Preparation method of hydrophobic sound transmission coating with micro-nano structure
The micro-nano structure coating is prepared from a composite material of polyurethane and epoxy resin, which solves the limitations of traditional coatings in waterproof, sound-permeable and anti-fouling properties, and achieves efficient hydrophobic, anti-fouling and sound-permeable properties in the marine environment. , suitable for marine equipment, and has good durability and environmental protection characteristics.
Patent Information
- Application Number
- CN202410966501.9
- Authority / Receiving Office
- CN · China
- Patent Type
- Applications(China)
- Current Assignee / Owner
- Filing Date
- 2024-07-18
- Publication Date
- 2024-10-11
AI Technical Summary
Traditional antifouling coatings have limitations in terms of waterproof and sound-permeable performance, and commonly used antifouling agents are toxic, making it difficult to have both sound-permeable and antifouling properties, and cannot effectively resist pollution and corrosion in the marine environment.
It uses a composite material of polyurethane and epoxy resin, uses a hydrophobic sound-transmitting coating with a micro-nano structure, and rationally regulates the ratio of soft and hard segments to form an orderly migration of polar bonds and non-polar bonds to achieve micro-nano convexities on the surface of the material. Structure, enhance hydrophobicity and sound transmission properties.
A coating with excellent hydrophobic, antifouling and sound-permeable properties in the marine environment has been achieved, reducing the adhesion of marine organisms and improving sound wave absorption and scattering effects. It is suitable for marine equipment, and the material is relatively environmentally friendly, has good durability and Self-cleaning properties.
Smart Images

Figure CN118755379A_ABST
Abstract
Description
Technical Field
[0001] The invention relates to a method for preparing a hydrophobic coating. Background Art
[0002] The research on marine antifouling coatings has always been an important topic in the field of marine engineering. There are various biological and non-biological factors in the marine environment, which can have adverse effects on acoustic equipment and materials. One of the main problems is that marine acoustic equipment and structures are easily affected by pollution, which may lead to a decline in acoustic performance or even failure. Therefore, the development of antifouling marine acoustic materials is an important part of ensuring the stable operation of acoustic equipment. However, there are certain restrictions on the performance and sound permeability of traditional antifouling coatings. Traditional antifouling hydrophobic coatings are usually prepared with silicone or fluorine-containing materials. Although these materials have good antifouling effects, they are not ideal waterproof and sound-permeable materials. At present, polyurethane is mostly used as a sound-permeable material for sound-permeable materials. Polyurethane has characteristics similar to seawater impedance. This acoustic impedance matching makes polyurethane an ideal choice for sound-permeable materials. It can effectively transmit sound energy and reduce energy loss, making it have important application potential in marine engineering. Therefore, in marine engineering, polyurethane materials are widely used in the manufacture of key components such as sonar reflectors, sonar windows, and sonar arrays. With the growing demand for sound-permeable materials in the marine engineering field, sound-permeable materials are easily corroded by pollutants and corrosive media in the marine environment, resulting in performance degradation and shortened life. In order to cope with pollution problems in the marine environment, such as algae, seaweed, corrosive substances, etc., they may adhere to the surface of marine engineering facilities, affecting the performance of sound-permeable materials. Researchers have begun to pay attention to the anti-fouling properties of sound-permeable materials. Materials with anti-fouling properties can reduce the adhesion of moisture and pollutants on the surface, maintain the cleanliness of the material and the stability of its performance. At present, the ideal polyurethane-based sound-permeable material cannot have both sound-permeable and anti-fouling properties. The existing sound-permeable coatings mainly achieve anti-fouling properties by adding anti-biological attachment agents or using bactericides, but most anti-fouling agents are toxic, and the international community has banned the use of harmful compounds in anti-fouling coatings for ships. In order to solve these problems, researchers have begun to explore new anti-fouling sound-permeable materials and preparation methods. Summary of the invention
[0003] In order to solve the above technical problems, the present invention provides a method for preparing a hydrophobic sound-transmitting coating with a micro-nano structure.
[0004] A method for preparing a hydrophobic sound-transmitting coating with a micro-nano structure is specifically completed by the following steps:
[0005] 1. Evenly mix the hydroxy-terminated polybutadiene, the catalyst and the isocyanate, and react them at 60°C to 80°C for a period of time to obtain a polyurethane prepolymer;
[0006] 2. Add bisphenol A epoxy resin to the polyurethane prepolymer, continue stirring and reacting for 3h to 6h at a certain temperature to obtain a polyurethane / epoxy resin system;
[0007] 3. Dissolve the polyurethane / epoxy resin system and amine curing agent in a polar solvent, stir evenly, filter using a mesh, and then brush, spray or spin-coat onto a glass plate, and then dry and cure in an oven to obtain a hydrophobic sound-transmitting coating with a micro-nano structure.
[0008] Principle of the present invention:
[0009] The polyurethane epoxy resin composite material (hydrophobic sound-transmitting coating with micro-nano structure) provided by the present invention has unique advantages; the composite of polyurethane and epoxy resin significantly improves the physical properties of the material; polyurethane has adjustable flexibility, while epoxy resin has excellent adhesion and mechanical properties; by reasonably regulating the ratio of polyurethane and epoxy resin, controlling the ratio of soft and hard segments to form an orderly migration of polar bonds and non-polar bonds, a micro-nano protrusion structure can be formed on the surface of the material, and the coating has both excellent hydrophobicity and good sound-transmitting performance; the surface microstructure of the coating is similar to the bionic microstructure of the biological epidermis, so that the coating has hydrophobicity, and the microstructure increases the contact area between the material and the sound wave, improves the absorption and scattering effect of the sound wave, thereby improving the sound-transmitting performance, so that the prepared coating has both antifouling performance and sound-transmitting performance. It is expected to play an important role in the field of marine antifouling and sound-transmitting.
[0010] Advantages of the present invention:
[0011] 1. The present invention is to mix HTPB type polyurethane and epoxy resin for cross-linking and curing, control the ratio of soft and hard segments to achieve orderly migration of polar bonds and non-polar bonds, and form a micro-nano structure coating, which has excellent anti-fouling performance and sound transmission performance;
[0012] 2. The hydrophobic sound-transmitting coating with micro-nano structure prepared by the present invention has excellent hydrophobicity and good sound transmission performance. The coating can effectively reduce the attachment of marine organisms and provide excellent sound transmission characteristics, and is suitable for the fields of ships, marine equipment, etc. The static water contact angle of the coating reaches 102°, and the sound transmission performance is good;
[0013] 3. The hydrophobic sound-transmitting coating with micro-nano structure prepared by the present invention has a hydrophobic micro-nano structure coating, which has both excellent hydrophobic antifouling performance and good sound-transmitting performance, overcoming the limitations of traditional materials. This new coating has good durability and can withstand the influence of common external factors while maintaining stable hydrophobic performance. HTPB type polyurethane (hydroxyl-terminated polybutadiene) and epoxy resin (bisphenol A type epoxy resin) are relatively environmentally friendly materials, without volatile organic compound emissions, and do not contain substances harmful to human health. It has broad application prospects in the field of antifouling and sound-transmitting;
[0014] Fourth, the hydrophobic sound-transmitting coating with micro-nano structure prepared by the present invention has significant hydrophobic properties, can effectively resist the erosion of water and pollutants, and protect the surface of the substrate; the micro-nano structure makes the coating have good self-cleaning properties, reducing the frequency and cost of cleaning and maintenance;
[0015] 5. The preparation process of the present invention is simple and has high stability, and is suitable for large-area coating and substrates with complex shapes;
[0016] 6. The hydrophobic sound-transmitting coating with micro-nano structure prepared by the present invention has broad application prospects in the fields of marine sound-transmitting anti-fouling, aerospace, building materials, etc. BRIEF DESCRIPTION OF THE DRAWINGS
[0017] Figure 1 This is an atomic force microscope scan of the hydrophobic sound-transmitting coating with micro-nano structure prepared in Example 1;
[0018] Figure 2 This is the static water contact angle of the hydrophobic sound-transmitting coating with micro-nano structure prepared in Example 1. DETAILED DESCRIPTION
[0019] Specific implementation method 1: This implementation method is a method for preparing a hydrophobic sound-transmitting coating with a micro-nano structure, which is specifically completed by the following steps:
[0020] 1. Evenly mix the hydroxy-terminated polybutadiene, the catalyst and the isocyanate, and react them at 60°C to 80°C for a period of time to obtain a polyurethane prepolymer;
[0021] 2. Add bisphenol A epoxy resin to the polyurethane prepolymer, continue stirring and reacting for 3h to 6h at a certain temperature to obtain a polyurethane / epoxy resin system;
[0022] 3. Dissolve the polyurethane / epoxy resin system and amine curing agent in a polar solvent, stir evenly, filter using a mesh, and then brush, spray or spin-coat onto a glass plate, and then dry and cure in an oven to obtain a hydrophobic sound-transmitting coating with a micro-nano structure.
[0023] Specific embodiment 2: This embodiment differs from specific embodiment 1 in that: the catalyst in step 1 is dibutyltin dilaurate; the isocyanate in step 1 is isophorone diisocyanate, hexamethylene diisocyanate, diphenylmethane diisocyanate, toluene diisocyanate or dicyclohexylmethane diisocyanate. The other steps are the same as those in specific embodiment 1.
[0024] Specific embodiment 3: This embodiment differs from specific embodiment 1 or 2 in that the molar ratio of -NCO in the isocyanate to -OH in the hydroxyl-terminated polybutadiene in step 1 is 1.4. The other steps are the same as those in specific embodiment 1 or 2.
[0025] Specific embodiment 4: This embodiment differs from specific embodiments 1 to 3 in that the mass of the catalyst in step 1 accounts for 0.01% to 0.015% of the total mass of the hydroxy-terminated polybutadiene, the catalyst and the isocyanate; the reaction time in step 1 is 4h to 6h. The other steps are the same as those in specific embodiments 1 to 3.
[0026] Specific embodiment 5: This embodiment differs from specific embodiments 1 to 4 in that the bisphenol A epoxy resin in step 2 is E44, E51 or E54. The other steps are the same as those in specific embodiments 1 to 4.
[0027] Specific embodiment 6: This embodiment differs from specific embodiments 1 to 5 in that: the reaction temperature in step 2 is 80°C to 100°C; the mass ratio of bisphenol A epoxy resin to polyurethane prepolymer in step 2 is (10 to 40): (60 to 90). The other steps are the same as those in specific embodiments 1 to 5.
[0028] Specific embodiment 7: This embodiment differs from specific embodiments 1 to 6 in that: the amine curing agent in step 3 is MOCA curing agent or DETDA curing agent; the polar solvent in step 3 is ketone solvent, ester solvent, ether solvent or thiol solvent. The other steps are the same as those in specific embodiments 1 to 6.
[0029] Specific embodiment eight: This embodiment differs from specific embodiments one to seven in that: the ketone solvent is acetone or butanone; the ester solvent is a mixture of one or more of methyl formate, dimethyl carbonate, ethyl acetate, tert-butyl acetate and sec-butyl acetate; the ether solvent is a mixture of one or more of ethyl ether, isopropyl ether, n-butyl ether and diphenyl ether; the thiol solvent is a mixture of one or more of methyl mercaptan, ethyl mercaptan and ethanedithiol. The other steps are the same as those of specific embodiments one to seven.
[0030] Specific embodiment 9: This embodiment differs from specific embodiments 1 to 8 in that: the mass ratio of the polyurethane / epoxy resin system and the amine curing agent in step 3 is (20-100):(6-32); the mass ratio of the polyurethane / epoxy resin system and the polar solvent in step 3 is (20g-100g):(2mL-40mL). The other steps are the same as specific embodiments 1 to 8.
[0031] Specific embodiment 10: This embodiment differs from specific embodiments 1 to 9 in that: the screen described in step 3 is 160 mesh to 250 mesh; the drying temperature described in step 3 is 50°C to 70°C, and the drying time is 2h to 4h; the curing temperature described in step 3 is 80°C to 100°C, and the curing time is 20h to 24h. The other steps are the same as specific embodiments 1 to 9.
[0032] The following examples are used to verify the beneficial effects of the present invention:
[0033] Embodiment 1: A method for preparing a hydrophobic sound-transmitting coating having a micro-nano structure, characterized in that the preparation method is specifically completed according to the following steps:
[0034] 1. Evenly mix hydroxy-terminated polybutadiene (HTPB), dibutyltin dilaurate and isocyanate, and react at 80° C. for 4 hours to obtain a polyurethane prepolymer;
[0035] The isocyanate described in step 1 is isophorone diisocyanate;
[0036] The molar ratio of -NCO in the isocyanate to -OH in the hydroxy-terminated polybutadiene described in step 1 is 1.4;
[0037] The mass of the dibutyltin dilaurate described in step 1 accounts for 0.015% of the total mass of the hydroxy-terminated polybutadiene, the catalyst and the isocyanate;
[0038] 2. Add bisphenol A epoxy resin to the polyurethane prepolymer, continue stirring and reacting at 100° C. for 3 hours to obtain a polyurethane / epoxy resin system;
[0039] The bisphenol A epoxy resin described in step 2 is E51;
[0040] The mass ratio of the bisphenol A epoxy resin to the polyurethane prepolymer described in step 2 is 20:80;
[0041] 3. Dissolve 100 parts of polyurethane / epoxy resin system and 24 parts of amine curing agent in 35 parts of ethyl acetate, stir evenly, filter with a 200-mesh sieve, spray onto a glass plate, dry in an oven at 50°C for 2h, and then cure at 80°C for 24h to obtain a hydrophobic sound-transmitting coating with a micro-nano structure;
[0042] The amine curing agent described in step three is MOCA curing agent.
[0043] Figure 1 This is an atomic force microscope scan of the hydrophobic sound-transmitting coating with micro-nano structure prepared in Example 1;
[0044] from Figure 1 It can be seen that the micro-protrusion structure on the surface of the hydrophobic sound-transmitting coating with micro-nano structure prepared in Example 1.
[0045] Figure 2 This is the static water contact angle of the hydrophobic sound-transmitting coating with micro-nano structure prepared in Example 1.
[0046] from Figure 2 It can be seen that the static water contact angle of the hydrophobic sound-transmitting coating with micro-nano structure prepared in Example 1 is 102°.
Claims
1. A method for preparing a hydrophobic sound-transmitting coating having a micro-nano structure, characterized in that The preparation method is specifically completed according to the following steps:
1. Evenly mix the hydroxy-terminated polybutadiene, the catalyst and the isocyanate, and react them at 60°C to 80°C for a period of time to obtain a polyurethane prepolymer; 2. Add bisphenol A epoxy resin to the polyurethane prepolymer, continue stirring and reacting for 3h to 6h at a certain temperature to obtain a polyurethane / epoxy resin system; 3. Dissolve the polyurethane / epoxy resin system and amine curing agent in a polar solvent, stir evenly, filter using a mesh, and then brush, spray or spin-coat onto a glass plate, and then dry and cure in an oven to obtain a hydrophobic sound-transmitting coating with a micro-nano structure.
2. The method for preparing a hydrophobic sound-transmitting coating having a micro-nano structure according to claim 1, characterized in that The catalyst described in step 1 is dibutyltin dilaurate; the isocyanate described in step 1 is isophorone diisocyanate, hexamethylene diisocyanate, diphenylmethane diisocyanate, toluene diisocyanate or dicyclohexylmethane diisocyanate.
3. The method for preparing a hydrophobic sound-transmitting coating having a micro-nano structure according to claim 1, characterized in that The molar ratio of -NCO in the isocyanate to -OH in the hydroxy-terminated polybutadiene described in step 1 is 1.
4.
4. The method for preparing a hydrophobic sound-transmitting coating having a micro-nano structure according to claim 1, characterized in that The mass of the catalyst described in step 1 accounts for 0.01% to 0.015% of the total mass of the terminal hydroxyl polybutadiene, the catalyst and the isocyanate; and the reaction time described in step 1 is 4h to 6h.
5. The method for preparing a hydrophobic sound-transmitting coating having a micro-nano structure according to claim 1, characterized in that The bisphenol A type epoxy resin described in step 2 is E44, E51 or E54.
6. The method for preparing a hydrophobic sound-transmitting coating having a micro-nano structure according to claim 1, characterized in that The reaction temperature in step 2 is 80° C. to 100° C.; the mass ratio of the bisphenol A epoxy resin to the polyurethane prepolymer in step 2 is (10 to 40): (60 to 90).
7. The method for preparing a hydrophobic sound-transmitting coating having a micro-nano structure according to claim 1, characterized in that The amine curing agent described in step 3 is a MOCA curing agent or a DETDA curing agent; the polar solvent described in step 3 is a ketone solvent, an ester solvent, an ether solvent or a thiol solvent.
8. The method for preparing a hydrophobic sound-transmitting coating having a micro-nano structure according to claim 7, characterized in that The ketone solvent is acetone or butanone; the ester solvent is a mixture of one or more of methyl formate, dimethyl carbonate, ethyl acetate, tert-butyl acetate and sec-butyl acetate; the ether solvent is a mixture of one or more of ethyl ether, isopropyl ether, n-butyl ether and diphenyl ether; the thiol solvent is a mixture of one or more of methyl mercaptan, ethyl mercaptan and ethanedithiol.
9. The method for preparing a hydrophobic sound-transmitting coating having a micro-nano structure according to claim 1, characterized in that The mass ratio of the polyurethane / epoxy resin system described in step 3 to the amine curing agent is (20-100):(6-32); the volume ratio of the mass of the polyurethane / epoxy resin system described in step 3 to the polar solvent is (20g-100g):(2mL-40mL).
10. The method for preparing a hydrophobic sound-transmitting coating having a micro-nano structure according to claim 1, characterized in that The sieve described in step three is 160 mesh to 250 mesh; the drying temperature described in step three is 50°C to 70°C, and the drying time is 2h to 4h; the curing temperature described in step three is 80°C to 100°C, and the curing time is 20h to 24h.
Citation Information
Patent Citations
Preparation method of composite superhydrophobic coating possessing abrasion-resistance performance
CN104327703A
Preparation method of epoxidized hydroyl-terminated polybutadiene type polyurethane low surface energy material
CN108285522A
Sealing coating material for deep sea underwater acoustic transducer and preparation method of sealing coating material
CN116063843A
Monohydroxylated 1,3-polybutadiene / polyisocyanate product reacted with hydroxyl-functional resin
US5378761A