance. Adding Cd 2+ Doped into CZTS to form Cu2(Cd x Zn 1-x )SnS4 (CCZTS), since the size of Cd atoms is larger than that of Cu atoms (0.160nm), it will inhibit Cu to a certain extent. ZnThe formation of defects, increasing the grain size while reducing the film holes, and optimizing the band structure (Journal of Applied Physics, 2013, 114(18): 183506). Pilvet pointed out that with the increase of Cd 2+ The proportion of Cd in CCZTS gradually increases, and the band gap decreases linearly from 1.5 eV to 1.06 eV (Thin Solid Films, 2015, 582: 180-183). This continuously adjustable band gap is a huge advantage of Cd doping compared to other element doping. Therefore, different stacking structures, such as CZTS / CCTS, CZTS / CCTS / CZTS, etc., can be designed to achieve gradient control of the energy band.
[0004] At present, the main methods for preparing CCZTS thin films are concentrated on magnetron sputtering, sol-gel method, etc. The common point of their preparation principles is that after forming a layer of precursor film on the substrate, the desired phase is obtained through heat treatment and chemical reaction. This process can be summarized as a "film formation-reaction" process. This process will produce intense element diffusion inside the film, which is not conducive to the formation of Cd gradient. The process of preparing thin films by nano-ink method can be summarized as a "reaction-film formation" process, that is, the desired phase has been obtained in the ink before preparing the film, and then the film is formed on the substrate by physical methods. This "pre-phase" advantage can reduce the element diffusion during the heat treatment of the film, so the desired element distribution inside the film can be obtained through reasonable experimental design. The preparation of Cu2ZnSnS4 and Cu2CdSnS4 nanoparticles is the key to the nanoparticle ink method. Our research group uses microwave liquid phase synthesis to control the preparation of Cu2ZnSnS4 and Cu2CdSnS4 nanoparticles of different shapes and sizes (Journal of Nanoparticle Research, 2014, 16: 2437). Summary of the invention
[0005] Purpose of the invention: The technical problem to be solved by the present invention is to provide a Cu2(Cd x Zn 1-x )SnS4 thin film and its preparation method do not require vacuum equipment, have low production cost, short preparation cycle, and are suitable for industrial large-scale production.
[0006] In order to achieve the above object, the technical solution adopted by the present invention is as follows: A Cu2(Cd x Zn 1-x ) The method for preparing SnS4 thin film comprises the following steps: (1) Ultrasonic cleaning is used to obtain a clean substrate; (2) Preparation of Cu2ZnSnS4 and Cu2CdSnS4 nanoparticles: using a copper-containing compound as a copper source, a zinc-containing compound as a zinc source, a tin-containing compound as a tin source, a sulfur-containing compound as a sulfur source, and polyvinyl pyrrolidone as a surfactant, dissolving them in a first organic solvent in sequence, and using a microwave liquid phase synthesis method to prepare Cu2ZnSnS4 nanoparticles; using a copper-containing compound as a copper source, a cadmium-containing compound as a cadmium source, a tin-containing compound as a tin source, a sulfur-containing compound as a sulfur source, and polyvinyl pyrrolidone as a surfactant, dissolving them in a first organic solvent in sequence, and using a microwave liquid phase synthesis method to prepare Cu2CdSnS4 nanoparticles; (3) Preparation of Cu2ZnSnS4 and Cu2CdSnS4 nano-inks: Dispersing the prepared Cu2ZnSnS4 nano-particles and Cu2CdSnS4 nano-particles in a second organic solvent to prepare Cu2ZnSnS4 nano-ink and Cu2CdSnS4 nano-ink respectively; (4) Preparation of a prefabricated thin film with a Cu2CdSnS4 and Cu2ZnSnS4 stacked structure: the prepared Cu2ZnSnS4 nano-ink and Cu2CdSnS4 nano-ink are sequentially applied to a substrate by a spin coating method to form a prefabricated thin film with a Cu2CdSnS4 and Cu2ZnSnS4 stacked structure; (5) Annealing treatment: annealing the Cu2CdSnS4 and Cu2ZnSnS4 laminated structure prefabricated film obtained in step (4) under a protective atmosphere to obtain; The Cu2(Cd x Zn 1-x )In SnS4 thin film, the value range of x is 0<x<1.
[0007] Specifically, in step (1), the substrate is soda-lime glass coated with a molybdenum film, and the substrate is ultrasonically cleaned in sequence using soap water, deionized water, ethanol, and deionized water.
[0008] Specifically, in step (2), the copper-containing compound is copper nitrate, copper chloride or copper acetate, the tin-containing compound is stannous chloride or tin chloride, the zinc-containing compound is zinc chloride or zinc acetate, the cadmium-containing compound is cadmium chloride or cadmium acetate, the sulfur-containing compound is one or a combination of two or more of thioacetamide, L-cysteine and 3-mercaptopropionic acid, and the first organic solvent is ethylene glycol.
[0009] Furthermore, in step (2), the prepared Cu2ZnSnS4 nanoparticles and Cu2CdSnS4 nanoparticles are annealed in an inert atmosphere at a temperature of 200-400°C and an annealing time of 20-60 min.
[0010] Preferably, in step (3), the second organic solvent is any one of n-propanol, triethanolamine, and ethylene glycol methyl ether, or a combination of two or more thereof.
[0011] Preferably, in step (3), the concentration of Cu2ZnSnS4 nanoparticles in the Cu2ZnSnS4 nano-ink is 50-500 mg / mL; the concentration of Cu2CdSnS4 nanoparticles in the Cu2CdSnS4 nano-ink is 50-500 mg / mL.
[0012] It should be noted that the preparation process of the above-mentioned Cu2ZnSnS4 nanoparticles and Cu2CdSnS4 nanoparticles can refer to the prior art document Wei Wang, Honglie Shen, Xiancong He, Jinze Li. Effects ofsulfur sources on properties of Cu2ZnSnS4nanoparticles[J]. Journal ofNanoparticle Research, 2014, 16: 2437.
[0013] Specifically, in step (4), the prepared Cu2ZnSnS4 nano-ink is applied to the substrate by spin coating, and then dried at 200-350°C for 1-5 min, and the above steps are repeated 5-15 times to form a Cu2ZnSnS4 prefabricated film with a certain thickness; then the Cu2CdSnS4 nano-ink is applied to the Cu2ZnSnS4 prefabricated film, and then dried at 200-350°C for 1-5 min, and the above steps are repeated 5-15 times to form a Cu2CdSnS4 prefabricated film with a certain thickness, so as to obtain a Cu2(Cd x Zn 1-x )SnS4 film, that is, the Cd concentration gradually increases from the film surface to the back; or, The coating order of the above Cu2ZnSnS4 nano-ink and Cu2CdSnS4 nano-ink was exchanged, and the conditions were the same to obtain Cu2(Cd x Zn 1-x ) SnS4 film, that is, the Cd concentration gradually decreases from the film surface to the back; or, The Cu2(Cd2SnS4) nano-ink, Cu2CdSnS4 nano-ink, and Cu2ZnSnS4 nano-ink are sequentially coated on the prefabricated film to obtain a Cu2(Cd2SnS4) nano-ink with a Cd "reverse V" gradient distribution. x Zn 1-x )SnS4 film, that is, the Cd concentration increases first and then decreases from the film surface to the back; or, The Cu2CdSnS4 nano-ink, Cu2ZnSnS4 nano-ink, and Cu2CdSnS4 nano-ink are sequentially coated on the prefabricated film to obtain a Cu2(Cd x Zn 1-x )SnS4 film, that is, the Cd concentration first decreases and then increases from the surface to the back of the film.
[0014] Preferably, in step (5), the annealing treatment is carried out in an inert gas or sulfur atmosphere, the annealing temperature is 610-630° C., the time is 30-70 min, and the gas pressure is 10-100 kPa.
[0015] Furthermore, the Cu2(Cd x Zn 1-x )SnS4 thin film is also within the protection scope of the present invention.
[0016] Furthermore, the present invention also claims the above-mentioned Cu2(Cd x Zn 1-x )Application of SnS4 thin film in the preparation of solar cells, photodetectors, and photo-splitting water anodes.
[0017] The principle of the present invention is as follows: Preparation of Cu2(Cd x Zn 1-x )The main methods for SnS4 thin films are currently concentrated on magnetron sputtering, sol-gel method, etc. The common point of their preparation principles is that after a layer of precursor film is formed on the substrate, the desired phase is obtained through heat treatment and chemical reaction. This process can be summarized as a "film formation-reaction" process. This process will produce intense element diffusion inside the film, which is not conducive to the formation of Cd gradient. The process of preparing thin films by the nano-ink method can be summarized as a "reaction-film formation" process, that is, the desired phase has been obtained in the ink before preparing the film, and then the film is formed on the substrate by physical methods. This "pre-phase formation" advantage can reduce the element diffusion during the heat treatment of the film, so the desired element distribution inside the film can be obtained through reasonable experimental design. The Cd element distribution gradient makes the band gap gradient distribution. The band gap gradient will affect the built-in electric field strength and the degree of light absorption of the solar cell, and finally prepare high-performance Cu2(Cd x Zn 1-x )SnS4 thin film. Beneficial Effects
[0018] (1) The present invention proposes a Cu2(Cd x Zn 1-x)SnS4 solar cell absorption layer Cd element gradient distribution preparation method, the method does not require vacuum equipment, low production cost, short preparation cycle, suitable for industrial large-scale production, preparation of Cu2 (Cd x Zn 1-x )The materials used in SnS4 thin films are cheap and easily available, which greatly reduces the production cost of solar cells and has good application prospects.
[0019] (2) The present invention makes full use of the advantages of nano-ink to store Cu2(Cd) with controllable distribution of Cd element within a certain range. x Zn 1-x )SnS4 film. The positive bandgap gradient inside the film will form an electric field inside the absorption layer. This additional electric field will increase the diffusion distance of carriers and help improve the collection efficiency of carriers. The negative bandgap gradient inside the film gradually decreases the bandgap, so there is less recombination at the pn junction interface and the open circuit voltage is improved. BRIEF DESCRIPTION OF THE DRAWINGS
[0020] The present invention will be further described in detail below in conjunction with the accompanying drawings and specific embodiments, and the above and / or other advantages of the present invention will become more clear.
[0021] Figure 1 The Cu2(Cd 0.3 Zn 0.7 )Scanning electron microscope (SEM) image of a cross section of a SnS4 solar cell.
[0022] Figure 2 The Cu2(Cd 0.3 Zn 0.7 )Energy dispersive spectrometer (EDS) line scan curve of SnS4 thin film.
[0023] Figure 3 Schematic diagram of the process of preparing Cu2ZnSnS4 thin film in Example 1: from bottom to top, glass substrate 1, back electrode Mo film 2, spin-coated Cu2ZnSnS4 (Cu2CdSnS4) film 3, spin-coated Cu2CdSnS4 (Cu2ZnSnS4) 4, and Cu2(CdSnS4) obtained after annealing. x Zn 1-x )SnS4 thin film 5.
[0024] Figure 4 The Cu2(Cd x Zn 1-x )X-ray diffraction (XRD) pattern of SnS4 thin film.
[0025] Figure 5The Cu2(Cd x Zn 1-x )Raman spectrum of SnS4 thin film.
[0026] Figure 6 The Cu2(Cd x Zn 1-x )Scanning electron microscope (SEM) image of the cross section of SnS4 thin film.
[0027] Figure 7 The Cu2(Cd x Zn 1-x )Energy dispersive spectrometer (EDS) line scan curve of SnS4 thin film.
[0028] Figure 8 The Cu2(Cd x Zn 1-x )Enlarged view of the line scan curve of the cross-sectional energy dispersive spectrometer (EDS) of SnS4 film for Cd and Zn elements.
[0029] Fig. 9 The Cu2(Cd x Zn 1-x )External quantum efficiency (EQE) curve of SnS4 solar cells.
[0030] Fig.10 The Cu2(Cd x Zn 1-x )Photocurrent response curves of SnS4 photodetector under 650 nm wavelength light and different power tests. DETAILED DESCRIPTION
[0031] The present invention can be better understood with reference to the following examples. Comparative Example
[0032] Preparation of Cu2(Cd 0.3 Zn 0.7 )SnS4 nanoparticles, the specific process parameters are as follows: weigh 0.7 mmol zinc acetate, 0.3 mmol cadmium acetate, 1 mmol stannous chloride, 1.8 mmol copper nitrate, 12 mmol thioacetamide and 0.6 g polyvinyl pyrrolidone and dissolve them in 50 mL ethylene glycol, stir evenly and put them into a microwave oven for heating, the microwave power is 800 W, the reaction time is 30 min, centrifuge and wash with ultrapure water to obtain Cu2(Cd 0.3 Zn 0.7The obtained nanoparticles were annealed at 300°C in a nitrogen atmosphere for 30 min, and the cleaned nanoparticles were dispersed in a mixed solvent of n-propanol and triethanolamine at a concentration of 50 mg / mL to prepare Cu2(Cd 0.3 Zn 0.7 )SnS4 nano-ink.
[0033] The prepared Cu2(Cd 0.3 Zn 0.7 )SnS4 nano-ink was spin-coated onto soda-lime glass coated with Mo film and dried at 300℃ for 2 min. This process was repeated 20 times to obtain Cu2(Cd 0.3 Zn 0.7 )SnS4 prefabricated film.
[0034] The prepared Cu2(Cd 0.3 Zn 0.7 ) The SnS4 prefabricated film was placed in the high temperature zone of a double-temperature zone vacuum tube annealing furnace and annealed in a sulfur atmosphere. The temperature was raised to 620 °C at 10 °C / min and kept at that temperature for 50 min. The sulfurization gas pressure was 20 kPa, and then the film was cooled to room temperature with the furnace. Figure 1 The Cu2(Cd 0.3 Zn 0.7 )SEM image of the cross section of the SnS4 solar cell. From the image, it can be seen that the layers of the device are clearly layered and in good contact. The bottom of the absorption layer is a fine-grained layer, and the top is a large-grained layer. Figure 2 This is the element distribution curve of the electron energy spectrum (EDS) of the absorption layer section. It can be seen that Cu2(Cd 0.3 Zn 0.7 ) The elements in the SnS4 film are evenly distributed and the proportions are in line with expectations. The film was prepared into solar cells and photodetectors. Example 1
[0035] Cu2ZnSnS4 nanoparticles were prepared by microwave liquid phase synthesis, 1 mmol zinc acetate was weighed, cadmium acetate was not weighed, and the other parameters were the same as the comparative example. Then the prepared nanoparticles were washed several times with deionized water and ethanol, the cleaned nanoparticles were annealed in a nitrogen atmosphere at 300°C for 30min, and dispersed in n-propanol at a concentration of 50 mg / mL to prepare Cu2ZnSnS4 nanoink. For Cu2CdSnS4 nanoparticles, 1 mmol cadmium acetate was weighed, zinc acetate was not weighed, and the other parameters were the same as the comparative example. Then the prepared nanoparticles were washed several times with deionized water and ethanol, the cleaned nanoparticles were annealed in a nitrogen atmosphere at 300°C for 30min, and dispersed in a mixed solvent of n-propanol and triethanolamine at a concentration of 50 mg / mL to prepare Cu2CdSnS4 nanoink.
[0036] The prepared Cu2CdSnS4 nano-ink was spin-coated onto the soda-lime glass coated with Mo film, dried at 300°C for 2 min, and the process was repeated 10 times; then the prepared Cu2ZnSnS4 nano-ink was spin-coated onto the Cu2CdSnS4 nano-film, also dried at 300°C for 2 min, and the process was repeated 10 times. A prefabricated film with a Cu2CdSnS4 / Cu2ZnSnS4 laminated structure was obtained.
[0037] Finally, the prepared Cu2CdSnS4 / Cu2ZnSnS4 stacked prefabricated film was placed in the high temperature zone of a double-temperature zone vacuum tube annealing furnace and annealed in a sulfur atmosphere. The temperature was raised to 620°C at 10°C / min and kept at that temperature for 50 min. The sulfurization gas pressure was 20 KPa, and then the film was cooled to room temperature with the furnace. Figure 3 Schematic diagram of the process of preparing Cu2ZnSnS4 thin film in this embodiment: from bottom to top, glass substrate 1, back electrode Mo film 2, spin-coated Cu2ZnSnS4 (Cu2CdSnS4) film 3, spin-coated Cu2CdSnS4 (Cu2ZnSnS4) 4, and Cu2 (Cd x Zn 1-x )SnS4 thin film 5.
[0038] Figure 4 The Cu2(Cd x Zn 1-x )SnS4 film XRD spectrum, the prepared film has obvious diffraction peaks, the diffraction peaks are sharp, indicating good crystallinity, the main diffraction peak is located between the main peaks of Cu2ZnSnS4 with kesterite structure and Cu2CdSnS4 with kesterite structure, it can be considered that Cu2(Cd x Zn 1-x )SnS4 thin film was successfully prepared. Figure 5 The prepared Cu2(Cd x Zn 1-x ) Raman spectrum of SnS4 thin film at 291 cm -1 、330 cm -1 and 361 cm -1 There are three Raman peaks at , which also correspond to Cu2ZnSnS4 with kesterite structure and Cu2CdSnS4 with kesterite structure. Figure 6 This is a SEM picture of the cross section of a Cu2ZnSnS4 solar cell. It can be seen from the figure that the various layers of the device are in good contact. Compared with the control example, the fine grain layer inside the absorption layer disappears and is transformed into a grain layer with an average grain size of the upper and lower layers. Figure 7The element distribution curve of the electron energy spectrum (EDS) test of the absorption layer section is the element distribution of Cu, Cd, Zn, Sn, and S. From 0-1μm, it is from the Mo electrode to the film surface. It can be seen that the element content of the film meets the requirements of Cu2(Cd x Zn 1-x ) The stoichiometric ratio of SnS4 material, the content of Cd and Zn elements is equivalent; Figure 8 It is an enlarged curve of the distribution of Cd and Zn element components. It is found that with the increase of the test depth, the Cd content decreases and the Zn content increases. The element distribution presents an obvious gradient distribution. The x value on the surface is 0.48, and the x value in the film close to the Mo layer is 0.56. The performance parameters of the solar cells obtained in the comparative example and embodiment 1 are shown in Table 1. By comparison, it can be seen that the performance of the solar cell prepared in embodiment 1 is significantly improved compared with the comparative example.
[0039] Table 1 Cu2(Cd x Zn 1-x )Performance parameters of SnS4 / CdS heterojunction solar cells Example 2
[0040] The parameters for preparing Cu2ZnSnS4 and Cu2CdSnS4 nanoparticles by microwave liquid phase synthesis are the same as those in Example 1. The prepared nanoparticles are then washed multiple times with deionized water and ethanol, annealed for 30 min in a nitrogen atmosphere at 300°C, and dispersed in a mixed solvent of n-propanol and triethanolamine at a concentration of 50 mg / mL to prepare Cu2ZnSnS4 and Cu2CdSnS4 nanoinks.
[0041] The prepared Cu2CdSnS4 nano-ink was spin-coated onto a glass substrate coated with a Mo film, dried at 300°C for 2 min, and this process was repeated 10 times; the prepared Cu2ZnSnS4 nano-ink was spin-coated onto a Cu2CdSnS4 nano-film, dried at 100°C for 10 min, and this process was repeated 10 times. A prefabricated film with a Cu2CdSnS4 / Cu2ZnSnS4 laminated structure was obtained.
[0042] Finally, the prepared Cu2CdSnS4 / Cu2ZnSnS4 laminated prefabricated film was placed in a vacuum tube annealing furnace and annealed in a sulfur atmosphere. The temperature was raised to 620°C at 10°C / min, kept for 50 min, and the annealing pressure was 20 kPa, and then cooled to room temperature with the furnace. The film was prepared as a photodetector, and the performance parameters of the photodetector obtained in the comparative example and Example 2 are shown in Table 2. Using an electron spectrometer (EDS) test, the Cd content on the surface of the film was high, with an x value of 0.53. Near the bottom layer, the Cd content in the film decreased, with an x value of 0.49.
[0043] Table 2 Cu2(Cd x Zn 1-x )Performance parameters of SnS4 / CdS heterojunction photodetector
[0044] By comparison, it can be seen that the two groups of samples have good light stability in the visible light range, and both have the best response to 650 nm wavelength light. The specific detection rate of Example 2 is one order of magnitude higher than that of the comparative example. This is because the positive gradient distribution will strengthen the built-in electric field, increase the separation efficiency of carriers, reduce the recombination of carriers, improve the responsiveness of the device, and ultimately improve the specific detection rate. Example 3
[0045] The parameters for preparing Cu2ZnSnS4 and Cu2CdSnS4 nanoparticles by microwave liquid phase synthesis are the same as those in Example 1. Then, the prepared nanoparticles are washed several times with deionized water and ethanol, annealed for 30 min in a nitrogen atmosphere at 300°C, and dispersed in a mixed solvent of n-propanol and triethanolamine at a concentration of 50 mg / mL to prepare Cu2ZnSnS4 and Cu2CdSnS4 nano-inks.
[0046] The prepared Cu2ZnSnS4 nano-ink was spin-coated onto soda-lime glass coated with Mo film, dried at 300 ℃ for 2 min, and this process was repeated 7 times; the prepared Cu2CdSnS4 nano-ink was spin-coated onto Cu2ZnSnS4 nano-film, dried at 300 ℃ for 2 min, and this process was repeated 7 times; the prepared Cu2ZnSnS4 nano-ink was spin-coated onto Cu2CdSnS4 nano-film, dried at 300 ℃ for 2 min, and this process was repeated 7 times to obtain a prefabricated film with a Cu2ZnSnS4 / Cu2CdSnS4 / Cu2ZnSnS4 stacked structure.
[0047] Finally, the prepared Cu2ZnSnS4 / Cu2CdSnS4 / Cu2ZnSnS4 stacked prefabricated film was placed in a vacuum tube annealing furnace and annealed in a sulfur atmosphere. The temperature was raised to 620 °C at 10 °C / min and kept at this temperature for 50 min. The annealing pressure was 20 kPa, and then the film was cooled to room temperature in the furnace.
[0048] It was prepared into a solar cell, and the device parameters were shown in Table 3.
[0049] Table 3 Cu2(Cd x Zn 1-x )Performance parameters of SnS4 / CdS heterojunction solar cells
[0050] By comparison, it can be seen that the performance of the solar cell prepared in Example 3 is significantly improved compared with that of the comparative example. The solar cell is tested for EQE (External Quantum Efficiency), which can reflect the proportion of photons received on the surface of the solar cell that are converted into current. The results are as follows: Fig. 9 As shown in the figure, the "inverse V" gradient of the Cd element can enhance the absorption of light by the solar cell. The integral current obtained by integrating the curve is consistent with the actual short-circuit current, which explains why the short-circuit current obtained in Example 3 is nearly twice that of the comparative example. In addition, Example 3 has stronger absorption of short-wavelength light, which is opposite to the comparative example, indicating that the recombination at this time mainly occurs at the back interface of the absorption layer. Example 4
[0051] The parameters for preparing Cu2ZnSnS4 and Cu2CdSnS4 nanoparticles by microwave liquid phase synthesis are the same as those in Example 1. Then, the prepared nanoparticles are washed several times with deionized water and ethanol, annealed for 30 min in a nitrogen atmosphere at 300°C, and dispersed in a mixed solvent of n-propanol and triethanolamine at a concentration of 50 mg / mL to prepare Cu2ZnSnS4 and Cu2CdSnS4 nano-inks.
[0052] The prepared Cu2CdSnS4 nano-ink was deposited on a soda-lime glass substrate by spin coating, dried at 300 ℃ for 2 min, and the process was repeated 7 times; the prepared Cu2ZnSnS4 nano-ink was spin coated on a Cu2CdSnS4 nano-film, dried at 300 ℃ for 2 min, and the process was repeated 7 times; the prepared Cu2CdSnS4 nano-ink was spin coated on a Cu2ZnSnS4 nano-film, dried at 300 ℃ for 2 min, and the process was repeated 7 times to obtain a prefabricated film with a Cu2CdSnS4 / Cu2ZnSnS4 / Cu2CdSnS4 stacked structure.
[0053] Finally, the prepared Cu2CdSnS4 / Cu2ZnSnS4 / Cu2CdSnS4 stacked prefabricated film was placed in the high temperature zone of a double-temperature zone vacuum tube annealing furnace and annealed in a sulfur atmosphere. The temperature was raised to 620 °C at 10 °C / min and kept at this temperature for 50 minutes. The sulfurization gas pressure was 20 kPa, and then the film was cooled to room temperature with the furnace.
[0054] It was prepared as a photodetector, and the obtained photoelectric response efficiency is shown in Table 4.
[0055] Table 4 Cu2(Cd x Zn 1-x )Performance parameters of SnS4 / CdS heterojunction photodetector
[0056] By comparison, it can be seen that the device with a "positive V" gradient of the Cd element obtained in Example 4 has a good light response in the visible light range, and has the best response to light with a wavelength of 650nm, and the specific detection rate is one order of magnitude higher than that of the comparative example. Subsequently, the photoelectric response of different powers under light with a wavelength of 650nm was tested, such as Fig.10 As shown in the figure, under the same wavelength of light, the photodetector prepared in Example 4 changes linearly with different powers, indicating that the performance of the device is stable under different powers. Example 5
[0057] Cu2ZnSnS4 nanoparticles were prepared by microwave liquid phase synthesis. 1 mmol zinc chloride, 1 mmol tin chloride, 1.8 mmol cuprous chloride, 12 mmol 3-mercaptopropionic acid and 0.6 g polyvinyl pyrrolidone were dissolved in 50 mL of ethylene glycol, stirred evenly and then heated in a microwave oven. The microwave power was 800 W and the reaction time was 30 min. The mixture was centrifuged and washed with ultrapure water and ethanol to obtain Cu2ZnSnS4 nanoparticles. For Cu2CdSnS4 nanoparticles, 1 mmol cadmium chloride, 1 mmol tin chloride, 1.8 mmol cupric chloride, 12 mmol 3-mercaptopropionic acid and 0.6 g polyvinyl pyrrolidone were dissolved in 50 mL of ethylene glycol, stirred evenly and then heated in a microwave oven. The microwave power was 800 W and the reaction time was 30 min. The mixture was centrifuged and washed with ultrapure water and ethanol to obtain Cu2ZnSnS4 nanoparticles. The obtained nanoparticles were annealed in a nitrogen atmosphere at 200 °C for 60 min, and the cleaned nanoparticles were dispersed in a mixed solvent of n-propanol and triethanolamine at a concentration of 500 mg / mL to prepare Cu2ZnSnS4 and Cu2CdSnS4 nano-inks.
[0058] The prepared Cu2CdSnS4 nano-ink was spin-coated onto the soda-lime glass coated with Mo film, dried at 350°C for 1 min, and the process was repeated 7 times; then the prepared Cu2ZnSnS4 nano-ink was spin-coated onto the Cu2CdSnS4 nano-film, also dried at 350°C for 1 min, and the process was repeated 7 times. A prefabricated film with a Cu2CdSnS4 / Cu2ZnSnS4 laminated structure was obtained.
[0059] Finally, the prepared Cu2CdSnS4 / Cu2ZnSnS4 stacked prefabricated film was placed in a vacuum tube annealing furnace and annealed under the protection of hydrogen sulfide atmosphere. The temperature was raised to 610 ℃ at 10 ℃ / min and kept at this temperature for 70 min. The annealing pressure was 10 kPa, and then the film was cooled to room temperature with the furnace. Example 6
[0060] Cu2ZnSnS4 nanoparticles were prepared by microwave liquid phase synthesis. 1 mmol zinc acetate, 1 mmol stannous chloride, 1.8 mmol copper acetate, 12 mmol L-cysteine and 0.6g polyvinyl pyrrolidone were dissolved in 50 mL of ethylene glycol, stirred evenly and then heated in a microwave oven. The microwave power was 800 W and the reaction time was 30 min. After centrifugation, the mixture was fully washed with ultrapure water and ethanol to obtain Cu2ZnSnS4 nanoparticles. For Cu2CdSnS4 nanoparticles, 1 mmol cadmium acetate, 1 mmol stannous chloride, 1.8 mmol copper acetate, 12 mmol L-cysteine and 0.6g polyvinyl pyrrolidone were dissolved in 50 mL of ethylene glycol. After stirring evenly, the mixture was heated in a microwave oven. The microwave power was 800 W and the reaction time was 30 min. After centrifugation, the mixture was fully washed with ultrapure water and ethanol to obtain Cu2ZnSnS4 nanoparticles. The obtained nanoparticles were annealed at 400 °C in a nitrogen atmosphere for 20 min, and the cleaned nanoparticles were dispersed in a mixed solvent of n-propanol and triethanolamine at a concentration of 100 mg / mL to prepare Cu2ZnSnS4 and Cu2CdSnS4 nanoinks.
[0061] The prepared Cu2CdSnS4 nano-ink was spin-coated onto soda-lime glass coated with Mo film, dried at 200 ℃ for 5 min, and this process was repeated 15 times; the prepared Cu2ZnSnS4 nano-ink was spin-coated onto the Cu2CdSnS4 prefabricated film, dried at 200 ℃ for 5 min, and this process was repeated 5 times to obtain a prefabricated film with a Cu2CdSnS4 / Cu2ZnSnS4 stacked structure.
[0062] Finally, the prepared Cu2CdSnS4 / Cu2ZnSnS4 stacked prefabricated film was placed in a vacuum tube annealing furnace and annealed in a nitrogen atmosphere. The temperature was raised to 630°C at 10°C / min and kept at that temperature for 30 min. The annealing pressure was 100 kPa, and then the film was cooled to room temperature with the furnace.
[0063] The present invention provides a Cu2(Cd x Zn 1-x ) SnS4 thin film and its preparation method and application ideas and methods, there are many methods and ways to implement the technical solution, the above is only the preferred embodiment of the present invention, it should be pointed out that for ordinary technicians in this technical field, without departing from the principle of the present invention, several improvements and modifications can be made, and these improvements and modifications should also be regarded as the protection scope of the present invention. All components not specified in this embodiment can be implemented by existing technologies.
Claims
1. A Cu2(Cd x Zn 1-x ) A method for preparing a SnS4 thin film, characterized in that: The steps include: (1) Ultrasonic cleaning is used to obtain a clean substrate; (2) Preparation of Cu2ZnSnS4 and Cu2CdSnS4 nanoparticles: using a copper-containing compound as a copper source, a zinc-containing compound as a zinc source, a tin-containing compound as a tin source, a sulfur-containing compound as a sulfur source, and polyvinyl pyrrolidone as a surfactant, dissolving them in a first organic solvent in sequence, and using a microwave liquid phase synthesis method to prepare Cu2ZnSnS4 nanoparticles; using a copper-containing compound as a copper source, a cadmium-containing compound as a cadmium source, a tin-containing compound as a tin source, a sulfur-containing compound as a sulfur source, and polyvinyl pyrrolidone as a surfactant, dissolving them in a first organic solvent in sequence, and using a microwave liquid phase synthesis method to prepare Cu2CdSnS4 nanoparticles; (3) Preparation of Cu2ZnSnS4 and Cu2CdSnS4 nano-inks: Dispersing the prepared Cu2ZnSnS4 nano-particles and Cu2CdSnS4 nano-particles in a second organic solvent to prepare Cu2ZnSnS4 nano-ink and Cu2CdSnS4 nano-ink respectively; (4) Preparation of a prefabricated thin film with a Cu2CdSnS4 and Cu2ZnSnS4 stacked structure: the prepared Cu2ZnSnS4 nano-ink and Cu2CdSnS4 nano-ink are sequentially applied to a substrate by a spin coating method to form a prefabricated thin film with a Cu2CdSnS4 and Cu2ZnSnS4 stacked structure; (5) Annealing treatment: annealing the Cu2CdSnS4 and Cu2ZnSnS4 laminated structure prefabricated film obtained in step (4) under a protective atmosphere to obtain; The Cu2(Cd x Zn 1-x )In SnS4 thin film, the value range of x is 0<x<1.
2. The Cu2(Cd2O3) with composition gradient according to claim 1 x Zn 1-x ) A method for preparing a SnS4 thin film, characterized in that: In step (1), the substrate is soda-lime glass coated with a molybdenum film, and the substrate is ultrasonically cleaned in sequence using soap water, deionized water, ethanol, and deionized water.
3. The Cu2(Cd2O3) with composition gradient according to claim 1 x Zn 1-x ) A method for preparing a SnS4 thin film, characterized in that: In step (2), the copper-containing compound is copper nitrate, copper chloride or copper acetate, the tin-containing compound is stannous chloride or tin chloride, the zinc-containing compound is zinc chloride or zinc acetate, the cadmium-containing compound is cadmium chloride or cadmium acetate, the sulfur-containing compound is one or a combination of two or more of thioacetamide, L-cysteine and 3-mercaptopropionic acid, and the first organic solvent is ethylene glycol.
4. The Cu2(Cd2O3) with composition gradient according to claim 1 x Zn 1-x ) A method for preparing a SnS4 thin film, characterized in that: In step (2), the prepared Cu2ZnSnS4 nanoparticles and Cu2CdSnS4 nanoparticles are annealed in an inert atmosphere at a temperature of 200-400°C and an annealing time of 20-60 min.
5. The Cu2(Cd2O3) with composition gradient according to claim 1 x Zn 1-x ) A method for preparing a SnS4 thin film, characterized in that: In step (3), the second organic solvent is any one of n-propanol, triethanolamine, and ethylene glycol methyl ether, or a combination of two or more thereof.
6. The Cu2(Cd2O3) with composition gradient according to claim 1 x Zn 1-x ) A method for preparing a SnS4 thin film, characterized in that: In step (3), the concentration of Cu2ZnSnS4 nanoparticles in the Cu2ZnSnS4 nano-ink is 50-500 mg / mL; the concentration of Cu2CdSnS4 nanoparticles in the Cu2CdSnS4 nano-ink is 50-500 mg / mL.
7. The Cu2(Cd2O3) with composition gradient according to claim 1 x Zn 1-x ) A method for preparing a SnS4 thin film, characterized in that: In step (4), the prepared Cu2ZnSnS4 nano-ink is applied to the substrate by spin coating, and then dried at 200-350°C for 1-5 min, and the above steps are repeated 5-15 times to form a Cu2ZnSnS4 prefabricated film with a certain thickness; then the Cu2CdSnS4 nano-ink is applied to the Cu2ZnSnS4 prefabricated film, and then dried at 200-350°C for 1-5 min, and the above steps are repeated 5-15 times to form a Cu2CdSnS4 prefabricated film with a certain thickness, so as to obtain a Cu2(Cd x Zn 1-x )SnS4 thin film; or, The coating order of the above Cu2ZnSnS4 nano-ink and Cu2CdSnS4 nano-ink was exchanged, and the conditions were the same to obtain Cu2(Cd x Zn 1-x )SnS4 thin film; or, The Cu2ZnSnS4 nano-ink, Cu2CdSnS4 nano-ink, and Cu2ZnSnS4 nano-ink are sequentially coated on the prefabricated film to obtain a Cu2(Cd x Zn 1-x )SnS4 thin film; or, The Cu2CdSnS4 nano-ink, Cu2ZnSnS4 nano-ink, and Cu2CdSnS4 nano-ink are sequentially coated on the prefabricated film to obtain a Cu2(Cd x Zn 1-x )SnS4 thin film.
8. The Cu2(Cd2O3) with composition gradient according to claim 1 x Zn 1-x ) A method for preparing a SnS4 thin film, characterized in that: In step (5), the annealing treatment is carried out in an inert gas or sulfur atmosphere, the annealing temperature is 610-630°C, the time is 30-70 min, and the gas pressure is 10-100 kPa.
9. The Cu2(Cd2O3) with composition gradient prepared by the preparation method according to any one of claims 1 to 8 x Zn 1-x )SnS4 thin film.
10. The Cu2(Cd2O3) with composition gradient according to claim 9 x Zn 1-x )Application of SnS4 thin film in the preparation of solar cells, photodetectors, and photo-splitting water anodes.