Carbonized light material and preparation method thereof
By regulating the water-to-solid ratio and generating nano-calcium carbonate crystals, combined with industrial exhaust carbonization and maintenance, the problem of insufficient molding and carbon absorption rates of existing carbonized lightweight materials has been solved, and the preparation of carbonized lightweight materials with high performance and low carbon emissions has been achieved.
Patent Information
- Application Number
- CN202410782436.4
- Authority / Receiving Office
- CN · China
- Patent Type
- Applications(China)
- Current Assignee / Owner
- Filing Date
- 2024-06-18
- Publication Date
- 2024-10-11
- Estimated Expiration
- 2044-06-18
AI Technical Summary
It is difficult to match the gas generation process and slurry thickening and hardening when molding existing carbonized lightweight materials, resulting in performance degradation or molding defects. In addition, carbonization products wrap around the surface of material particles, inhibiting the reaction rate, resulting in insufficient carbon absorption rate.
By adjusting the water-to-solid ratio, the capillary structure is controlled, and carbonizable calcium materials, pozzolanic materials, thickeners and soluble carbonates are used to form an ultra-high water-to-solid ratio system, generate nano-calcium carbonate crystals, promote the carbonization reaction, and improve carbonization. performance, and uses industrial exhaust gas to absorb carbon dioxide during the carbonization curing process.
It achieves both good mechanical properties and durability under low bulk density, simplifies the preparation process, avoids molding defects, increases the degree of carbonization and carbon absorption, and reduces carbon emissions.
Smart Images

Figure BDA0004897545960000041
Abstract
Description
Technical Field
[0001] The invention belongs to the technical field of building materials, and in particular relates to a carbonized lightweight material and a preparation method thereof. Background Art
[0002] At present, the commonly used lightweight building materials (autoclaved aerated concrete, sintered bricks, etc.) will emit a large amount of carbon dioxide during the production process. With the increasing severity of global climate change and pollution, the development of low-carbon lightweight materials is imperative. Carbonization of industrial tail gas to maintain lightweight materials can absorb carbon dioxide during the material production process, which has become an important research direction.
[0003] When existing carbonized lightweight materials are formed, pores are usually introduced physically or chemically to control the bulk density. However, this method has certain problems, such as the difficulty in matching the gas generation process with the slurry thickening and hardening process, resulting in performance degradation or molding defects. In addition, during the carbonization reaction, the carbonization products will be wrapped on the surface of the carbonized material particles, the reaction rate will be inhibited, and the carbon absorption rate will be insufficient. Summary of the invention
[0004] The main purpose of the present invention is to provide a carbonized lightweight material and a preparation method thereof in view of the problems and shortcomings of the prior art. By adjusting the water-to-solid ratio to control the capillary structure, good mechanical properties and durability are taken into account while ensuring a low bulk density. The preparation method involved is relatively simple and easy to operate, and is suitable for promotion and application.
[0005] To achieve the above object, the technical solution adopted by the present invention is:
[0006] A carbonized light material, the raw materials and their weight proportions include: 30-35 parts of carbonizable calcium material, 5-10 parts of volcanic ash material, 0.2-1 part of thickener, 1-3 parts of soluble carbonate, and 60-65 parts of water.
[0007] In the above scheme, the carbonizable calcium material includes but is not limited to steel slag, magnesium slag, and calcium carbide mud, wherein the carbonizable component (C 3 S.C. 2 S.C. 3 S 2 , CS, CH, etc.) is not less than 75%, and the specific surface area is 400-700m 2 / kg.
[0008] Preferably, the carbonizable components in the carbonizable calcareous material are C 3 S.C. 2 The total content of S is not less than 70%, and the specific surface area is 550-650m 2 / kg.
[0009] In the above scheme, the volcanic ash material includes but is not limited to fly ash, slag, silica fume, and kaolin, with a specific surface area of not less than 500m 2 / kg, activity index not less than 85%.
[0010] In the above scheme, the thickener is cellulose ether, with a 1% solid content, a room temperature thickening capacity of 2 to 20 Pa·s, a thixotropic index of 1.5 to 4.5, and a molecular weight of 100,000 to 300,000.
[0011] In the above scheme, the soluble carbonate is a normal salt and / or an acid salt (bicarbonate); wherein the normal salt includes but is not limited to one or more of sodium carbonate, potassium carbonate, ammonium carbonate, lithium carbonate, etc.; the acid salt includes but is not limited to one or more of sodium bicarbonate, potassium bicarbonate, ammonium bicarbonate, lithium bicarbonate, etc. The effective component is required to be not less than 85%.
[0012] The above-mentioned method for preparing a carbonized lightweight material comprises the following preparation steps:
[0013] (1) weighing a carbonizable calcium material, a volcanic ash material, a thickener, a soluble carbonate, and water according to a ratio and stirring them uniformly to obtain a slurry;
[0014] (2) heating the obtained slurry under stirring conditions and keeping the temperature constant;
[0015] (3) pouring the heated slurry into a mold and curing it, and demolding it after hardening to obtain a green body;
[0016] (4) The green body is carbonized and cured to obtain a carbonized lightweight material product.
[0017] In the above scheme, in step (1), the slurry is stirred for 10 to 20 minutes, and the stirring rate is 60 to 90 r / min.
[0018] In the above scheme, in step (2), the heating method of the slurry is not limited, such as high-temperature steam heating or high-temperature air heating, with a heating rate of 5 to 15°C / min, and keeping the temperature at 70 to 80°C for 5 to 10 minutes. The stirring rate during the slurry heating process is controlled at 30 to 60 r / min.
[0019] Furthermore, the temperature of the high-temperature steam is 100-150°C; the temperature of the high-temperature air is 150-200°C.
[0020] Furthermore, the water-to-solid ratio of the slurry after heat preservation in step (2) is 1.2 to 1.5.
[0021] In the above scheme, in step (3), the static curing time is 2.5 to 3.5 hours, the temperature in the curing room is 80 to 90° C., and the relative humidity is 90 to 100%.
[0022] In the above scheme, in step (4), the gas used for carbonization curing is not limited, such as industrial carbon-containing tail gas or industrial-grade carbon dioxide. The carbon dioxide concentration in the carbonization gas is not less than 15 vol%, the carbonization curing time is 6 to 12 hours, the curing temperature is 60 to 90° C., the curing pressure is 0.3 to 0.7 MPa, and the relative humidity is 40 to 60%.
[0023] The performance optimization mechanism of the carbonized lightweight material of the present invention includes:
[0024] 1) Under the regulation of the nano calcium carbonate crystals generated by the thickener and soluble carbonate, the effective molding under the ultra-high water-to-solid ratio conditions of the present invention (slurry after heat preservation and heating) is achieved, and no water seepage and stratification phenomenon occurs. The bulk density of the material is adjusted by a large number of capillaries formed by water. The capillary pores are small in diameter, which effectively reduces the stress concentration phenomenon at the pore wall of the porous material under load, which is beneficial to improve the strength. The cellulose ether thickener contains a large number of -OH groups, and the electrostatic effect and Ca 2+ The coordination increases the local supersaturation and promotes the nucleation of calcite products in the early stage of carbonization curing. In addition, the alkyl groups contained in cellulose ether can significantly reduce the surface tension and interfacial energy of water, resulting in a decrease in the surface energy of calcite crystals, which is conducive to the stable growth of crystals; the introduced cellulose ether can promote the nucleation and growth of calcite products and improve the carbonization performance.
[0025] 2) The present invention adopts an ultra-high water-to-solid ratio formulation system, so that a large amount of liquid phase exists in the slurry, which promotes the double decomposition reaction between the soluble carbonate and the carbonizable calcium material, and uniformly generates a large amount of nano calcium carbonate in the liquid phase. Due to its large specific surface area, the slurry consistency is further increased. When used in combination with a thickener, the slurry has higher stability and better molding effect.
[0026] 3) The nano-calcium carbonate evenly dispersed in the liquid phase acts as a crystal nucleus to deposit part of the carbonization product on its surface, promoting a more uniform distribution of the carbonization product in the liquid phase, further reducing the pore size of the internal capillary pores of the green body, thereby improving the carbonization performance. The crystal nucleus effect makes the carbonization product no longer mainly concentrated on the surface of the carbonizable calcium material particles, and the thickness of the carbonization product layer on the particle surface is reduced, making it easier for calcium ions to diffuse through the carbonization product layer and react with carbon dioxide to form calcium carbonate, which is beneficial to shorten the carbonization curing time, improve the carbonization degree and carbon absorption.
[0027] 4) After the double decomposition reaction of soluble carbonate, a large amount of soluble alkali is generated, which can be used as an alkali activator to promote the hydration reaction of volcanic ash materials. The presence of a large amount of liquid phase provides sufficient space for the accumulation of hydration products. The hydration products and carbonization products are mutually cemented, which further improves the performance of lightweight materials. In addition, in the presence of soluble alkali, the solubility of carbon dioxide increases, which also promotes the carbonization reaction.
[0028] Compared with the prior art, the present invention has the following beneficial effects:
[0029] 1) The molding process is simple, the capillaries in the slurry are evenly distributed, and it is not easy to cause problems such as collapse and deformation during the pore making process of conventional porous materials, thus ensuring the stability of performance.
[0030] 2) Carbonizable materials are mostly industrial solid wastes, such as steel slag, magnesium slag, calcium carbide mud, etc., which have significant economic and environmental benefits.
[0031] 3) During the carbonization maintenance process of lightweight materials, carbon dioxide in industrial exhaust gas can be absorbed, which is beneficial to reducing carbon emissions. DETAILED DESCRIPTION
[0032] The present invention will be further described in detail below in conjunction with the embodiments to facilitate a clearer understanding of the present invention, but they do not limit the present invention.
[0033] In the following embodiments and comparative examples, the carbonizable calcium material is steel slag, and its main chemical composition and mass percentage include: 2 S 58%, C 3 S16%, Ca(OH) 2 5%, C 3 S 2 5%, Ca 2 Fe 2 O 5 6%, CaCO 3 5%, SiO 2 4%, its specific surface area is 580m 2 / kg; the volcanic ash materials are metakaolin and slag, of which the specific surface area of metakaolin is 630m 2 / kg, activity index 92%, slag specific surface area 560m 2 / kg, activity index 96%. Cellulose ether is produced by Zhengzhou Yuxiang Chemical Products Company, with a thickening capacity of 12Pa·s at 1% solid content, a thixotropic index of 2.1, and a molecular weight of 200,000. The soluble carbonate is sodium carbonate, with an effective ingredient of 92%. The carbonization gas uses cement kiln industrial tail gas, with a temperature of 75°C, a relative humidity of 45%, and a carbon dioxide concentration of 19vol%.
[0034] Example 1
[0035] A carbonized lightweight material based on capillary pore regulation, the preparation method of which comprises the following steps:
[0036] 1) 32 parts of steel slag, 6 parts of metakaolin, 0.6 parts of cellulose ether, 2 parts of sodium carbonate and 60 parts of water were mixed to obtain a slurry, wherein the mixing time was 15 min and the stirring rate was 60 r / min;
[0037] 2) The slurry is heated by 120℃ high-temperature steam with a heating rate of 10℃ / min, and kept warm for 10min when heated to 75℃; the stirring rate during the slurry heating process is controlled at 30r / min; the water-to-solid ratio of the slurry after insulation is 1.25;
[0038] 3) After the slurry is cast and formed, it is placed in a static room for curing for 3 hours. The temperature in the curing room is 85°C and the relative humidity is 95%;
[0039] 4) The green body obtained by demoulding after hardening is subjected to carbonization curing with industrial tail gas from a cement kiln to obtain a carbonized lightweight material, wherein the carbonization curing time is 8 hours and the pressure is 0.5 MPa.
[0040] Example 2
[0041] A carbonized lightweight material based on capillary pore regulation, the preparation method of which is substantially the same as that of Example 1, except that the carbonization curing time is 12 hours and the pressure is 0.5 MPa.
[0042] Example 3
[0043] A carbonized lightweight material based on capillary pore regulation, the preparation method of which is roughly the same as that of Example 1, except that: 32 parts of steel slag, 6 parts of slag, 0.6 parts of cellulose ether, 2 parts of sodium carbonate, and 60 parts of water are mixed evenly to obtain a slurry.
[0044] Comparative Example 1
[0045] A carbonized lightweight material based on capillary pore regulation, the preparation method of which is substantially the same as that of Example 1, except that the thickener used is triphenyl phenol polyoxyethylene ether methacrylate, which has a thickening capacity of 9 Pa·s at 1% solid content and a thixotropic index of 2.9.
[0046] Comparative Example 2
[0047] A carbonized lightweight material based on capillary pore regulation, the preparation method of which is substantially the same as that of Example 1, except that no volcanic ash material is used.
[0048] Comparative Example 3
[0049] A carbonized lightweight material based on capillary pore regulation, the preparation method of which is substantially the same as that of Example 1, except that: no soluble carbonate is used.
[0050] Comparative Example 4
[0051] A carbonized lightweight material based on capillary pore regulation, whose preparation method is roughly the same as that of Example 1, except that: the slurry is heated by high-temperature air (200°C) with a heating rate of 10°C / min, and is kept warm for 10 minutes when heated to 75°C; the stirring rate is controlled at 30r / min during the slurry heating process; and the water-to-solid ratio of the slurry after insulation is 0.9.
[0052] The carbonized aerated concrete obtained in Examples 1 to 3 and Comparative Examples 1 to 4 was subjected to performance tests, and the results are shown in Table 1.
[0053] Table 1 Carbonized lightweight material performance test results
[0054]
[0055] The above embodiments are only examples for clear explanation, and are not intended to limit the implementation methods. For ordinary technicians in the relevant field, other different forms of changes or modifications can be made based on the above description. It is not necessary and impossible to list all the implementation methods here, so the obvious changes or modifications derived are still within the protection scope of the invention.
Claims
1. A carbonized lightweight material, characterized in that: The raw materials and their weight proportions include: 30-35 parts of carbonizable calcium material, 5-10 parts of volcanic ash material, 0.2-1 part of thickener, 1-3 parts of soluble carbonate and 60-65 parts of water.
2. The carbonized lightweight material according to claim 1, characterized in that: The carbonizable component content of the carbonizable calcium material is not less than 75wt%, and the specific surface area is 400-700m 2 / kg.
3. The carbonized lightweight material according to claim 1, characterized in that: The specific surface area of the volcanic ash material is not less than 500m 2 / kg, activity index not less than 85%.
4. The carbonized lightweight material according to claim 1, characterized in that: The thickener is cellulose ether, with a 1% solid content and a room temperature thickening capacity of 2 to 20 Pa·s and a thixotropic index of 1.5 to 4.
5.
5. The carbonized lightweight material according to claim 1, characterized in that: The soluble carbonate is a normal salt and / or an acid salt.
6. The method for preparing a carbonized lightweight material according to any one of claims 1 to 5, characterized in that: The method comprises the following preparation steps: (1) weighing a carbonizable calcium material, a volcanic ash material, a thickener, a soluble carbonate, and water according to a ratio and stirring them uniformly to obtain a slurry; (2) heating the obtained slurry under stirring conditions and keeping the temperature constant; (3) pouring the heated slurry into a mold and curing it, and demolding it after hardening to obtain a green body; (4) The green body is carbonized and cured to obtain a carbonized lightweight material product.
7. The preparation method according to claim 6, characterized in that: In step (2), the heating temperature is 70-80° C. and the insulation time is 5-10 min.
8. The preparation method according to claim 6, characterized in that: The water-to-solid ratio of the slurry after heat preservation in step (2) is 1.2 to 1.
5.
9. The preparation method according to claim 6, characterized in that: In step (3), the static curing time is 2.5 to 3.5 hours, the temperature in the curing room is 80 to 90° C., and the relative humidity is 90 to 100%.
10. The preparation method according to claim 6, characterized in that: In step (4), in the carbonization curing step, the carbon dioxide concentration in the carbonization gas is not less than 15 vol%, the carbonization curing time is 6 to 12 hours, the curing temperature is 60 to 90° C., the curing pressure is 0.3 to 0.7 MPa, and the relative humidity is 40 to 60%.
Citation Information
Patent Citations
CO2-driven consolidated lightweight concrete and preparation method thereof
CN113968701A
Solid waste-based concrete lightweight wallboard and preparation method thereof
CN116444242A
High-strength carbonized aerated concrete and preparation method thereof
CN117185755A
Fiber-reinforced cement composition, concrete structure, and method for producing concrete base material
JP2005008486A
Carbonation hardening body and manufacturing method thereof
JP2023049167A