Nitrogen-impermeable high-temperature-resistant coating and preparation method and application thereof

By plating a silver layer on the surface of aero-engine parts and spraying a high-temperature resistant silicone modified coating to form a composite coating structure, the problem of anti-nitridation and corrosion resistance of aero-engines in high-temperature environments is solved, and a more efficient coating is achieved. performance and longer service life.

CN118755294APending Publication Date: 2024-10-11CHINA HANGFA GUIZHOU LIYANG AVIATION POWER CO LTD
View PDF 3 Cites 0 Cited by

Patent Information

Application Number
CN202410828719.8
Authority / Receiving Office
CN · China
Patent Type
Applications(China)
Current Assignee / Owner
Filing Date
2024-06-25
Publication Date
2024-10-11

AI Technical Summary

Technical Problem

Aeroengines face material performance requirements for nitriding resistance, corrosion resistance and high temperature resistance in high-temperature and high-pressure environments. Existing technologies are difficult to effectively meet these harsh conditions, especially the lack of anti-nitriding properties, which leads to reduced coating performance and shortened life.

Method used

It adopts a composite coating structure of a silver-plated layer and a high-temperature-resistant silicone-modified hydrophobic layer. The silver-plated layer is prepared by electroplating or chemical plating, and the silicone-modified coating is sprayed on its surface, combined with nano-level high-temperature resistant material particles. Form an anti-nitriding and high-temperature resistant coating.

Benefits of technology

It significantly improves the nitriding resistance, high temperature resistance and corrosion resistance of aero engine parts, reduces the coating thickness and cost, extends the service life of the parts, and maintains good nitriding resistance in high temperature environments.

✦ Generated by Eureka AI based on patent content.

Smart Images

  • Figure CN118755294A_ABST
    Figure CN118755294A_ABST
Patent Text Reader

Abstract

The invention discloses an anti-nitrogen high-temperature-resistant coating and a preparation method and application thereof.The anti-nitrogen high-temperature-resistant coating comprises a single silver plating layer or a combination of the silver plating layer and a hydrophobic layer, the silver plating layer is located on the surface of a base body, the hydrophobic layer is arranged on the surface of the silver plating layer, and the hydrophobic layer has high temperature resistance and hydrophobic performance. When the composite coating containing the silver plating layer and the hydrophobic layer is prepared, the silver plating layer is formed on the surface of a substrate through electroplating or chemical plating, and then the hydrophobic layer is formed in a spraying mode. The material can be applied to aero-engine parts, is low in preparation cost, can greatly improve the anti-nitriding performance, has high temperature resistance, and prolongs the service life of the parts.
Need to check novelty before this filing date? Find Prior Art

Description

Technical Field

[0001] The present invention belongs to the field of surface modification technology, specifically to the structure and preparation method of a high-temperature resistant modified coating at a specific location in an aircraft engine, and explores its anti-nitriding, corrosion-resistant and high-temperature resistant properties. Background Art

[0002] Aircraft engines are complex thermal machines that can work reliably for a long time under harsh environmental conditions of high temperature, high pressure and high speed rotation. Among all kinds of weapons and equipment, the requirements for materials of aircraft engines are particularly prominent. The harsh operating conditions of aircraft engines with high speed and high temperature, as well as the requirements for life and high reliability, have raised the demand for material performance to the extreme. Nowadays, the performance of aircraft engines has put forward higher requirements for engine materials and manufacturing, which are not limited to high temperature resistance, oxidation resistance, high strength, etc., but also put forward new requirements, such as anti-nitriding properties. Summary of the invention

[0003] The present invention aims to provide an anti-nitriding and high-temperature resistant coating and a preparation method and application thereof, which can greatly improve the anti-nitriding, high-temperature resistance and corrosion resistance of aircraft engine parts, reduce costs and coating thickness, and increase their service life.

[0004] To achieve the above object, the present invention adopts the following technical solutions:

[0005] Anti-nitriding high temperature resistant coating, including a single silver-plated layer, or a combination of a silver-plated layer and a hydrophobic layer;

[0006] The silver-plated layer is located on the surface of the substrate;

[0007] The hydrophobic layer is located on the surface of the silver-plated layer and has both high temperature resistance and hydrophobicity.

[0008] Furthermore, the maximum temperature of the effective working temperature range of the hydrophobic layer is 650°C.

[0009] Furthermore, the hydrophobic layer is an organosilicon modified coating.

[0010] Furthermore, the organosilicon modified coating is based on an organosilicon water repellent agent and is obtained by adding solid particles of a high temperature resistant material with a particle size of nanometers.

[0011] As described above, the method for preparing the anti-nitriding and high temperature resistant coating comprises a composite coating of a silver plating layer and a hydrophobic layer, and comprises the following preparation steps:

[0012] S1, obtaining a silver plating layer on the substrate surface by electroplating or chemical plating;

[0013] S2, spraying an organosilicon modified material on the surface of the silver-plated layer obtained in S1 to form a hydrophobic layer.

[0014] The application of the above-mentioned anti-nitriding and high-temperature resistant coating in aircraft engines.

[0015] Furthermore, the applications of anti-nitriding high temperature resistant coatings in aircraft engines include gearboxes, fan casings, heat exchangers, intermediate casings, combustion chamber sealing liners, combustion chamber inner cover rings and guide vanes.

[0016] Compared with the prior art, the present invention has the following characteristics:

[0017] (1) The coating preparation cost is low, and all the silicone water-repellent agents currently sold on the market can be used as preparation raw materials;

[0018] (2) Convenient modification. Since high temperature resistance is required, the modification can be achieved by adding nano-sized high temperature resistant material particles to the silicone water repellent.

[0019] (3) Compared with the traditional anti-nitriding structure, the coating thickness of the present invention is significantly reduced (no need to improve the anti-nitriding effect by stacking or increasing the thickness of the anti-nitriding structure), the anti-nitriding effect is better, and the adaptability is stronger (including corrosion resistance, weather resistance and number of cycles);

[0020] (4) Since the silver-plated layer and the hydrophobic layer can each effectively prevent nitriding, when a composite structure of the silver-plated layer and the hydrophobic layer is adopted, the advantages of both can be fully utilized, while at the same time the amount of silver used can be reduced, thereby reducing the preparation cost (especially for parts with very large surface areas);

[0021] (5) The preparation process of the silver-plated layer and the hydrophobic layer is simple. Electroplating, chemical plating and spraying are all mature processes and do not require special preparation methods.

[0022] Compared with the prior art, the anti-nitriding coating structure of the present invention can be used in specific parts of aircraft engines to extend the service life of various parts or blades of aircraft engines. It is not only oil-resistant, high-temperature-resistant and corrosion-resistant, but also can extend the service life of various components of aircraft engines. BRIEF DESCRIPTION OF THE DRAWINGS

[0023] Figure 1 This is a microscopic comparison of two different coating structures in the case of gas nitriding once;

[0024] Figure 2 This is a microscopic comparison of two different coating structures in the case of gas nitriding twice;

[0025] Figure 3 This is a microscopic comparison of two different coating structures after three times of gas nitriding;

[0026] Figure 4 This is a microscopic comparison of two different coating structures after gas nitriding for 4 times;

[0027] Figure 5 This is a typical application scenario of the anti-nitriding and high-temperature resistant coating in the present invention. DETAILED DESCRIPTION

[0028] The present invention is further described below in conjunction with specific embodiments, but it should not be understood that the scope of the subject matter described in the present invention is limited to the following embodiments. Without departing from the above-mentioned technical ideas of the present invention, various modifications, substitutions and changes made according to common technical knowledge and customary means in the field are included in the scope of the present invention.

[0029] The basic idea of ​​the present invention is to use a single silver-plated layer or spray a high-temperature resistant silicone modified coating on the surface of the silver-plated layer to explore the anti-nitriding properties of the single coating or the composite coating.

[0030] Silver is a silvery white, forgeable, plastic and reflective precious metal. With its excellent performance and relatively low cost, it has become one of the most widely used precious metals. Among all metals, silver has the best electrical conductivity and good thermal conductivity, ductility, reflectivity, corrosion resistance and welding performance. Silver plating has excellent electrical conductivity, decorative properties, weldability and low contact resistance. It is widely used in aviation, electronics, communications and other industrial fields and is in great demand.

[0031] The present invention adopts the form of silver plating on the substrate surface and silver plating on the surface plus spraying modified hydrophobic coating to conduct research. In the case of only silver layer, it is found that there may be a possibility that the material is in contact with water molecules in the air during use, resulting in water staying on the surface of the silver layer. The environment in which the substrate material is used is mostly high temperature and high pressure or there are corrosive gases such as SO 2 , H 2 S etc., are soluble in the water attached to the silver layer surface to form an acidic solution, causing damage to the coating. Or, the water attached to the silver layer surface causes electrochemical corrosion to the silver layer, which is also unavoidable. For the above reasons, when the matrix material is only silver-plated, a hydrophobic layer (high temperature resistant organosilicon modified coating) is sprayed on the silver layer surface, which can prevent the retention of water on the silver layer surface, prevent the multiple damages to the coating, and extend the service life of the coating. Meanwhile, the hydrophobic film made by the organosilicon hydrophobic agent selected in the present invention also has the advantages of high temperature resistance, good adhesion, etc., and can greatly improve the performance of the coating structure, namely, by modifying the organosilicon hydrophobic agent, improve its characteristics such as high temperature resistance, corrosion resistance and adhesion.

[0032] In this embodiment, the surface of the base material is modified by two treatment methods: silver plating on the surface of the base material and silver plating on the surface + spraying a hydrophobic film layer (high-temperature resistant silicone modified coating). The difference in anti-nitriding performance between spraying a high-temperature resistant silicone modified coating on the surface of the silver layer and only silver plating is explored.

[0033] In this embodiment, a high temperature resistant silicone modified coating is prepared using an organosilicon hydrophobic agent and nano-scale tungsten particles, and the organosilicon hydrophobic agent is a high temperature hydrophobic agent (model KN-8) produced by Konetz. Tungsten particles are added to the organosilicon hydrophobic agent at room temperature and stirred evenly for spraying.

[0034] The comparative test scheme is as follows:

[0035] 1. Two different surfaces of the base material are electroplated with silver, one of which is only silver-plated and is set as surface A, and the other surface is sprayed with a heat-resistant silicone modified coating on the surface of the silver-plated layer to form a hydrophobic film layer and is set as surface B. The desired coating structure can be obtained, and the coating thickness of surface A is approximately equal to that of surface B. 2. The prepared coated structure sample is placed in a gas nitriding furnace for comparative experiments. The parameters of the nitriding experiment are controlled to be the same, the nitriding temperature is 610°C, and the nitriding time is 40h. A total of four groups of comparative experiments are performed.

[0036] like Figure 1 The following is a microscopic comparison of the structures of the two coatings in the case of gas nitriding once. Figure 1 You can see:

[0037] Figure (A) shows, from left to right, the surface morphology and cross-sectional morphology of the coating surface A (only the silver-plated layer) when gas nitrided once, under a metallographic microscope at 50 times, 100 times, and 200 times (the rightmost A section in Figure (A) is observed at 200 times, and from left to right in the A section are the base material area, the silver-plated layer area, and the inlay material area used in the preparation of the metallographic sample);

[0038] Figure (B) shows the surface morphology and cross-sectional morphology of the coating surface B (silver-plated layer + hydrophobic film layer) when gas nitrided once under a metallographic microscope at 50 times, 100 times, and 200 times (the rightmost B section in Figure (B) was observed at 200 times, and from left to right in the B section are the inlay material area used in the preparation of the metallographic sample, the silver-plated layer + heat-resistant silicone modified coating area, and the substrate material area).

[0039] from Figure 2 You can see:

[0040] Figure (A) shows the surface morphology and cross-sectional morphology of the coating surface A (only the silver-plated layer) when gas nitrided twice under a metallographic microscope at 50 times, 100 times, and 200 times (the rightmost A section in Figure (A) is observed at 200 times, and from left to right are the base material area, the silver-plated layer area, and the inlay material area used in the preparation of the metallographic sample);

[0041] Figure (B) shows the surface morphology and cross-sectional morphology of the coating surface B (silver-plated layer + hydrophobic film layer) when gas nitrided twice under a metallographic microscope at 50 times, 100 times, and 200 times (the rightmost B cross-section in Figure (B) was observed at 200 times, and from left to right are the inlay material area used in the preparation of the metallographic sample, the silver-plated layer + heat-resistant silicone modified coating area, and the substrate material area).

[0042] from Figure 3 You can see:

[0043] Figure (A) shows the surface morphology and cross-sectional morphology of the coating surface A (only the silver-plated layer) when gas nitrided three times under a metallographic microscope at 50 times, 100 times, and 200 times (the rightmost A section in Figure (A) is observed at 200 times, and from the lower left to the upper right are the inlay material area, the silver-plated layer area, and the base material area used in the preparation of the metallographic sample);

[0044] Figure (B) shows the surface morphology and cross-sectional morphology of the coating surface B (silver-plated layer + hydrophobic film layer) when gas nitrided three times under a metallographic microscope at 50 times, 100 times, and 200 times (the rightmost B cross-section in Figure (B) was observed at 200 times, and from the lower left to the upper right are the base material area, the silver-plated layer + heat-resistant silicone modified coating area, and the inlay material area used in the preparation of the metallographic sample).

[0045] from Figure 4 You can see:

[0046] Figure (A) shows the surface morphology and cross-sectional morphology of the coating surface A (only the silver-plated layer) when gas nitrided 4 times under a metallographic microscope at 50 times, 100 times, and 200 times (the rightmost A section in Figure (A) is observed at 200 times, and from the upper left to the lower right are the base material area, the silver-plated layer area, and the inlay material area used in the preparation of the metallographic sample);

[0047] Figure (B) shows the surface morphology and cross-sectional morphology of the coating surface B (silver-plated layer + hydrophobic film layer) when gas nitrided 4 times under a metallographic microscope at 50 times, 100 times, and 200 times (the rightmost B cross-section in Figure (B) was observed at 200 times, and from the upper left to the lower right are the inlay material area used in the preparation of the metallographic sample, the silver-plated layer + heat-resistant silicone modified coating area, and the substrate material area).

[0048] Compare Figure 1 to Figure 4The following conclusions can be drawn: the coating structure was placed in a gas nitriding furnace for nitriding, the nitriding temperature was set to 610°C, and the nitriding time was set to 40 hours. After four comparative experiments, it can be observed that the silver-plated layer on the B side of the coating had no cracks or bubbles, and only the hydrophobic film layer had cracks or partial detachment, showing excellent high temperature resistance and anti-nitriding performance. It can be seen from the comparison that the performance of the silver-plated layer + hydrophobic film layer is better than that of the silver-plated layer alone. Figure 5 The solution of the present invention can be applied to a variety of different aircraft engine parts to meet different needs.

[0049] The contents not described in detail in the specification of the present invention belong to the prior art known to the professional and technical personnel in the field. Although the illustrative specific embodiments of the present invention are described above to facilitate the understanding of the present invention by the technical personnel in the field, it should be clear that the present invention is not limited to the scope of the specific embodiments. For ordinary technicians in the field of this technology, as long as various changes are within the spirit and scope of the present invention defined and determined by the attached claims, these changes are obvious, and all inventions and creations using the concept of the present invention are protected.

Claims

1. Anti-nitriding high temperature resistant coating, characterized in that: A single silver-plated layer or a composite coating of a silver-plated layer and a hydrophobic layer; The silver-plated layer is located on the surface of the substrate; The hydrophobic layer is located on the surface of the silver-plated layer and has both high temperature resistance and hydrophobicity.

2. The anti-nitriding high temperature resistant coating according to claim 1, characterized in that: The maximum temperature of the effective working temperature range of the hydrophobic layer is 650°C.

3. The anti-nitriding high temperature resistant coating according to claim 1, characterized in that: The hydrophobic layer is an organosilicon modified coating.

4. The anti-nitriding high temperature resistant coating according to claim 3, characterized in that: The organosilicon modified coating is based on an organosilicon water repellent agent and is obtained by adding solid particles of a high temperature resistant material with a particle size of nanometers.

5. The method for preparing the anti-nitriding high temperature resistant coating according to claim 1, characterized in that: The anti-nitriding high temperature resistant coating comprises a composite coating of a silver plating layer and a hydrophobic layer, and comprises the following preparation steps: S1, obtaining a silver plating layer on the substrate surface by electroplating or chemical plating; S2, spraying an organosilicon modified material on the surface of the silver-plated layer obtained in S1 to form a hydrophobic layer.

6. Use of the anti-nitriding and high-temperature resistant coating according to claim 1 in aircraft engines.

7. Application of the anti-nitriding and high temperature resistant coating in an aircraft engine according to claim 6, characterized in that: It includes a gear box, a fan casing, a heat exchanger, an intermediate casing, a combustion chamber sealing sleeve, a combustion chamber cover ring and guide vanes.

Citation Information

Patent Citations

  • Superhydrophobic coating material and preparation method of superhydrophobic coating material and application thereof

    CN109023449A

  • Metal surface fluoride-free super-hydrophobic coating and preparation method thereof

    CN110951296A

  • Semiconductor packaging silver colloid diffusion prevention technology

    CN115895437A