Preparation method of high-purity graphite material

Through the pressurized kneading and roasting process of carbonaceous aggregates and chemical modifiers, the interfacial functional groups and free radical transition layers are constructed, which solves the problems of long preparation cycle, high cost and low homogeneity in the preparation of high-purity graphite materials, and improves It improves the flexural strength, compressive strength and density of graphite materials.

CN118754666AActive Publication Date: 2024-10-11HUNAN UNIV

Patent Information

Application Number
CN202410990964.9
Authority / Receiving Office
CN · China
Patent Type
Applications(China)
Current Assignee / Owner
Filing Date
2024-07-23
Publication Date
2024-10-11
Estimated Expiration
2044-07-23

AI Technical Summary

Technical Problem

The existing high-purity graphite material preparation process has problems such as long preparation cycle, high production cost and low material homogeneity. Moreover, the traditional pressurized kneading method results in low bonding strength between asphalt and aggregate, which affects the comprehensive performance of graphite materials.

Method used

Carbonaceous aggregates are mixed with chemical modifiers and then kneaded under pressure. Chemical modifiers are used to build interfacial functional groups and free radical transition layers to promote the uniform combination and carbonization of asphalt and aggregates, and achieve tight connection through pressure roasting. Reduce the number of roasting times and improve the overall performance of the material.

Benefits of technology

The preparation process of high-purity graphite materials is simplified, the cycle is shortened, the cost is reduced and the comprehensive performance is improved, and graphite materials with high flexural strength, compressive strength and density are prepared.

✦ Generated by Eureka AI based on patent content.

Smart Images

  • Figure CN118754666A_ABST
    Figure CN118754666A_ABST
Patent Text Reader

Abstract

The invention discloses a preparation method of a high-purity graphite material, which comprises the following steps: (1) mixing carbon aggregate and asphalt, and carrying out pressurized mixing and kneading to obtain a paste material; (2) rolling, crushing and sieving the paste obtained in the step (1) to obtain pressed powder; performing cold isostatic pressing treatment on the pressed powder to obtain a green block; (3) carrying out pressure roasting on the green block obtained in the step (2) to obtain a roasted block; and (4) carrying out graphitization treatment on the roasted block obtained in the step (3) to obtain the high-purity graphite material. According to the preparation method disclosed by the invention, by virtue of a synergistic effect of pressurized kneading and pressurized roasting, the asphalt is more uniformly spread on the surface of the carbon aggregate and infiltrated into pores of the carbon aggregate to form a sintering neck, and pressurized roasting promotes carbonization and ring formation of the asphalt, so that tight connection of different aggregates is realized, and the homogeneity of the material is improved; the high-purity graphite material which does not need to be impregnated and roasted for multiple times is prepared.
Need to check novelty before this filing date? Find Prior Art

Description

Technical Field

[0001] The invention belongs to the field of carbon materials, and in particular relates to a method for preparing a graphite material. Background Art

[0002] High-purity graphite materials are materials with a carbon content of more than 99.9%. They have the advantages of low resistivity, good thermal shock resistance, high mechanical strength, high temperature resistance, corrosion resistance, self-lubrication, and easy precision machining. They are widely used in single crystal furnace heaters, metal continuous casting graphite crystallizers, hydrogen fuel cell electrode plates, graphite electrodes for EDM, and national defense science and technology and nuclear industry. With the development of new energy and technological progress in my country, the demand for high-purity graphite materials has increased at an annual rate of 20%, and the existing high-purity graphite output is far from meeting market demand. At present, the preparation of high-purity graphite materials in China continues the traditional process, with asphalt as a binder and calcined coke as aggregate, and undergoes screening, batching, kneading, sheeting, grinding, molding, roasting, impregnation, graphitization and purification. In order to achieve high density and high strength, it is necessary to impregnate and roast the roasted samples of carbon graphite materials for multiple times, which not only prolongs the preparation cycle, increases energy consumption, and increases production costs, but also leads to reduced homogeneity of graphite materials.

[0003] Patent application CN116573937A proposes an efficient method for preparing special carbon and its kneading process, wherein the raw materials are kneaded, crushed, formed, roasted, impregnated and graphitized; modified asphalt is used as a binder and kneaded under pressure with coke powder, so that the modified asphalt is uniformly infiltrated into the pores of the coke powder and uniformly coated on the particle surface of the coke powder; the physical and chemical properties of the product are greatly improved, the structure of the product is dense, the yield is improved, and it has good industrialization prospects. However, the pressurized kneading method adopted in this patent makes the asphalt and aggregate only a simple physical bond, and the bonding strength is low, which greatly affects the comprehensive performance of the graphite material.

[0004] Therefore, the existing technology needs to be improved, and it is urgent to improve the preparation efficiency of high-purity graphite materials and improve their comprehensive performance from the perspective of raw material modification and preparation process improvement. Therefore, it is of great significance to provide a method for preparing high-purity graphite materials with a simple preparation process, short preparation cycle, low production cost and excellent comprehensive performance. Summary of the invention

[0005] The technical problem to be solved by the present invention is to overcome the deficiencies and defects mentioned in the above background technology and provide a method for preparing a high-purity graphite material with a simple preparation process, a short preparation cycle, a low production cost and excellent comprehensive performance.

[0006] In order to solve the above technical problems, the technical solution proposed by the present invention is:

[0007] A method for preparing a high-purity graphite material comprises the following steps:

[0008] (1) mixing carbonaceous aggregate and asphalt and kneading them under pressure to obtain a paste;

[0009] (2) rolling, crushing and sieving the paste obtained in step (1) to obtain pressed powder; and cold isostatic pressing the pressed powder to obtain a green body block;

[0010] (3) pressurizing and calcining the green block obtained in step (2) to obtain a calcined block;

[0011] (4) The calcined block obtained in step (3) is graphitized to obtain a high-purity graphite material.

[0012] In the above preparation method, preferably, the carbonaceous aggregate is first mixed with a chemical modifier and then mixed with asphalt for pressurized kneading, the chemical modifier includes an organic modifier and / or an inorganic modifier, the organic modifier includes one or more of oleic acid, washing oil and nitronaphthalene, the inorganic modifier includes ammonium persulfate, and the mass ratio of the chemical modifier to the carbonaceous aggregate is (1-5):100.

[0013] The present invention first mixes carbonaceous aggregate with chemical modifier, and the chemical modifier constructs interface functional groups and free radical transition layers between primary and secondary aggregates, and has high chemical activity and wettability. When asphalt infiltrates the gap between aggregates during pressurized mixing, the aggregates and liquid asphalt are fully adsorbed and evenly spread. In the subsequent pressurized roasting, the self-sintering behavior of the interface functional groups and free radical transition layers, due to the homogeneity of the combination of asphalt and aggregate during pressurized mixing, inhibits the rapid migration of light components of asphalt, and makes the product uniform. The groups in the chemical modifier can promote decomposition and polycondensation reactions, etc., increase the carbonization ring rate of asphalt, increase the residual carbon content of asphalt, shorten the roasting time, and improve the yield rate. That is, the present invention first mixes carbonaceous aggregate with chemical modifier, and uses chemical modifier to modify aggregate, which is conducive to improving the effect of pressurized mixing and pressurized roasting, and improving the synergistic effect of the two.

[0014] In the above preparation method, more preferably, the chemical modifier includes an organic modifier and an inorganic modifier, the organic modifier is washing oil, the inorganic modifier is ammonium peroxydisulfate, and the mass ratio of the washing oil to the ammonium peroxydisulfate is 1:(0.5-3). More preferably, the mass ratio of the washing oil to the ammonium peroxydisulfate is 1:2. In a more preferred scheme, washing oil and ammonium peroxydisulfate are used in combination, and the synergistic effect of the two has a better modification effect on the aggregate. Specifically, the washing oil acts as a lubricant in the pressurized kneading stage, which can reduce the friction between the aggregate particles, improve the fluidity of the mixture, make it easier for ammonium peroxydisulfate and asphalt to penetrate between the aggregates to form a close contact, and prevent the aggregate particles from breaking during the kneading process. The intact particles help to maintain the original characteristics of their surface, so that the ammonium peroxydisulfate reacts more efficiently with the aggregate surface to form a functional group and free radical transition layer. During the subsequent pressurized kneading to promote the reaction between the modifier and the aggregate, some low-boiling hydrocarbon molecules in the wash oil will begin to evaporate, while higher-boiling hydrocarbon molecules will not volatilize. The wash oil partially volatilizes and decomposes, and the released light hydrocarbons and volatile components cooperate with ammonium persulfate under pressure to promote the formation of the interface functional groups and free radical transition layer. The non-volatile part continues to act as a lubricant, improves the fluidity of the mixture, and can improve the mass transfer efficiency during the subsequent pressurized roasting. During the subsequent pressurized kneading to promote the reaction between the modifier and the aggregate, the ammonium persulfate will decompose to produce ammonia and sulfate ions; the ammonia will react with the carbon atoms of the aggregate to form amino functional groups, which can react with the functional groups produced by the asphalt. The covalent bonds of ammonia break at about 200°C and the free radicals (nitrogen and hydrogen) produced by the decomposition can also react with the hydroxyl and carboxyl groups produced by the asphalt to form a transition layer; the sulfate ions can react with the surface of the carbon material to form stable chemical bonds. That is, using ammonium persulfate as a modifier can promote the formation of interface functional groups and free radical transition layers, improve the bonding between asphalt and aggregate during pressurized mixing, and facilitate obtaining high-performance carbon materials after subsequent pressurized roasting.

[0015] In the above preparation method, preferably, the carbonaceous aggregate is first mixed with the chemical modifier and comprises the following steps:

[0016] The chemical modifier and anhydrous ethanol are stirred and dispersed uniformly in a mass ratio of (1-3):100, and then the carbonaceous aggregate is added, and the anhydrous ethanol is removed after mixing uniformly. Then, the mixture is placed in a pressurized kneading pot, mixed at 100-110°C for 1-2h, and the kneading pot speed is 10-50r / min to remove moisture;

[0017] The mixture is then mixed under pressure at 200-250° C. and 0.5-1 MPa for 1-3 hours with the rotating speed of the kneading pot being 10-50 r / min to obtain a modified carbonaceous aggregate.

[0018] The present invention first kneads at 100-110°C under normal pressure to facilitate dehydration and fully disperse the aggregate. Then, the mixture is mixed under pressure at 200-250°C and 0.5-1MPa for 1-3h. During the process, the chemical modifier and the carbonaceous aggregate are fully mixed and reacted, which can promote the formation of the interface functional groups and free radical transition layer between the aggregates. The process is carried out under a pressurized environment, and more preferably in a very small closed space. For example, after the chemical modifier and the carbonaceous aggregate are placed in a container and then sealed, the remaining volume is only 1 / 2 of the total volume of the chemical modifier and the carbonaceous aggregate. Under the above-mentioned pressurized conditions, the synergistic effect of the washing oil and ammonium persulfate can be promoted, and the volatile components of the washing oil and the decomposition products of the ammonium persulfate can better react with the carbonaceous aggregate. At the same time, under pressure conditions, the chemical reaction between the chemical modifier and the aggregate surface can be promoted to enhance the intermolecular force.

[0019] In the above preparation method, preferably, during the pressurized kneading, the asphalt is added to the pressurized kneading pot filled with the modified carbonaceous aggregate, and the pressurized kneading is carried out in a closed space at a pressure of 0.5-3MPa, the pressurized kneading temperature is controlled to be 240-270°C, the kneading time is 1-2h, and the volatile matter of the paste is controlled to be between 11-12%. In the pressurized atmosphere, the fluidity of the asphalt increases, and the pressurized kneading can make the asphalt continuously penetrate into the gaps between the aggregates, and the plasticity of the paste increases, which is conducive to the carbonization of the asphalt into rings in the subsequent pressurized roasting, and realizes the close connection of different aggregates; when the pressurized kneading is carried out at 0.5-3MPa, the volatile matter in the asphalt will volatilize, and the asphalt volatile matter is kept as the pressurized atmosphere. The pressure of the volatile matter helps to push the asphalt into tiny pores, thereby increasing the saturation of the carbon material, and the aromatic hydrocarbon molecules in the asphalt volatile matter are easy to undergo polymerization reaction to form larger molecular polymers, promote the reaction between aromatic hydrocarbon molecules, increase the molecular weight and cross-linking degree of the asphalt, thereby improving its adhesion and adsorption. At the same time, the sulfur, nitrogen and other heteroatoms in the volatile matter of asphalt can act as catalysts to promote the cross-linking reaction between asphalt molecules. During the subsequent pressurized roasting, the components in the asphalt decompose and condense with the aggregate, making the green body shrink evenly and improving the yield rate. In addition, after being modified by chemical modifiers, under pressurized conditions, the asphalt can better react chemically with the functional groups on the surface of the carbon material to form chemical bonds, thereby enhancing the interaction between the asphalt and the carbon material.

[0020] In the above preparation method, preferably, the carbonaceous aggregate comprises calcined petroleum coke aggregate (primary aggregate) with a D50 of 15-20 μm and graphite powder (secondary aggregate) with a D50 of 1-5 μm, and the mass ratio of the calcined petroleum coke aggregate to the graphite powder is (7-9): (1-3). The particle size ratio and mass ratio of the above primary aggregate and secondary aggregate are controlled, with the large particles of the primary aggregate as the skeleton and the secondary aggregate filling the gaps between the large particles, so that the aggregates are stacked more densely.

[0021] In the above preparation method, preferably, the asphalt is a high-temperature molten asphalt with a softening point of 160-200°C, and the mass ratio of the carbonaceous aggregate to the asphalt is (7-9): (1-3). The use of high-temperature molten asphalt in the present invention has better effects than modified asphalt. This is because the high-temperature molten asphalt has a better coordination effect with the pressurized mixing and kneading and pressurized roasting of the present application, which is more conducive to the synergistic effect of the two. During the pressurized mixing stage, the high-temperature molten asphalt has a higher fluidity, which enables the asphalt to better penetrate between the carbon material particles and form a close contact. At the same time, during the pressurized roasting stage, the volatile matter in the high-temperature molten asphalt is easier to diffuse and transfer mass at high temperatures, which helps the beneficial components in the asphalt to migrate to the surface and interior of the carbon material more quickly, which is more conducive to the subsequent pressurized roasting effect.

[0022] The mass ratio of carbonaceous aggregate to asphalt is (7-9): (1-3) The reasons for the limitation are as follows:

[0023] On the one hand, since two kinds of aggregates are used and the small particles are filled into the gaps between the large particles, the pores on the aggregate surface are uniform and the specific surface area is moderate. By controlling the above mass ratio, the aggregate and the asphalt can be fully adsorbed. On the other hand, by controlling the above mass ratio, during pressurized kneading, the asphalt volatiles are used as a kind of pressurized atmosphere, which improves the adsorption of the asphalt. In the subsequent roasting, under the action of pressure, the shrinkage of the green body is increased, the volatile gas penetrates into the interior of the green body, and the polycondensation reaction is deposited inside, thereby improving the density of the material.

[0024] In the above preparation method, preferably, the slurry is sheeted, crushed, and sieved to obtain a pressed powder, which comprises the following steps: sheeting the slurry 1-3 times, the sheet thickness is 1-2 mm, the sheet temperature corresponds to the pressurized kneading temperature, after cooling, crushing, passing through a 160-325 mesh sieve, mixing for 0.5-1h, and obtaining a pressed powder;

[0025] During the cold isostatic pressing treatment, the pressed powder is loaded into the mold sleeve of the isostatic pressing mold, vacuum-packed after compaction, placed in a cold isostatic pressing device, and isostatically pressed at 150-200 MPa for 5-20 minutes, and then the pressure is released to obtain a green block.

[0026] In the above preparation method, preferably, the pressure roasting is carried out in a closed space, the roasting pressure is 0.1-3MPa, and the roasting is carried out at 800-1200°C for 2-4h, and then cooled to obtain a roasted block. The roasting pressure is controlled to be 0.1-3MPa, which is conducive to ensuring the effect of pressure roasting and does not require high bearing capacity of the equipment.

[0027] In the above preparation method, preferably, the graphitization treatment is carried out at 2000-3000° C. for 1-2 hours and then cooled to obtain a high-purity graphite material.

[0028] In the present invention, the method for preparing the high-purity graphite material may more specifically include the following steps:

[0029] (1) using a Raymond mill and a high-energy airflow mill to prepare calcined petroleum coke aggregate with a particle size D50 of 15-20 μm, artificial graphite powder, flake graphite powder (high purity) or high-power graphite electrode powder with a D50 of 1-5 μm, and the chemical modifier is one or more of oleic acid, washing oil, nitronaphthalene and ammonium persulfate;

[0030] (2) adding the calcined petroleum coke obtained in step (1) and the graphite powder obtained in step (1) into a mixer in a mass ratio of 7-9:1-3 and mixing for 1-2 hours until the mixture is uniform without particle segregation, thereby obtaining a carbonaceous aggregate;

[0031] (3) After the chemical modifier and anhydrous ethanol are stirred and dispersed uniformly in a mass ratio of 1-3:100, the carbonaceous aggregate is added in a mass ratio of 1-5:100, the anhydrous ethanol is removed after mixing uniformly, and then the mixture is placed in a pressurized kneading pot, mixed at 100-110° C. for 1-2 hours, with the kneading pot rotating at 10-50 r / min, to remove moisture; and then pressurized and mixed at 200-250° C. and 0.5-1 MPa for 1-3 hours, with the kneading pot rotating at 10-50 r / min, to obtain a modified carbonaceous aggregate;

[0032] (4) adding high-temperature molten asphalt with a softening point of 160-200°C into a pressure kneading pot at a mass ratio of 7-9:1-3, and performing pressure kneading at a pressure of 0.5-3MPa. The pressure kneading temperature is controlled at 240-270°C, the kneading time is 1-2h, and the volatile matter of the paste is controlled between 11-12%;

[0033] (5) After kneading, the paste obtained in step (4) is rolled 1-3 times, the thickness of the rolled sheet is 1-2 mm, and the rolling temperature corresponds to the kneading temperature. After cooling to room temperature, it is crushed, passed through a 160-325 mesh sieve, and mixed for 0.5-1h to obtain a pressed powder;

[0034] (6) The pressed powder obtained in step (5) is placed in the mold sleeve of the isostatic pressing mold, vibrated and then vacuum packaged, placed in a cold isostatic pressing device, and isostatically pressed at 150-200 MPa for 5-20 min, then gradually released, the sample is taken out, the packaging tape is peeled off, and after being left for 2-10 h, a density of 1.55-1.60 g / cm 3 A green block;

[0035] (7) The green body prepared in step (6) is placed in a graphite crucible. After the six sides of the green body are filled with the filling material, it is placed in a roasting furnace. During the roasting process, argon / nitrogen is passed through, and the pressure in the furnace is maintained at 0.1-3 MPa. The pressure is maintained and roasted according to the set temperature curve. After the temperature is lowered to 150-300°C by program control, it is naturally cooled to room temperature to obtain a density of 1.59-1.70 g / cm 3 calcined block;

[0036] (8) The calcined block prepared in step (7) is placed in a vacuum graphitization furnace under atmosphere protection, treated at 2000-3000°C for 1-2h, the temperature is dropped to 100-300°C under program control, and then naturally cooled to room temperature to obtain a density of 1.65-1.85 g / cm 3 The graphitized block is a high-purity graphite material.

[0037] Aiming at the problems of long production cycle, high production cost, low material homogeneity caused by multiple impregnation and roasting in the traditional preparation method of high-purity graphite materials, the present invention uses one or more of oleic acid, washing oil, nitronaphthalene and ammonium persulfate as chemical modifiers, utilizes the strong electron-withdrawing ability of its chemical groups, first mixes with carbonaceous aggregate to modify the carbonaceous aggregate, and during pressurized kneading, the chemical modifier builds interface functional groups and free radical transition layers between primary and secondary aggregates under pressure (the chemical modifier enhances the bonding force between primary and secondary aggregates through chemical bonding, improves the overall The stability of the structure is used to construct the interface functional groups; the free radical transition layer formed at the same time provides additional interaction forces between the primary and secondary aggregates through covalent bonds or non-covalent bonds), so that the interface functional groups and free radical transition layer are constructed between the primary and secondary aggregates, which have high chemical activity and wettability. When it is subsequently mixed with asphalt and kneaded under pressure, the chemical groups promote the polymerization of the aromatic free radicals of the binder, so that the binder asphalt is easier to wet and evenly spread on the surface of the carbonaceous aggregate, and penetrate into the pores of the carbonaceous aggregate at a faster speed to form a kneaded paste with good homogeneity. At the same time, asphalt can also promote the formation of interface functional groups and free radical transition layers. The asphalt undergoes chemical reactions, and free radicals and functional groups are also formed, which react with the free radicals or functional groups on the surface of the modified carbon material to form stable chemical bonds, making the combination tighter and the kneading effect better. During the pressurized roasting stage, the escape of volatiles can be suppressed, and the product can be homogenized. Under the action of pressure, the chemical modifier will polymerize the unstable molecules that should be pyrolyzed and volatilized during the carbonization process into stable polycyclic aromatic hydrocarbon macromolecules and remain in the binder carbonization, and simultaneously convert the generated intermediates into polycyclic aromatic hydrocarbons, further associate the binder molecules into macromolecules, promote the dehydrogenation polycondensation reaction of the binder, catalyze the coking polycondensation, make the interface functional groups and free radical transition layer show self-sintering behavior, and make the macromolecules that are evenly spread and penetrated on the surface and pores of the aggregate effectively form sintering necks between carbonaceous aggregates. At the same time, under the action of pressure, during the roasting process, the aromatic hydrocarbon free radicals generated by the binder first attack the oxygen on the chemical group and are consumed, so that the thermal decomposition reaction of the generated free radicals is terminated in advance, thereby avoiding the thermal decomposition and escape of a large number of unstable components in the form of volatiles, increasing the amount of residual carbon, and improving the comprehensive performance of the material.

[0038] Different from the common pressurization method of introducing inert gas, the pressurized kneading adopted by the present invention does not introduce inert gas, but relies on the joint action of air and asphalt volatiles as the pressurized atmosphere, and the pressure is maintained by the up and down movement of the pressure valve piston, which is simple to operate and saves costs. At the same time, asphalt volatiles as the pressurized atmosphere maintain the activity of α and β components, which is conducive to the combination and adsorption of asphalt and aggregate during the kneading process, so that the asphalt is evenly spread, laying the foundation for subsequent pressurized roasting. Using air as the pressurized atmosphere increases the cross-linking degree of asphalt, thereby increasing the strength of graphite materials.

[0039] Compared with the prior art, the advantages of the present invention are:

[0040] The preparation method of the present invention improves the preparation process, and by means of the synergistic effect of pressurized kneading and pressurized roasting, the asphalt is spread more evenly on the surface of the carbonaceous aggregate and infiltrated into the pores of the carbonaceous aggregate to form a sintering neck. On this basis, pressurized roasting promotes the carbonization of the asphalt into a ring, realizes the close connection of different aggregates, improves the homogeneity of the material, and prepares a high-purity graphite material that does not require impregnation and multiple roasting, improves the comprehensive performance of the material, shortens the production cycle, and increases the production capacity and profit of the enterprise. BRIEF DESCRIPTION OF THE DRAWINGS

[0041] In order to more clearly illustrate the embodiments of the present invention or the technical solutions in the prior art, the drawings required for use in the embodiments or the description of the prior art will be briefly introduced below. Obviously, the drawings described below are some embodiments of the present invention. For ordinary technicians in this field, other drawings can be obtained based on these drawings without paying creative work.

[0042] Figure 1 The test results of the flexural strength and compressive strength of the high-purity graphite material of Example 1 and the corresponding cross-sectional micromorphology images (in the figure, (a) is the flexural strength image, (c) is the compressive strength image, (b) is the 5μm cross-sectional micromorphology image, and (d) is the 10μm cross-sectional micromorphology image).

[0043] Figure 2 These are the surface polarization images and surface micromorphology images of the high-purity graphite material in Example 1 (in the images, (a) is the 100μm surface polarization image, (c) is the 500μm surface polarization image, (b) is the 5μm surface micromorphology image, and (d) is the 20μm surface micromorphology image).

[0044] Figure 3 These are the test results of the flexural strength and compressive strength of the high-purity graphite material of Comparative Example 1 and the corresponding cross-sectional micromorphology images (in the figures, (a) is the flexural strength image, (c) is the compressive strength image, (b) is the 5 μm cross-sectional micromorphology image, and (d) is the 10 μm cross-sectional micromorphology image).

[0045] Figure 4 These are the surface polarization images and surface micromorphology images of the high-purity graphite material of Comparative Example 1 (in the images, (a) is the 100 μm surface polarization image, (c) is the 500 μm surface polarization image, (b) is the 5 μm surface micromorphology image, and (d) is the 20 μm surface micromorphology image). DETAILED DESCRIPTION

[0046] In order to facilitate the understanding of the present invention, the present invention will be described more comprehensively and meticulously below in conjunction with the accompanying drawings and preferred embodiments of the present invention, but the protection scope of the present invention is not limited to the following specific embodiments.

[0047] Unless otherwise defined, all the professional terms used below have the same meanings as those generally understood by those skilled in the art. The professional terms used herein are only for the purpose of describing specific embodiments and are not intended to limit the scope of protection of the present invention.

[0048] Unless otherwise specified, various raw materials, reagents, instruments and equipment used in the present invention can be purchased from the market or prepared by existing methods.

[0049] Embodiment 1:

[0050] A method for preparing a high-purity graphite material comprises the following steps:

[0051] 1) Using a Raymond mill and a high-energy airflow mill to prepare calcined petroleum coke with a particle size D50 of 17 μm, artificial graphite powder with a D50 of 5 μm, washing oil and ammonium persulfate as chemical modifiers; high-temperature molten asphalt with a softening point of 170°C is set aside.

[0052] 2) adding the calcined petroleum coke obtained in step 1) and the graphite powder obtained in step 1) into a mixer at a mass ratio of 8:2 and mixing for 1 hour; and preparing a chemical modifier with a mass ratio of washing oil and ammonium persulfate of 1:2.

[0053] 3) After the chemical modifier and anhydrous ethanol are stirred and dispersed uniformly in a mass ratio of 2:100, the carbonaceous aggregate obtained in step 2) is added in a mass ratio of 5:100, and the anhydrous ethanol is removed after mixing evenly. Then, the mixture is put into a pressurized kneading pot, dry-mixed at 110° C. for 1 h at a speed of 10 r / min to remove moisture; and then pressurized and mixed at 210° C. at 1 MPa for 2.5 h at a kneading pot speed of 10 / min to obtain a modified carbonaceous aggregate.

[0054] 4) Add the high-temperature molten asphalt to the pressurized kneading pot filled with modified carbonaceous aggregate at a mass ratio of 7:3 of the mixed powder and the high-temperature molten asphalt, maintain the pressure at 3MPa for pressurized kneading, control the kneading temperature at 250℃, and kneading time for 1h. After kneading, quickly transfer the paste to the material hopper of the sheet rolling machine, roll the sheet 3 times, the sheet thickness is 2mm, the sheet rolling temperature corresponds to the kneading temperature, cool the material after the sheet rolling is completed, wait for the material temperature to drop to room temperature, set aside for 10h, crush and grind, pass through a 200-mesh sieve, and mix for 0.5h to obtain pressed powder.

[0055] 5) The pressed powder obtained in step 4) is pressed into a block at 1 MPa for 60 seconds, and then vacuum-sealed in a bag and placed for 2-10 hours; the block is placed in a cold isostatic pressing device, isostatically pressed at 200 MPa for 10 minutes, and then the pressure is gradually released. The sample is taken out, the packaging tape is peeled off, and after being placed for 10 hours, a density of 1.60 g / cm 3 of green blocks.

[0056] 6) The green body prepared in step 5) is placed in a graphite crucible. After the six sides of the green body are filled with the filling material, it is placed in a tubular roasting furnace. During the roasting process, argon / nitrogen is passed and the pressure in the furnace is maintained at 3 MPa. The green body is roasted at 1050°C for 4 hours. After the temperature is lowered to 200°C by program control, it is naturally cooled to room temperature to obtain a density of 1.67 g / cm 3 of calcined blocks.

[0057] 7) The calcined block prepared in step 6) was placed in a vacuum graphitization furnace under atmosphere protection and treated at 2500°C for 2 h. After the temperature was reduced to 300°C by program control, it was naturally cooled to room temperature to obtain a density of 1.83 g / cm 3 The graphitized block is a baked graphitized graphite material.

[0058] According to the YB / T4379-2014 standard, the graphite material obtained in step 6) was tested for bulk density, open porosity, resistivity, flexural strength, compressive strength and Shore hardness. The bulk density was 1.83 g / cm 3 , open porosity is 11.0%, resistivity is 12.8μΩ·m, flexural strength is 61.85MPa, compressive strength is 120.27MPa, and Shore hardness is 77HSD.

[0059] The test results of the flexural strength and compressive strength of the graphite material obtained in this embodiment are as follows: Figure 1 (a) and Figure 1 As shown in (c), the cross-sectional microscopic morphology of flexural strength and compressive strength are shown in Figure 1 (b) and Figure 1 As shown in (d), Figure 1 (a) and Figure 1 From (c), we can see that the flexural strength and compressive strength of the graphite material are 61.85MPa and 120.27MPa respectively, which is a significant improvement compared with the graphite material prepared by the traditional process. From the corresponding microscopic morphology, we can see that the aggregates are tightly connected with each other, with high density, and the pores between the particles are small, with an average pore size of less than 2μm, and no through holes appear. Figure 2 The surface polarization image and the surface microscopic morphology image show that the pore structure of the sample is evenly distributed, and the pore size is generally small, and most of them are single independent pores. Therefore, the graphite material has excellent flexural and compressive strength properties.

[0060] Embodiment 2:

[0061] A method for preparing a high-purity graphite material comprises the following steps:

[0062] 1) Using a Raymond mill and a high-energy airflow mill to prepare calcined petroleum coke with a particle size D50 of 17 μm, artificial graphite powder with a D50 of 5 μm, oleic acid and ammonium persulfate as chemical modifiers; and high-temperature molten asphalt with a softening point of 170°C for standby use.

[0063] 2) adding the calcined petroleum coke obtained in step 1) and the graphite powder obtained in step 1) into a mixer at a mass ratio of 8:2 and mixing for 1 hour; preparing a chemical modifier with oleic acid and ammonium persulfate at a mass ratio of 1:2.

[0064] 3) After the chemical modifier and anhydrous ethanol are stirred and dispersed uniformly in a mass ratio of 2:100, the carbonaceous aggregate obtained in step 2) is added in a mass ratio of 5:100, and the anhydrous ethanol is removed after mixing evenly. Then, the mixture is put into a pressurized kneading pot, dry-mixed at 110° C. for 1 h at a speed of 10 r / min to remove moisture; and then pressurized and mixed at 210° C. at 1 MPa for 2.5 h at a kneading pot speed of 10 / min to obtain a modified carbonaceous aggregate.

[0065] 4) Add the high-temperature molten asphalt to the pressurized kneading pot filled with modified carbonaceous aggregate at a mass ratio of 7:3 of the mixed powder and the high-temperature molten asphalt, maintain the pressure at 1MPa for pressurized kneading, control the kneading temperature at 250℃, and kneading time for 1h. After kneading, quickly transfer the paste to the material hopper of the sheet rolling machine, roll the sheet 3 times, the sheet thickness is 2mm, the sheet rolling temperature corresponds to the kneading temperature, cool the material after the sheet rolling is completed, wait for the material temperature to drop to room temperature, set aside for 10h, crush and grind, pass through a 200-mesh sieve, and mix for 0.5h to obtain pressed powder.

[0066] 5) The pressed powder obtained in step 4) is pressed into a block at 1 MPa for 60 seconds, and then vacuum-sealed and placed for 2-10 hours; the block is placed in a cold isostatic pressing device, isostatically pressed at 200 MPa for 10 minutes, and then the pressure is gradually released. The sample is taken out, the packaging tape is peeled off, and after being placed for 10 hours, a density of 1.58 g / cm 3 of green blocks.

[0067] 6) The green body prepared in step 5) is placed in a graphite crucible. After the six sides of the green body are filled with the filling material, it is placed in a tubular roasting furnace. During the roasting process, argon / nitrogen is passed and the pressure in the furnace is maintained at 1 MPa. The green body is roasted at 1050°C for 4 hours. After the temperature is lowered to 200°C by program control, it is naturally cooled to room temperature to obtain a density of 1.64 g / cm 3 of the calcined block.

[0068] 7) The calcined block prepared in step 6) was placed in a vacuum graphitization furnace under atmosphere protection and treated at 2500°C for 2 h. After the temperature was reduced to 300°C by program control, it was naturally cooled to room temperature to obtain a density of 1.81 g / cm 3 The graphitized block is a baked graphitized graphite material.

[0069] According to the YB / T4379-2014 standard, the graphite material obtained in step 6) was tested for bulk density, open porosity, resistivity, flexural strength, compressive strength and Shore hardness. The bulk density was 1.81 g / cm 3 , open porosity is 12.0%, resistivity is 13.2μΩ·m, flexural strength is 59.82MPa, compressive strength is 113.44MPa, and Shore hardness is 69HSD.

[0070] Embodiment 3:

[0071] A method for preparing a high-purity graphite material comprises the following steps:

[0072] 1) Using a Raymond mill and a high-energy airflow mill to prepare calcined petroleum coke with a particle size D50 of 17 μm and artificial graphite powder with a D50 of 5 μm; using nitronaphthalene and ammonium persulfate as chemical modifiers and high-temperature molten asphalt with a softening point of 170°C for standby use.

[0073] 2) adding the calcined petroleum coke obtained in step 1) and the graphite powder obtained in step 1) into a mixer at a mass ratio of 8:2 and mixing for 1 hour; preparing a chemical modifier with nitronaphthalene and ammonium persulfate at a mass ratio of 1:2.

[0074] 3) After the chemical modifier and anhydrous ethanol are stirred and dispersed uniformly in a mass ratio of 2:100, the carbonaceous aggregate obtained in step 2) is added in a mass ratio of 5:100, and the anhydrous ethanol is removed after mixing evenly. Then, the mixture is put into a pressurized kneading pot, dry-mixed at 110° C. for 1 h at a speed of 10 r / min to remove moisture; and then pressurized and mixed at 210° C. at 1 MPa for 2.5 h at a kneading pot speed of 10 / min to obtain a modified carbonaceous aggregate.

[0075] 4) Add the high-temperature molten asphalt to the pressurized kneading pot filled with modified carbonaceous aggregate at a mass ratio of 7:3 of the mixed powder and the high-temperature molten asphalt, maintain the pressure at 3MPa for pressurized kneading, control the kneading temperature at 250℃, and kneading time for 1h. After kneading, quickly transfer the paste to the material hopper of the sheet rolling machine, roll the sheet 3 times, the sheet thickness is 2mm, the sheet rolling temperature corresponds to the kneading temperature, cool the material after the sheet rolling is completed, wait for the material temperature to drop to room temperature, set aside for 10h, crush and grind, pass through a 200-mesh sieve, and mix for 0.5h to obtain pressed powder.

[0076] 5) The pressed powder obtained in step 4) is pressed into a block at 1 MPa for 60 seconds, and then vacuum-sealed in a bag and placed for 2-10 hours; the block is placed in a cold isostatic pressing device, isostatically pressed at 200 MPa for 10 minutes, and then the pressure is gradually released. The sample is taken out, the packaging tape is peeled off, and after being placed for 10 hours, a density of 1.57 g / cm 3 of green blocks.

[0077] 6) The green body prepared in step 5) is placed in a graphite crucible. After the six sides of the green body are filled with the filling material, it is placed in a tubular roasting furnace. During the roasting process, argon / nitrogen is passed and the pressure in the furnace is maintained at 3 MPa. The green body is roasted at 1050°C for 4 hours. After the temperature is lowered to 200°C by program control, it is naturally cooled to room temperature to obtain a density of 1.62 g / cm 3 of calcined blocks.

[0078] 7) The calcined block prepared in step 6) was placed in a vacuum graphitization furnace under atmosphere protection and treated at 2500°C for 2 h. After the temperature was reduced to 300°C by program control, it was naturally cooled to room temperature to obtain a density of 1.78 g / cm 3 The graphitized block is a baked graphitized graphite material.

[0079] According to the YB / T4379-2014 standard, the graphite material obtained in step 6) was tested for bulk density, open porosity, resistivity, flexural strength, compressive strength and Shore hardness. The bulk density was 1.78 g / cm 3 , open porosity is 13.2%, resistivity is 14.1μΩ·m, flexural strength is 45.57MPa, compressive strength is 106.78MPa, and Shore hardness is 58HSD.

[0080] Embodiment 4:

[0081] 1) Using a Raymond mill and a high-energy airflow mill to prepare calcined petroleum coke with a particle size D50 of 17 μm and artificial graphite powder with a D50 of 5 μm, wash oil is used as a chemical modifier; high-temperature molten asphalt with a softening point of 170°C is set aside.

[0082] 2) The calcined petroleum coke obtained in step 1) and the graphite powder obtained in step 1) are added into a mixer at a mass ratio of 8:2 and mixed for 1 hour.

[0083] 3) After the chemical modifier and anhydrous ethanol are stirred and dispersed uniformly in a mass ratio of 2:100, the carbonaceous aggregate obtained in step 2) is added in a mass ratio of 5:100, and the anhydrous ethanol is removed after mixing evenly. Then, the mixture is put into a pressurized kneading pot, dry-mixed at 110° C. for 1 h at a speed of 10 r / min to remove moisture; and then pressurized and mixed at 210° C. at 1 MPa for 2.5 h at a kneading pot speed of 10 / min to obtain a modified carbonaceous aggregate.

[0084] 4) Add the high-temperature molten asphalt to the pressurized kneading pot filled with modified carbonaceous aggregate at a mass ratio of 7:3 of the mixed powder and the high-temperature molten asphalt, maintain the pressure at 3MPa for pressurized kneading, control the kneading temperature at 250℃, and kneading time for 1h. After kneading, quickly transfer the paste to the material hopper of the sheet rolling machine, roll the sheet 3 times, the sheet thickness is 2mm, the sheet rolling temperature corresponds to the kneading temperature, cool the material after the sheet rolling, wait for the material temperature to drop to room temperature, set aside for 10h, crush and grind, pass through a 200-mesh sieve, and mix for 0.5h to obtain pressed powder.

[0085] 5) The pressed powder obtained in step 4) is pressed into a block at 1 MPa for 60 seconds, and then vacuum-sealed and placed for 2-10 hours; the block is placed in a cold isostatic pressing device, isostatically pressed at 200 MPa for 10 minutes, and then the pressure is gradually released. The sample is taken out, the packaging tape is peeled off, and after being placed for 10 hours, a density of 1.55 g / cm 3 of green blocks.

[0086] 6) The green body prepared in step 5) is placed in a graphite crucible. After the six sides of the green body are filled with the filling material, it is placed in a tubular roasting furnace. During the roasting process, argon / nitrogen is passed and the pressure in the furnace is maintained at 3 MPa. The green body is roasted at 1050°C for 4 hours. After the temperature is lowered to 200°C by program control, it is naturally cooled to room temperature to obtain a density of 1.59 g / cm 3 of the calcined block.

[0087] 7) The calcined block prepared in step 6) was placed in a vacuum graphitization furnace under atmosphere protection, treated at 2500°C for 2h, the temperature was dropped to 300°C by program control, and then naturally cooled to room temperature to obtain a density of 1.70g / cm 3 The graphitized block is a baked graphitized graphite material.

[0088] According to the YB / T4379-2014 standard, the graphite material obtained in step 7) was tested for bulk density, open porosity, resistivity, flexural strength, compressive strength and Shore hardness. The bulk density was 1.70 g / cm 3 , open porosity is 13.8%, resistivity is 15.1μΩ·m, flexural strength is 40.58MPa, compressive strength is 96.47MPa, and Shore hardness is 53HSD.

[0089] Embodiment 5:

[0090] 1) Using a Raymond mill and a high-energy airflow mill to prepare calcined petroleum coke with a particle size D50 of 17 μm, artificial graphite powder with a D50 of 5 μm, ammonium persulfate as a chemical modifier, and high-temperature molten asphalt with a softening point of 170° C., for standby use.

[0091] 2) The calcined petroleum coke obtained in step 1) and the graphite powder obtained in step 1) are added into a mixer at a mass ratio of 8:2 and mixed for 1 hour.

[0092] 3) After the chemical modifier and anhydrous ethanol are stirred and dispersed uniformly in a mass ratio of 2:100, the carbonaceous aggregate obtained in step 2) is added in a mass ratio of 5:100, and the anhydrous ethanol is removed after mixing evenly. Then, the mixture is put into a pressurized kneading pot, dry-mixed at 110° C. for 1 h at a speed of 10 r / min to remove moisture; and then pressurized and mixed at 210° C. at 1 MPa for 2.5 h at a kneading pot speed of 10 / min to obtain a modified carbonaceous aggregate.

[0093] 4) Add the high-temperature molten asphalt to the pressurized kneading pot filled with modified carbonaceous aggregate at a mass ratio of 7:3 of the mixed powder and the high-temperature molten asphalt, maintain the pressure at 3MPa for pressurized kneading, control the kneading temperature at 250℃, and kneading time for 1h. After kneading, quickly transfer the paste to the material hopper of the sheet rolling machine, roll the sheet 3 times, the sheet thickness is 2mm, the sheet rolling temperature corresponds to the kneading temperature, cool the material after the sheet rolling is completed, wait for the material temperature to drop to room temperature, set aside for 10h, crush and grind, pass through a 200-mesh sieve, and mix for 0.5h to obtain pressed powder.

[0094] 5) The pressed powder obtained in step 4) is pressed into a block at 1 MPa for 60 seconds, and then vacuum-sealed in a bag and placed for 2-10 hours; the block is placed in a cold isostatic pressing device, isostatically pressed at 200 MPa for 10 minutes, and then the pressure is gradually released. The sample is taken out, the packaging tape is peeled off, and after being placed for 10 hours, a density of 1.56 g / cm 3 of green blocks.

[0095] 6) The green body prepared in step 5) is placed in a graphite crucible. After the six sides of the green body are filled with the filling material, it is placed in a tubular roasting furnace. During the roasting process, argon / nitrogen is passed and the pressure in the furnace is maintained at 3 MPa. The green body is roasted at 1050°C for 4 hours. After the temperature is lowered to 200°C by program control, it is naturally cooled to room temperature to obtain a density of 1.61 g / cm 3 of calcined blocks.

[0096] 7) The calcined block prepared in step 6) was placed in a vacuum graphitization furnace under atmosphere protection and treated at 2500°C for 2h. After the temperature was reduced to 300°C by program control, it was naturally cooled to room temperature to obtain a density of 1.72 g / cm 3 The graphitized block is a baked graphitized graphite material.

[0097] According to the YB / T4379-2014 standard, the graphite material obtained in step 6) was tested for bulk density, open porosity, resistivity, flexural strength, compressive strength and Shore hardness. The bulk density was 1.72 g / cm 3 , open porosity is 13.6%, resistivity is 14.7μΩ·m, flexural strength is 42.66MPa, compressive strength is 100.68MPa, and Shore hardness is 56HSD.

[0098] Embodiment 6:

[0099] Compared with Example 1, the main difference is that step 3) is different, and other conditions are the same. Step 3) is as follows:

[0100] Step 3) After the chemical modifier and anhydrous ethanol are stirred and dispersed uniformly in a mass ratio of 2:100, the carbonaceous aggregate obtained in step 2) is added in a mass ratio of 5:100, and the anhydrous ethanol is removed after mixing evenly. Then, the mixture is placed in a pressurized kneading pot and dry-mixed at 110° C. for 1 h at a speed of 10 r / min to remove moisture; then, the mixture is mixed at normal pressure at 210° C. for 2.5 h at a kneading pot speed of 10 / min to obtain a modified carbonaceous aggregate.

[0101] According to the YB / T4379-2014 standard, the graphite material obtained in step 6) was tested for bulk density, open porosity, resistivity, flexural strength, compressive strength and Shore hardness. The bulk density was 1.82 g / cm 3 , open porosity is 11.5%, resistivity is 13.1μΩ·m, flexural strength is 60.16MPa, compressive strength is 115.62MPa, and Shore hardness is 74HSD.

[0102] Comparative Example 1:

[0103] A method for preparing a high-purity graphite material comprises the following steps:

[0104] 1) Using a Raymond mill and a high-energy airflow mill to prepare calcined petroleum coke with a particle size D50 of 17 μm, artificial graphite powder with a D50 of 5 μm, washing oil and ammonium persulfate as chemical modifiers; high-temperature molten asphalt with a softening point of 170°C is set aside.

[0105] 2) adding the calcined petroleum coke obtained in step 1) and the graphite powder obtained in step 1) into a mixer at a mass ratio of 8:2 and mixing for 1 hour; and preparing a chemical modifier with a mass ratio of washing oil and ammonium persulfate of 1:2.

[0106] 3) After the chemical modifier and anhydrous ethanol are stirred and dispersed uniformly in a mass ratio of 2:100, the carbonaceous aggregate obtained in step 2) is added in a mass ratio of 5:100, and the anhydrous ethanol is removed after mixing evenly. Then, the mixture is put into a pressurized kneading pot, dry-mixed at 110° C. for 1 h at a speed of 10 r / min to remove moisture; and then mixed at 210° C. at normal pressure for 2.5 h at a kneading pot speed of 10 / min to obtain a modified carbonaceous aggregate.

[0107] 4) Add the high-temperature molten asphalt to the pressurized kneading pot filled with modified carbonaceous aggregate at a mass ratio of 7:3 of the mixed powder and the high-temperature molten asphalt, without pressurization, and control the kneading temperature at 250°C for 1 hour. After kneading, the paste is quickly transferred to the material hopper of the sheet rolling machine, and the sheet is rolled 3 times with a sheet thickness of 2mm. The sheet rolling temperature corresponds to the kneading temperature. After the sheet rolling is completed, the material is cooled. After the material temperature is reduced to room temperature, it is placed for 10 hours and then crushed and ground, passed through a 200-mesh sieve, and mixed for 0.5 hours to obtain a pressed powder.

[0108] 5) The pressed powder obtained in step 4) is pressed into a block at 1 MPa for 60 seconds, and then vacuum-sealed and placed for 2-10 hours; the block is placed in a cold isostatic pressing device, and isostatically pressed at 200 MPa for 10 minutes, and then the pressure is gradually released, the sample is taken out, the packaging tape is peeled off, and after being placed for 10 hours, a density of 1.50 g / cm 3 of green blocks.

[0109] 6) The green body prepared in step 5) is placed in a graphite crucible. After the six sides of the green body are filled with the filling material, it is placed in a tubular roasting furnace. During the roasting process, argon / nitrogen is passed and the pressure in the furnace is maintained at 0.1 MPa (atmospheric pressure). The green body is roasted at 1050°C for 4 hours, and the temperature is lowered to 200°C by program control, and then naturally cooled to room temperature to obtain a density of 1.54 g / cm 3 of calcined blocks.

[0110] 7) The calcined block prepared in step 6) was placed in a vacuum graphitization furnace under atmosphere protection, treated at 2500°C for 2h, and the temperature was dropped to 300°C by program control, and then naturally cooled to room temperature to obtain a density of 1.73 g / cm3 The graphitized block is a baked graphitized graphite material.

[0111] According to the YB / T4379-2014 standard, the graphite material obtained in step 6) was tested for bulk density, open porosity, resistivity, flexural strength, compressive strength and Shore hardness. The bulk density was 1.73 g / cm 3 , open porosity is 14.0%, resistivity is 15.4μΩ·m, flexural strength is 39.61MPa, compressive strength is 87.99MPa, and Shore hardness is 54HSD.

[0112] The test results of the flexural strength and compressive strength of the graphite material obtained in this comparative example are as follows: Figure 3 (a) and Figure 1 As shown in (c), the cross-sectional microscopic morphology of flexural strength and compressive strength are shown in Figure 3 (b) and Figure 3 As shown in (d), Figure 3 (a) and Figure 3 As shown in (c), the flexural strength and compressive strength of the graphite material are 39.61MPa and 87.99MPa respectively, which are inferior to the graphite material prepared by pressurized kneading in Example 1. The corresponding microscopic morphology shows that the aggregates are not tightly connected, there are many cracks, and the structural density is poor. Figure 4 The surface polarization image and the surface microscopic morphology image show that the pore structure distribution uniformity of the sample is poor and the pore size is large.

[0113] Comparative Example 2:

[0114] A method for preparing a high-purity graphite material comprises the following steps:

[0115] 1) Using a Raymond mill and a high-energy airflow mill to prepare calcined petroleum coke with a particle size D50 of 17 μm, artificial graphite powder with a D50 of 5 μm, washing oil and ammonium persulfate as chemical modifiers, and modified asphalt with a softening point of 105°C, the mixture is set aside.

[0116] 2) adding the calcined petroleum coke obtained in step 1) and the graphite powder obtained in step 1) into a mixer at a mass ratio of 8:2 and mixing for 1 hour; and preparing a chemical modifier with a mass ratio of washing oil and ammonium persulfate of 1:2.

[0117] 3) After the chemical modifier and anhydrous ethanol are stirred and dispersed uniformly in a mass ratio of 2:100, the carbonaceous aggregate obtained in step 2) is added in a mass ratio of 5:100, and the anhydrous ethanol is removed after mixing evenly. Then, the mixture is put into a pressurized kneading pot, dry-mixed at 110° C. for 1 h at a speed of 10 r / min to remove moisture; and then pressurized and mixed at 210° C. at 1 MPa for 2.5 h at a kneading pot speed of 10 / min to obtain a modified carbonaceous aggregate.

[0118] 4) When the temperature is cooled to 150°C, the modified asphalt is added to the pressure kneading pot containing modified carbonaceous aggregate at a mass ratio of 7:3 of the mixed powder and modified asphalt, and the pressure is maintained at 3MPa for pressure kneading. The kneading temperature is controlled at 190°C and the kneading time is 1h. After the kneading is completed, the paste is quickly transferred to the material hopper of the sheet rolling machine, and the sheet is rolled 3 times with a sheet thickness of 2mm. The sheet rolling temperature corresponds to the kneading temperature. After the sheet rolling is completed, the material is cooled. After the material temperature is reduced to room temperature, it is placed for 10 hours and then crushed and ground, passed through a 200-mesh sieve, and mixed for 0.5 hours to obtain a pressed powder.

[0119] 5) The pressed powder obtained in step 4) is pressed into a block at 1 MPa for 60 seconds, and then vacuum-sealed and placed for 2-10 hours; the block is placed in a cold isostatic pressing device, isostatically pressed at 200 MPa for 10 minutes, and then the pressure is gradually released. The sample is taken out, the packaging tape is peeled off, and after being placed for 10 hours, a density of 1.45 g / cm 3 of green blocks.

[0120] 6) The green body prepared in step 5) is placed in a graphite crucible. After the six sides of the green body are filled with the filling material, it is placed in a tubular roasting furnace. During the roasting process, argon / nitrogen is passed and the pressure in the furnace is maintained at 3 MPa. The green body is roasted at 1050°C for 4 hours. After the temperature is lowered to 200°C by program control, it is naturally cooled to room temperature to obtain a density of 1.50 g / cm 3 of calcined blocks.

[0121] 7) The calcined block prepared in step 6) was placed in a vacuum graphitization furnace under atmosphere protection, treated at 2500°C for 2h, the temperature was dropped to 300°C by program control, and then naturally cooled to room temperature to obtain a density of 1.66 g / cm 3 The graphitized block is a baked graphitized graphite material.

[0122] According to the YB / T4379-2014 standard, the graphite material obtained in step 7) was tested for bulk density, open porosity, resistivity, flexural strength, compressive strength and Shore hardness. The bulk density was 1.66 g / cm 3, open porosity is 14.1%, resistivity is 15.3μΩ·m, flexural strength is 36.84MPa, compressive strength is 77.07MPa, and Shore hardness is 50HSD.

[0123] Comparative Example 3:

[0124] A method for preparing a high-purity graphite material comprises the following steps:

[0125] 1) Using a Raymond mill and a high-energy airflow mill to prepare calcined petroleum coke with a particle size D50 of 17 μm and artificial graphite powder with a D50 of 5 μm; high-temperature molten asphalt with a softening point of 170° C., set aside.

[0126] 2) The calcined petroleum coke obtained in step 1) and the graphite powder obtained in step 1) are added into a mixer at a mass ratio of 8:2 and mixed for 1 hour.

[0127] 3) The mixed aggregate obtained in step 2) is put into a pressurized kneading pot, dry-mixed at 110°C for 1 hour, with a rotation speed of 10r / min, and the water is removed. The temperature is continued to rise to 210°C, and high-temperature molten asphalt is added at a mass ratio of 7:3 of the mixed powder and high-temperature molten asphalt, and melted to the corresponding temperature. No pressurized kneading is performed, and the kneading temperature is controlled at 250°C, the kneading speed is 50r / min, and the kneading time is 1 hour. After the kneading is completed, the paste is quickly transferred to the material hopper of the sheet rolling machine, and the sheet is rolled 3 times, the sheet thickness is 2mm, and the sheet rolling temperature corresponds to the kneading temperature. After the sheet rolling is completed, the material is cooled. After the material temperature drops to room temperature, it is placed for 10 hours and then crushed and ground, passed through a 200-mesh sieve, and then mixed for 0.5 hours to obtain a pressed powder.

[0128] 4) The pressed powder obtained in step 3) is pressed into a block at 1 MPa for 60 seconds, and then vacuum-sealed and placed for 2-10 hours; the block is placed in a cold isostatic pressing device, and isostatically pressed at 200 MPa for 10 minutes, and then the pressure is gradually released, the sample is taken out, the packaging tape is peeled off, and the block is placed for 10 hours to obtain a density of 1.46 g / cm 3 of green blocks.

[0129] 5) The green body prepared in step 4) is placed in a graphite crucible. After the six sides of the green body are filled with the filling material, it is placed in a tubular roasting furnace. During the roasting process, argon / nitrogen is passed and the pressure in the furnace is maintained at 0.1 MPa (atmospheric pressure). It is roasted at 1050°C for 4 hours, and the temperature is lowered to 200°C by program control, and then naturally cooled to room temperature to obtain a density of 1.49 g / cm 3 of the calcined block.

[0130] 6) The calcined block prepared in step 5) was placed in a vacuum graphitization furnace under atmosphere protection and treated at 2500°C for 2h. After the temperature was reduced to 300°C by program control, it was naturally cooled to room temperature to obtain a density of 1.67g / cm 3 The graphitized block is a baked graphitized graphite material.

[0131] According to the YB / T4379-2014 standard, the graphite material obtained in step 6) was tested for bulk density, open porosity, resistivity, flexural strength, compressive strength and Shore hardness. The bulk density was 1.67 g / cm 3 , open porosity is 13.4%, resistivity is 14.5μΩ·m, flexural strength is 34.89MPa, compressive strength is 69.56MPa, and Shore hardness is 47HSD.

[0132] Ultra-high purity isostatic graphite materials were prepared according to the methods in Examples 1-6 and Comparative Examples 1-3, and the volume density, open porosity, resistivity, flexural strength, compressive strength, and Shore hardness were calculated according to the YB / T4379-2014 standard; the measurement results are shown in Table 1 below.

[0133] Table 1: Performance data of graphite materials in Examples 1-6 and Comparative Examples 1-3

[0134] Bulk density Open porosity Resistivity Flexural strength Compressive strength Shore hardness Example 1 <![CDATA[1.83g / cm 3 ]]> 11.0% 12.8μΩ·m 61.85MPa 120.27MPa 77HSD Example 2 <![CDATA[1.81g / cm 3 ]]> 12.0% 13.2μΩ·m 59.82MPa 113.44MPa 69HSD Example 3 <![CDATA[1.78g / cm 3 ]]> 13.2% 14.1μΩ·m 45.57MPa 106.78MPa 58HSD Example 4 <![CDATA[1.70g / cm 3 ]]> 13.8% 15.1μΩ·m 40.58MPa 96.47MPa 53HSD Example 5 <![CDATA[1.72g / cm 3 ]]> 13.6% 14.7μΩ·m 42.66MPa 100.68MPa 56HSD Example 6 <![CDATA[1.82g / cm 3 ]]> 11.5% 13.1μΩ·m 60.16MPa 115.62MPa 74HSD Comparative Example 1 <![CDATA[1.73g / cm 3 ]]> 14.0% 15.4μΩ·m 39.61MPa 87.99MPa 54HSD Comparative Example 2 <![CDATA[1.66g / cm 3 ]]> 14.1% 15.3μΩ·m 36.84MPa 77.07MPa 50HSD Comparative Example 3 <![CDATA[1.67g / cm 3 ]]> 13.4% 14.5μΩ·m 34.89MPa 69.56MPa 47HSD

[0135] It can be seen from Table 1 above:

[0136] In Example 1, washing oil and ammonium persulfate are used as chemical modifiers, and the graphite material obtained by pressurized kneading and pressurized calcination cooperate with each other to achieve the best performance.

[0137] By comparing Example 1 and Example 2, it can be seen that washing oil and ammonium persulfate are preferred as chemical modifiers. At the same time, pressure kneading and pressure calcination at 3 MPa are better than pressure kneading and pressure calcination at 1 MPa. The cross-linking degree of asphalt is increased in the kneading stage, the polymerization of macromolecules in the asphalt is promoted, and the formation of sintering necks is more conducive to the calcination stage. The obtained graphite material has higher volume density, smaller open porosity, smaller resistivity, higher flexural strength and compressive strength, and higher Shore hardness.

[0138] From the comparison between Example 1 and Example 3, it can be seen that washing oil and ammonium persulfate are preferred as chemical modifiers, and the graphite material obtained has higher volume density, smaller open porosity, lower resistivity, higher flexural strength and compressive strength, and higher Shore hardness.

[0139] From the comparison between Example 1 and Example 4, it can be seen that the graphite material prepared by pressure kneading and pressure calcination using washing oil and ammonium persulfate in combination as chemical modifiers has higher volume density, smaller open porosity, lower resistivity, higher flexural strength and compressive strength, and higher Shore hardness than using washing oil alone as a chemical modifier.

[0140] From the comparison between Example 1 and Example 5, it can be seen that the graphite material prepared by using washing oil and ammonium persulfate in combination as chemical modifiers through pressure kneading and pressure calcination has higher volume density, smaller open porosity, lower resistivity, higher flexural strength and compressive strength, and higher Shore hardness than using ammonium persulfate alone as a chemical modifier.

[0141] From the comparison between Example 1 and Example 6, it can be seen that when washing oil and ammonium persulfate are used in combination as chemical modifiers and when the aggregate is modified by the chemical modifier, pressurized kneading is used. Compared with normal pressure kneading, the graphite material obtained has higher volume density, smaller open porosity, lower resistivity, higher flexural strength and compressive strength, and higher Shore hardness.

[0142] From the comparison between Example 1 and Comparative Example 1, it can be seen that when washing oil and ammonium persulfate are added alone as chemical modifiers and the synergistic effect of pressure kneading and pressure calcination is not adopted, the green density is low and the residual carbon amount during calcination is low, which is not conducive to the formation of sintering necks during carbonization. However, under the action of chemical modifiers, the graphite material prepared by the synergistic effect of pressure kneading and pressure calcination has higher volume density, smaller open porosity, lower resistivity, higher flexural strength and compressive strength, and higher Shore hardness.

[0143] From the comparison between Example 1 and Comparative Example 2, it can be seen that the use of high-temperature molten asphalt as a binder is optimal, which reflects the advantages of high-temperature molten asphalt under the synergistic effect of pressurized mixing and pressurized calcination. The wettability of the modified asphalt is low in the mixing and kneading stage, and the polymerization ability of the macromolecules is weak, which is more unfavorable for the formation of sintering necks in the calcination stage. Only under the action of the chemical modifier, the high-temperature molten asphalt can produce a graphite material with higher volume density, smaller open porosity, smaller resistivity, higher flexural strength and compressive strength, and higher Shore hardness through the synergistic effect of pressurized mixing and pressurized calcination.

[0144] From the comparison between Example 1 and Comparative Example 3, it can be seen that only when washing oil and ammonium persulfate are used as chemical modifiers and the synergistic effect of 3MPa pressure kneading and 3MPa pressure calcination is adopted, the graphite material obtained has a higher volume density, a smaller open porosity, a lower resistivity, higher flexural strength and compressive strength, and a higher Shore hardness.

Claims

1. A method for preparing a high-purity graphite material, characterized in that: The following steps are involved: (1) mixing carbonaceous aggregate and asphalt and kneading them under pressure to obtain a paste; (2) rolling, crushing and sieving the paste obtained in step (1) to obtain pressed powder; and cold isostatic pressing the pressed powder to obtain a green body block; (3) pressurizing and calcining the green block obtained in step (2) to obtain a calcined block; (4) The calcined block obtained in step (3) is graphitized to obtain a high-purity graphite material.

2. The preparation method according to claim 1, characterized in that: The carbonaceous aggregate is first mixed with a chemical modifier and then mixed with asphalt for pressurized kneading. The chemical modifier includes an organic modifier and / or an inorganic modifier. The organic modifier includes one or more of oleic acid, washing oil and nitronaphthalene. The inorganic modifier includes ammonium persulfate. The mass ratio of the chemical modifier to the carbonaceous aggregate is (1-5):

100.

3. The preparation method according to claim 2, characterized in that: The chemical modifier includes an organic modifier and an inorganic modifier, the organic modifier is washing oil, the inorganic modifier is ammonium persulfate, and the mass ratio of the washing oil to the ammonium persulfate is 1:(0.5-3).

4. The preparation method according to claim 2, characterized in that: The carbonaceous aggregate is first mixed with the chemical modifier and comprises the following steps: The chemical modifier and anhydrous ethanol are stirred and dispersed uniformly in a mass ratio of (1-3):100, and then the carbonaceous aggregate is added, and the anhydrous ethanol is removed after mixing uniformly. Then, the mixture is placed in a pressurized kneading pot, mixed at 100-110°C for 1-2h, and the kneading pot speed is 10-50r / min to remove moisture; The mixture is then mixed under pressure at 200-250° C. and 0.5-1 MPa for 1-3 hours with the rotating speed of the kneading pot being 10-50 r / min to obtain a modified carbonaceous aggregate.

5. The preparation method according to claim 4, characterized in that: During pressure kneading, add asphalt into a pressure kneading pot filled with modified carbonaceous aggregate, and perform pressure kneading in a closed space at a pressure of 0.5-3MPa. The pressure kneading temperature is controlled at 240-270°C, the kneading time is 1-2h, and the volatile matter of the paste is controlled between 11-12%.

6. The preparation method according to claim 1, characterized in that: The carbonaceous aggregate comprises calcined petroleum coke aggregate with a D50 of 15-20 μm and graphite powder with a D50 of 1-5 μm, and the mass ratio of the calcined petroleum coke aggregate to the graphite powder is (7-9):(1-3).

7. The preparation method according to claim 1, characterized in that: The asphalt is high-temperature molten asphalt with a softening point of 160-200° C., and the mass ratio of the carbonaceous aggregate to the asphalt is (7-9):(1-3).

8. The preparation method according to any one of claims 1 to 7, characterized in that: The paste is sheeted, crushed, and sieved to obtain a pressed powder, comprising the following steps: sheeting the paste 1-3 times, the sheet thickness is 1-2 mm, the sheeting temperature corresponds to the pressurized kneading temperature, after cooling, crushing, passing through a 160-325 mesh sieve, mixing for 0.5-1h, and obtaining a pressed powder; During the cold isostatic pressing treatment, the pressed powder is loaded into the mold sleeve of the isostatic pressing mold, vacuum-packed after compaction, placed in a cold isostatic pressing device, and isostatically pressed at 150-200 MPa for 5-20 minutes, and then the pressure is released to obtain a green block.

9. The preparation method according to any one of claims 1 to 7, characterized in that: During the pressure roasting, it is carried out in a closed space, the roasting pressure is 0.1-3MPa, and the roasting is carried out at 800-1200°C for 2-4h, and then cooled to obtain a roasted block.

10. The preparation method according to any one of claims 1 to 7, characterized in that: The graphitization treatment is carried out at 2000-3000°C for 1-2 hours and then cooled to obtain high-purity graphite material.

Citation Information

Patent Citations

  • Coldsmashed carbon material

    CN1051342A

  • Preparation method and application of low-cost high-purity graphite material

    CN114702316A

  • Carbon graphite material with low porosity and high mechanical strength and preparation method thereof

    CN115583835A

  • Method for manufacturing carbon nagtive electrode material of lithium ion cell

    CN1624955A

  • Method for improving carbon and / or graphite materials

    GB1281176A

Cited By

  • Porous graphite material and preparation method thereof

    CN119390473A

  • A porous graphite material and its preparation method

    CN119390473B

  • Preparation method of modified coal pitch and preparation method of carbon material

    CN121379188A