Maleic anhydride grafted polymer fluid loss reducer

Through maleic anhydride graft polymer filtration loss reduction agent, the problems of chemical incompatibility and abnormal viscosity during the conversion of filtration loss reduction agent in drilling fluid are solved, and good performance in oil-based and water-based are achieved, reducing the performance of the oil-based and water-based products. Filtration loss and improve the stability and environmental protection of drilling fluid.

CN118755456BActive Publication Date: 2024-11-22SICHUAN SHANG ZHI DENG NEW MATERIALS CO LTD
View PDF 0 Cites 0 Cited by

Patent Information

Application Number
CN202411238965.4
Authority / Receiving Office
CN · China
Patent Type
Patents(China)
Current Assignee / Owner
Filing Date
2024-09-05
Publication Date
2024-11-22
Estimated Expiration
2044-09-05

AI Technical Summary

Technical Problem

During the drilling process, the conversion of filtration loss agents between oil-based and water-based drilling fluids often leads to chemical incompatibility, viscosity and rheology abnormalities, resulting in filtration loss control failure, increasing the risk of complex problems in the hole, and Bringing environmental and health risks.

Method used

Maleic anhydride grafted polymer filtration loss agent, which consists of unsaturated anhydride, polyethylene glycol, lignin, polar wax, nanosilica and initiator, and amphiphilicity is formed through a specific preparation process. The polymer can show good dispersion and stability in both oil-based and water-based, form a dense barrier layer and reduce the penetration of the filtrate.

Benefits of technology

Effectively reduce filtration loss, improve the thermal stability and shear stability of drilling fluid, enhance the biodegradability and environmental friendliness of the materials, and is suitable for drilling operations under complex formation conditions, significantly improving drilling efficiency and safety.

✦ Generated by Eureka AI based on patent content.

Smart Images

  • Figure SMS_1
    Figure SMS_1
Patent Text Reader

Abstract

The invention discloses a maleic anhydride grafted polymer fluid loss reducer, relates to the technical field of fluid loss reducers, and is composed of the following raw materials, 5-8 parts of unsaturated anhydride, 2-3 parts of polyethylene glycol, 30-50 parts of lignin, 25-35 parts of polar wax, 2-5 parts of nano-silicon dioxide, 0.7-1 parts of initiator and 170-190 parts of organic solvents, by weight; the formula fluid loss reducer can effectively reduce the filtration rate, form a dense and thin filter cake, thereby protecting the well wall to the greatest extent and reducing the invasion of formation fluids. At the same time, it maintains a moderate viscosity, ensures the good fluidity and carrying capacity of the drilling fluid, and does not interfere with normal drilling operations. In addition, the fluid loss reducer can still maintain stable performance under high temperature conditions, has good thermal stability, and is suitable for use in complex downhole environments of high temperature and high pressure. These characteristics make it show a wide range of adaptability in both oil-based and water-based drilling fluids, and is a highly efficient drilling fluid additive.
Need to check novelty before this filing date? Find Prior Art

Description

Technical Field

[0001] The invention relates to the technical field of fluid loss reducers, and in particular to a maleic anhydride grafted polymer fluid loss reducer. Background Art

[0002] Fluid loss reducers are key additives in drilling fluids and completion fluids. They are mainly used to control the phenomenon of liquid infiltration into the formation during drilling, thereby preventing wellbore collapse and formation pollution. They reduce fluid loss by forming a dense filter cake, increasing drilling fluid viscosity and plugging formation pores. Commonly used fluid loss reducers include organic compounds and inorganic materials such as bentonite and calcium carbonate. With the development of drilling technology, fluid loss reducers have gradually evolved in the direction of environmental protection, high temperature and high pressure adaptability, and nanomaterial application to improve performance stability and reduce costs, thereby better meeting the needs under complex geological conditions.

[0003] In addition, in order to adapt to changes in formation conditions, solve downhole problems, meet environmental and economic requirements, improve drilling efficiency, and meet specific technical and operational requirements. For example, in high-temperature and high-pressure formations or unstable formations, oil-based drilling fluids have better stability and lubricity than water-based drilling fluids, and are suitable for drilling operations under complex formation conditions. In areas with higher environmental requirements, water-based drilling fluids have more advantages due to their lower environmental impact. Therefore, in different drilling stages and environmental conditions, it is often necessary to switch between these two drilling fluids to ensure the safety, efficiency, and environmental friendliness of drilling operations.

[0004] However, the fluid loss reducers commonly used in oil-based drilling fluids and water-based drilling fluids are different. During the conversion process, mixed pollution of different types of fluid loss reducers will be involved. Mixing different fluid loss reducers may lead to chemical incompatibility, abnormal viscosity and rheology, and failure of fluid loss control. These problems may reduce the performance of the drilling fluid, make it impossible to effectively control the fluid loss, and increase the risk of complex problems downhole, and may also bring environmental and health hazards.

[0005] Therefore, developing an oil-based and water-based dual-purpose fluid loss reducer can effectively avoid this problem and improve drilling efficiency. Summary of the invention

[0006] The present invention aims to provide a maleic anhydride grafted polymer fluid loss reducer to solve the above problems.

[0007] The present invention is achieved through the following technical solutions:

[0008] A maleic anhydride grafted polymer fluid loss reducer comprises the following components by weight: 5-8 parts of unsaturated anhydride, 2-3 parts of polyethylene glycol, 30-50 parts of lignin, 25-35 parts of polar wax, 2-5 parts of nano silicon dioxide, 0.7-1 parts of initiator and 170-190 parts of organic solvent; wherein the unsaturated anhydride is maleic anhydride.

[0009] The maleic anhydride grafted polymer fluid loss reducer also includes the following preparation process:

[0010] S1: dissolving or dispersing lignin and polar wax in an organic solvent to form a uniform solution or suspension, slowly adding an initiator under stirring conditions, and heating the reaction mixture until all raw material components are fully reacted to obtain solution I;

[0011] S2: adding unsaturated acid anhydride to solution I, adjusting the reaction temperature, maintaining the stirring speed, and waiting for the raw material components to fully react to obtain solution II;

[0012] S3: dissolving polyethylene glycol in an organic solvent to form a uniform solution, then adding unsaturated acid anhydride, slowly adding an initiator under stirring, and heating the mixture until all raw material components are fully reacted to obtain solution III;

[0013] S4: Mixing solution II and solution III under stirring conditions at 500-900 rpm, slowly adding nano-silicon dioxide, maintaining the stirring conditions for 10-30 minutes, and drying and crushing the obtained product to obtain the maleic anhydride grafted polymer fluid loss reducer.

[0014] The maleic anhydride grafted polymer fluid loss reducer uses benzoyl peroxide as an initiator and toluene as an organic solvent. The weight ratio of polar wax to lignin is between 0.3 and 1, which is used to control the lignin to fully react and polymerize with the polar wax and control the overall performance in different base liquids; the polar wax uses a polar wax with a size between 500-3000 Daltons, and the lignin uses a lignin with a size between 20000-50000 Daltons; by controlling the size ratio of polar wax to lignin, it is ensured that the polar wax and lignin polymer have balanced amphiphilicity (hydrophilicity and hydrophobicity), and by controlling the molecular size of lignin and polar wax, the interface compatibility, mechanical properties and barrier properties of the composite material can be effectively improved. More matching molecular sizes help to form more stable chemical bonds or physical entanglements, thereby enhancing the strength and flexibility of the material. At the same time, larger lignin and polar wax molecules can form a denser structure and improve the water and gas barrier capacity of the material. In addition, the control of molecular size can also adjust the amphiphilicity of lignin and polar wax grafted polymers, making them better adapted to different base liquids and optimizing the performance of composite materials. In this way, the thermal stability, mechanical strength and biodegradability of the material can be adjusted as needed to meet the performance of the polymer in oil-based and water-based. Finally, the polymer is further modified by maleic anhydride to enable it to perform better in oil-based and water-based.

[0015] The preparation temperature range of solution I is 80-90 degrees Celsius, the stirring speed is 500-900 rpm, and the reaction time is 3-6 hours; the reaction temperature range of solution II is 60-80 degrees Celsius, the stirring speed is 500-900 rpm, and the reaction time is 2-4 hours; the reaction temperature range of solution III is 60-80 degrees Celsius, the stirring speed is 500-900 rpm, and the reaction time is 3-5 hours; by controlling the screening conditions of solution I, solution II and solution III, the full reaction of the polar groups therein is ensured.

[0016] Compared with the prior art, the present invention has the following advantages and beneficial effects:

[0017] 1. In the fluid loss reducer of the present invention, the lignin grafted polar wax itself has good amphiphilicity and can show excellent dispersibility and stability at the oil-water interface. This performance is crucial for both oil-based and water-based drilling fluids. The introduction of maleic anhydride further enhances the hydrophilicity of the polymer and increases the reactivity of the polymer, making it more prominent in the water-based system. Maleic anhydride grafting can form a denser protective layer on the filter cake by chemically reacting with the mineral surface, significantly reducing the fluid loss;

[0018] 2. The grafted polymer of the fluid loss reducer of the present invention can form an efficient barrier layer, reduce the penetration of drilling fluid through the filter cake, and thus effectively reduce the fluid loss. The grafted polymer of lignin, polar wax and maleic anhydride can form a more dense and uniform structure on the surface of the filter cake, reduce the permeability of the filtrate, and thus effectively control the fluid loss;

[0019] 3. In the fluid loss reducer of the present invention, the lignin grafted polymer can maintain good performance under high temperature and high pressure environment, which helps to improve the thermal stability and shear stability of the drilling fluid. The polar group of maleic anhydride increases the solubility and stability of the polymer in the aqueous phase, so that the rheological properties of the drilling fluid are improved and the risk of well wall instability is reduced;

[0020] 4. In the fluid loss reducer of the present invention, lignin is derived from natural materials, and the grafted polymer of lignin, polar wax and maleic anhydride has certain biodegradability and environmental friendliness, and meets the requirements of green environmental protection in drilling operations;

[0021] 5. The fluid loss reducer of the present invention is a fluid loss reducer in which lignin is grafted with polar wax and then grafted with maleic anhydride as a whole to form an amphiphilic polymer, which exhibits excellent dual-use effects in oil-based and water-based drilling fluids. Its unique amphiphilic structure enables the polymer to be evenly dispersed in the oil-based drilling fluid and form a dense filter cake, significantly reducing the fluid loss. At the same time, in the water-based drilling fluid, through the action of its hydrophilic group, the solubility and stability of the polymer in water are enhanced, further improving the anti-fluid loss performance of the water-based drilling fluid. This material not only exhibits good adaptability and stability in different types of drilling fluids, but also, because it is derived from natural lignin, it has certain environmental protection and biodegradability, and is suitable for wide application in modern drilling operations. DETAILED DESCRIPTION

[0022] In order to make the purpose, technical solutions and advantages of the present invention more clearly understood, the present invention is further described in detail below in conjunction with embodiments. The illustrative embodiments of the present invention and their description are only used to explain the present invention and are not intended to limit the present invention.

[0023] Example 1

[0024] A maleic anhydride grafted polymer fluid loss reducer is prepared from the following raw materials in parts by weight: 7 parts of maleic anhydride, 3 parts of polyethylene glycol, 35 parts of lignin, 35 parts of polar wax, 4 parts of nano silicon dioxide, 0.9 parts of benzoyl peroxide and 180 parts of toluene.

[0025] The maleic anhydride grafted polymer fluid loss reducer also includes the following preparation process:

[0026] S1: 35 parts of lignin and 35 parts of polar wax are dissolved or dispersed in 160 parts of toluene solvent to form a uniform solution or suspension, 0.8 parts of benzoyl peroxide are slowly added under stirring conditions at 600 rpm, and the reaction mixture is heated to 80 degrees Celsius, and the reaction conditions are maintained until all raw material components are fully reacted for 4 hours to obtain solution I;

[0027] S2: Add 6 parts of maleic anhydride to solution I, adjust the reaction temperature to 65 degrees Celsius, maintain the stirring speed at 600 rpm, and maintain the reaction conditions until all raw material components are fully reacted for 2.5 hours to obtain solution II;

[0028] S3: 3 parts of polyethylene glycol are dissolved in 20 parts of toluene solvent to form a uniform solution, and then 1 part of maleic anhydride is added, and 0.1 part of benzoyl peroxide is slowly added under stirring conditions at 600 rpm, and the mixture is heated to 65 degrees Celsius, and the reaction conditions are maintained until all raw material components are fully reacted for 4 hours to obtain solution III;

[0029] S4: Mix solution II and solution III under stirring at 600 rpm, slowly add 4 parts of nano-silicon dioxide, maintain the stirring condition for 20 minutes, heat and dry the obtained product, and crush it to obtain the maleic anhydride grafted polymer fluid loss reducer.

[0030] The lignin is a complex organic polymer compound that mainly exists in the cell walls of plants. Its molecular structure contains a large number of aromatic rings and functional groups such as phenolic hydroxyl groups, which makes lignin hydrophobic to a certain extent. However, lignin also contains a certain number of polar groups (such as hydroxyl groups, carboxyl groups, etc.), which can form hydrogen bonds with water molecules, giving lignin a certain hydrophilicity. Therefore, natural lignin itself has a certain amphiphilicity. The polar wax generally refers to waxy substances containing polar groups, such as fatty acids and their esters, alcohols, etc. These polar groups can interact with water molecules, making these waxy substances hydrophilic to a certain extent. The hydrocarbon chains of the wax make it hydrophobic (polar wax is more hydrophobic). When lignin is grafted with polar wax, the hydrophobic part of lignin interacts with the hydrophobic part of polar wax, and the polar groups of lignin and polar wax can also interact with each other. This grafting reaction can further enhance the amphiphilicity of the material, so that it has good dispersibility and stability in different media. The material after grafting lignin and polar wax has amphiphilicity because it contains both hydrophilic and hydrophobic parts. At the same time, the size of the lignin and polar wax participating in the reaction is constrained, wherein the polar wax adopts a polar wax with a size between 500-3000 Daltons, and the lignin adopts a lignin with a size between 20000-50000 Daltons. The high molecular polymer after grafting lignin and polar wax has amphiphilicity, and the amphiphilicity is further enhanced, which helps the dissolution of the high molecular polymer in oil-based or water-based. This amphiphilicity enables the polymer to show good dispersibility and stability in both oil-based and water-based systems. In oil-based systems, such polymers can interact with oil through their hydrophobic parts to enhance dispersibility. In water-based systems, their polar group parts can interact with water to stabilize the suspension system or be used as an emulsifier. The lignin and polar wax grafted polymers are then polymerized with maleic anhydride (maleic anhydride is about 100 Daltons in size, and multiple maleic anhydrides can be grafted onto the polymer), which is a compound containing highly polar groups. After being grafted with lignin or other polymer materials, the polymer acquires significant hydrophilicity, while the hydrophobic part of the raw material maintains its hydrophobic properties. Therefore, this grafted polymer is also amphiphilic. In oil-based systems, the hydrophobic part of the maleic anhydride grafted polymer is compatible with oil, while the polar groups can give it dispersibility and stability in water. In water-based systems, the polar groups enhance the interaction with water, allowing it to adapt to the water base.

[0031] It is worth noting that the production of lignin in the molecular weight range of 20,000-50,000 Dalton (Da) can be carried out by a variety of methods, including separation and extraction, polymer modification and molecular weight classification. For example, the sulfite process (this lignin is usually derived from the pulp and paper industry and is obtained through the sulfite process. It has a wide range of molecular weights, and after proper treatment, lignin of 20,000-50,000 Da can be obtained), the alkaline process (lignin extracted from plants through an alkaline process has a larger molecular weight and is closer to the required range), the method of controlling temperature and time (the molecular weight of lignin can be controlled by adjusting the temperature and time of extraction. Lower extraction temperatures and shorter extraction times help to maintain a higher molecular weight), by controlling the type of solvent (selecting a suitable solvent system, such as organic solvents, water or alkaline solutions, can affect the solubility and molecular weight of lignin. Using milder solvents can reduce the degradation of lignin and retain a higher molecular weight), oxidative polymerization (the molecular weight of lignin can be increased to 20,000-50,000 by controlling the conditions of the oxidative polymerization reaction, such as the concentration and temperature of oxygen or peroxide. Da range. Oxidative polymerization is usually carried out under mild conditions to avoid excessive degradation), cross-linking reaction (by introducing cross-linking agents, such as formaldehyde, glutaraldehyde, etc., to form chemical bonds between lignin molecules and increase their molecular weight. The cross-linking reaction needs to be precisely controlled to avoid excessive cross-linking resulting in excessive molecular weight), gel permeation chromatography (GPC) (GPC technology can be used to separate lignin in the target molecular weight range. This method can accurately grade lignin according to molecular weight and select lignin parts of 20,000-50,000 Da) and ultrafiltration technology (using ultrafiltration membranes with different pore sizes to separate lignin molecules according to molecular weight and retain the required high molecular weight parts) and other methods or methods for production. Finally, the molecular weight and distribution of lignin are characterized by using nuclear magnetic resonance (NMR), infrared spectroscopy (FTIR), mass spectrometry (MS) and other technologies to ensure that the produced lignin meets the requirements of 20,000-50,000 Da. In addition, the production of polar waxes in the molecular weight range of 500-3000 Da can be carried out by the following methods, including polymerization, degradation and modification. For example, low molecular weight polymer polymerization (by controlling the conditions of the polymerization reaction, such as reaction time, temperature, concentration of the initiator, etc., to synthesize polar waxes with a specific molecular weight range. For example, by free radical polymerization or ring-opening polymerization, at lower temperatures and shorter reaction times, polymers with molecular weights between 500-3000 Da can be obtained. By introducing different types of monomers during the polymerization process, such as ethylene, acrylates, etc., low molecular weight copolymers with polar functional groups can be produced.These copolymers can have the desired polarity and target molecular weight), thermal degradation (by heating high molecular weight polymers, controlling the degradation time and temperature, reducing the polymer chain length, and obtaining polar waxes in the desired molecular weight range. This method can be achieved by thermal cracking under controlled conditions), chemical degradation (using acids, alkalis or other chemical reagents to treat high molecular weight polar waxes to cause degradation reactions and reduce the molecular weight to the desired range. Chemical degradation can be carried out by hydrolysis, transesterification, etc.), modified polyethylene glycol (by chemically modifying polyethylene glycol (PEG), introducing polar functional groups such as hydroxyl, carboxyl, sulfonic acid, etc., and controlling the reaction conditions and chain length, 500-3000 Da polar wax. Common modification reactions include esterification, etherification, cross-linking, etc.), adding polar groups (in the process of synthesis or degradation, polar waxes within the target molecular weight range are obtained by introducing polar monomers or chemical modifications. For example, maleic anhydride, acrylic acid, alcohols, etc. are used for grafting or cross-linking reactions) and molecular weight selective separation (through membrane filtration, ultrafiltration or gel permeation chromatography (GPC) and other separation techniques, mixed polymers or degradation products are graded to select components with molecular weights between 500-3000 Da. These separation techniques can accurately control the molecular weight distribution of the final product), thereby producing polar waxes with a target molecular weight range.

[0032] Example 2

[0033] A maleic anhydride grafted polymer fluid loss reducer is prepared from the following raw materials in parts by weight: 6 parts of maleic anhydride, 3 parts of polyethylene glycol, 40 parts of lignin, 35 parts of polar wax, 4 parts of nano silicon dioxide, 0.9 parts of benzoyl peroxide and 180 parts of toluene.

[0034] The maleic anhydride grafted polymer fluid loss reducer also includes the following preparation process:

[0035] S1: 40 parts of lignin and 35 parts of polar wax are dissolved or dispersed in 160 parts of toluene to form a uniform solution or suspension, 0.8 parts of benzoyl peroxide are slowly added under stirring conditions at 600 rpm, and the reaction mixture is heated to 80 degrees Celsius, and the reaction conditions are maintained until all raw material components are fully reacted for 4 hours to obtain solution I;

[0036] S2: Add 5 parts of maleic anhydride to solution I, adjust the reaction temperature to 65 degrees Celsius, maintain the stirring speed at 600 rpm, and maintain the reaction conditions until all raw material components are fully reacted for 2.5 hours to obtain solution II;

[0037] S3: 3 parts of polyethylene glycol are dissolved in 20 parts of toluene to form a uniform solution, and then 1 part of maleic anhydride is added, and 0.1 part of benzoyl peroxide is slowly added under stirring at 600 rpm, and the mixture is heated to 65 degrees Celsius. The reaction conditions are maintained until all raw material components are fully reacted for 4 hours to obtain solution III;

[0038] S4: Mix solution II and solution III under stirring conditions at 600 rpm, slowly add 4 parts of nano-silicon dioxide, maintain the stirring conditions for 20 minutes, heat and dry the obtained product to obtain a product, and grind the obtained product to obtain the maleic anhydride grafted polymer fluid loss reducer.

[0039] Example 3

[0040] A maleic anhydride grafted polymer fluid loss reducer is prepared from the following raw materials in parts by weight: 8 parts of maleic anhydride, 3 parts of polyethylene glycol, 50 parts of lignin, 30 parts of polar wax, 5 parts of nano silicon dioxide, 1 part of benzoyl peroxide and 190 parts of toluene.

[0041] The maleic anhydride grafted polymer fluid loss reducer also includes the following preparation process:

[0042] S1: 50 parts of lignin and 30 parts of polar wax are dissolved or dispersed in 170 parts of toluene solvent to form a uniform solution or suspension, 0.9 parts of benzoyl peroxide are slowly added under stirring conditions at 600 rpm, and the reaction mixture is heated to 80 degrees Celsius, and the reaction conditions are maintained until all raw material components are fully reacted for 4 hours to obtain solution I;

[0043] S2: Add 6 parts of maleic anhydride to solution I, adjust the reaction temperature to 65 degrees Celsius, maintain the stirring speed at 600 rpm, and maintain the reaction conditions until all raw material components are fully reacted for 2.5 hours to obtain solution II;

[0044] S3: 3 parts of polyethylene glycol were dissolved in 20 parts of water to form a uniform solution, and then 2 parts of maleic anhydride were added, and 0.1 parts of benzoyl peroxide were slowly added under stirring conditions at 600 rpm, and the mixture was heated to 65 degrees Celsius. The reaction conditions were maintained until the raw material components were fully reacted for 4 hours to obtain solution III;

[0045] S4: Mix solution II and solution III under stirring at 600 rpm, slowly add 5 parts of nano-silicon dioxide, maintain the stirring condition for 20 minutes, heat and dry the obtained product, and crush it to obtain the maleic anhydride grafted polymer fluid loss reducer.

[0046] Example 4

[0047] A maleic anhydride grafted polymer fluid loss reducer is prepared from the following raw materials in parts by weight: 6 parts of maleic anhydride, 2 parts of polyethylene glycol, 40 parts of lignin, 30 parts of polar wax, 2 parts of nano silicon dioxide, 0.9 parts of benzoyl peroxide and 180 parts of toluene.

[0048] The maleic anhydride grafted polymer fluid loss reducer also includes the following preparation process:

[0049] S1: 40 parts of lignin and 30 parts of polar wax are dissolved or dispersed in 160 parts of toluene solvent to form a uniform solution or suspension, 0.8 parts of benzoyl peroxide are slowly added under stirring conditions at 600 rpm, and the reaction mixture is heated to 80 degrees Celsius, and the reaction conditions are maintained until all raw material components are fully reacted for 4 hours to obtain solution I;

[0050] S2: Add 5 parts of maleic anhydride to solution I, adjust the reaction temperature to 65 degrees Celsius, maintain the stirring speed at 600 rpm, and maintain the reaction conditions until all raw material components are fully reacted for 2.5 hours to obtain solution II;

[0051] S3: 2 parts of polyethylene glycol are dissolved in 20 parts of toluene solvent to form a uniform solution, and then 1 part of maleic anhydride is added, and 0.1 part of benzoyl peroxide is slowly added under stirring conditions at 600 rpm, and the mixture is heated to 65 degrees Celsius, and the reaction conditions are maintained until all raw material components are fully reacted for 4 hours to obtain solution III;

[0052] S4: Mix solution II and solution III under stirring at 600 rpm, slowly add 2 parts of nano-silicon dioxide, maintain the stirring condition for 20 minutes, heat and dry the obtained product, and crush it to obtain the maleic anhydride grafted polymer fluid loss reducer.

[0053] Example 5

[0054] A maleic anhydride grafted polymer fluid loss reducer is prepared from the following raw materials in parts by weight: 5 parts of maleic anhydride, 3 parts of polyethylene glycol, 30 parts of lignin, 25 parts of polar wax, 3 parts of nano silicon dioxide, 0.7 parts of benzoyl peroxide and 170 parts of toluene.

[0055] The maleic anhydride grafted polymer fluid loss reducer also includes the following preparation process:

[0056] S1: 30 parts of lignin and 25 parts of polar wax are dissolved or dispersed in 150 parts of toluene solvent to form a uniform solution or suspension, 0.6 parts of benzoyl peroxide are slowly added under stirring conditions at 600 rpm, and the reaction mixture is heated to 80 degrees Celsius, and the reaction conditions are maintained until all raw material components are fully reacted for 4 hours to obtain solution I;

[0057] S2: Add 4 parts of maleic anhydride to solution I, adjust the reaction temperature to 65 degrees Celsius, maintain the stirring speed at 600 rpm, and maintain the reaction conditions until all raw material components are fully reacted for 2.5 hours to obtain solution II;

[0058] S3: 3 parts of polyethylene glycol are dissolved in 20 parts of toluene solvent to form a uniform solution, and then 1 part of maleic anhydride is added, and 0.1 part of benzoyl peroxide is slowly added under stirring conditions at 600 rpm, and the mixture is heated to 65 degrees Celsius, and the reaction conditions are maintained until all raw material components are fully reacted for 4 hours to obtain solution III;

[0059] S4: Mix solution II and solution III under stirring conditions at 600 rpm, slowly add 3 parts of nano-silicon dioxide, maintain the stirring conditions for 20 minutes, heat and dry the obtained product, and crush it to obtain the maleic anhydride grafted polymer filtrate reducer.

[0060] Comparative Example 1 is composed of the following formula: 7 parts of maleic anhydride, 3 parts of polyethylene glycol, 35 parts of lignin, 4 parts of nano-silicon dioxide, 0.9 parts of benzoyl peroxide and 180 parts of toluene.

[0061] Comparative Example 1 was prepared by the following preparation process:

[0062] S1: 35 parts of lignin and 6 parts of maleic anhydride are dissolved or dispersed in 160 parts of toluene solvent to form a uniform solution or suspension, 0.8 parts of benzoyl peroxide are slowly added under stirring conditions at 600 rpm, and the reaction mixture is heated to 75 degrees Celsius, and the reaction conditions are maintained until the raw material components are fully reacted for 2.5 hours to obtain solution I;

[0063] S2: 3 parts of polyethylene glycol are dissolved in 20 parts of toluene solvent to form a uniform solution, and then 1 part of maleic anhydride is added, and 0.1 part of benzoyl peroxide is slowly added under stirring conditions of 600 rpm, and the mixture is heated to 65 degrees Celsius, and the reaction conditions are maintained until all raw material components are fully reacted for 4 hours to obtain solution II;

[0064] S3: Mix solution I and solution II under stirring at 600 rpm, slowly add 4 parts of nano-silicon dioxide, maintain the stirring condition for 20 minutes, heat and dry the obtained product, and crush it to obtain the filtrate reducer of Comparative Example 1.

[0065] Comparative Example 2 is composed of the following formula: 7 parts of maleic anhydride, 3 parts of polyethylene glycol, 35 parts of polar wax, 4 parts of nano silicon dioxide, 0.9 parts of benzoyl peroxide and 180 parts of toluene.

[0066] Comparative Example 2 was prepared by the following preparation process:

[0067] S1: 35 parts of polar wax and 6 parts of maleic anhydride are dissolved or dispersed in 160 parts of toluene solvent to form a uniform solution or suspension, 0.8 parts of benzoyl peroxide are slowly added under stirring at 600 rpm, and the reaction mixture is heated to 80 degrees Celsius, and the reaction conditions are maintained until the raw material components are fully reacted for 2.5 hours to obtain solution I;

[0068] S2: 3 parts of polyethylene glycol are dissolved in 20 parts of toluene solvent to form a uniform solution, and then 1 part of maleic anhydride is added, and 0.1 part of benzoyl peroxide is slowly added under stirring conditions of 600 rpm, and the mixture is heated to 65 degrees Celsius, and the reaction conditions are maintained until all raw material components are fully reacted for 4 hours to obtain solution II;

[0069] S3: Mix solution I and solution II under stirring at 600 rpm, and slowly add 4 parts of nano-silicon dioxide, maintain the stirring condition for 20 minutes, and heat and dry the obtained product to obtain a product, and crush it to obtain the filtrate reducer of Comparative Example 2.

[0070] Comparative Example 3 is composed of the following formula: 7 parts of maleic anhydride, 3 parts of polyethylene glycol, 35 parts of lignin, 5 parts of polar wax, 4 parts of nano-silicon dioxide, 0.9 parts of benzoyl peroxide and 180 parts of toluene.

[0071] The preparation steps are basically the same as those of the embodiments (the difference is that the proportions of each component in the steps are adjusted accordingly).

[0072] Comparative Example 4 is composed of the following formula: 7 parts of maleic anhydride, 3 parts of polyethylene glycol, 35 parts of lignin, 50 parts of polar wax, 4 parts of nano-silicon dioxide, 0.9 parts of benzoyl peroxide and 180 parts of toluene.

[0073] The preparation steps are basically the same as those of the embodiments (the difference is that the proportions of each component in the steps are adjusted accordingly).

[0074] Performance Testing:

[0075] Multi-index performance tests were performed on each embodiment, and the indicators included filtration rate (mL / 30min), viscosity (cP), filter cake thickness (mm), thermal stability (°C), sedimentation (%), suspension (%) and pH value. The following is a description of several test methods and means: Index 1, filtration rate (mL / 30min), using API filtration tester. The drilling fluid sample was placed in the filtration tester, filtered at standard pressure (usually 100 psi) for 30 minutes, and the collected filtrate volume was measured in mL. The filtration rate reflects the filtration control ability of the drilling fluid, and the lower the value, the better. Index 2, viscosity (cP), using a rotational viscometer (such as Fann 35A). The viscosity of the drilling fluid was measured at a specified shear rate in centipoise (cP). Through the viscosity data at different rotation speeds, the rheological properties of the drilling fluid can be understood, which affects its pumping performance and fluid control. Index 3, filter cake thickness (mm), measured by API filtration test. After the filtration test is completed, open the filter loss meter and measure the thickness of the filter cake in millimeters (mm). The filter cake thickness reflects the density of the barrier layer formed by the drilling fluid on the surface of the formation. Indicator 4, thermal stability (°C), thermal aging test, the drilling fluid sample is placed in a high-temperature autoclave, aged at a specific temperature for several hours, and then its performance changes are measured. Based on the initial filtration loss, and the performance reduction threshold (proportional value) is set, the gradient heat is repeated from 160°C to reduce the temperature by 10°C once, and the threshold temperature interval is measured and then the test is reduced by 2°C, and then the interval is measured and the test is reduced by 1°C until the specific temperature threshold is measured. The thermal stability test is designed to evaluate the stability and performance retention of the drilling fluid under high temperature conditions. Indicator 5, sedimentation (%), static sedimentation test, the drilling fluid sample is left to stand for a period of time (usually 24 hours), and then the sedimentation of solid particles is measured, and the sedimentation rate is calculated, expressed as a percentage (%). Sedimentation reflects the stability of solid particles in the drilling fluid, and the lower the value, the better. Indicator 6, Suspension (%), dynamic suspension test, measures the degree of suspension of solid particles in drilling fluid under stirring conditions, usually by visual inspection or particle size analyzer to measure the volume fraction of suspended particles and expressed as a percentage (%). Suspension reflects the dispersion stability of solid particles in drilling fluid, the higher the value, the better. Indicator 7, pH value, pH meter measurement, use a calibrated pH meter to directly measure the pH value of the drilling fluid sample. The pH value affects the chemical stability of the drilling fluid and its compatibility with the formation rock, and is usually ideal in the neutral to slightly alkaline range (about 7.0-9.5).

[0076] Table 1 is the performance test results of each embodiment:

[0077]

[0078] From the data in Table 1, the performance of the fluid loss reducers of each embodiment in different base fluids can be analyzed. The oil-based fluid loss rates of Examples 1-5 are all lower than the water-based fluid loss rates, indicating that these fluid loss reducers perform better in oil-based environments, effectively reducing the amount of fluid loss, thereby reducing the invasion of formation fluids and drilling fluid losses. In oil-based and water-based environments, the viscosity of these fluid loss reducers remains within an appropriate range (35-45 cP), which indicates that the fluid loss reducers can work effectively without significantly increasing the viscosity of the drilling fluid, thereby maintaining good drilling fluid fluidity and carrying capacity. The filter cake thickness formed by the fluid loss reducers of each embodiment in oil-based and water-based environments is relatively thin (1.1-1.4 mm), indicating that the filter cake has good compactness, can effectively prevent the penetration of formation fluids, and reduces the damage to the well wall. The thermal stability of the fluid loss reducers of each embodiment in an oil-based environment is high (above 100°C), which indicates that these fluid loss reducers can still maintain stable performance under high temperature conditions, will not decompose or fail due to high temperature, and are therefore suitable for high-temperature downhole environments. The sedimentation of the fluid loss reducers in the oil-based and water-based drilling fluids is very low (0.2-0.4%), which indicates that the fluid loss reducers can well maintain the uniformity of the drilling fluid, prevent the sedimentation of solid particles, and thus maintain the suspension and fluidity of the drilling fluid. The fluid loss reducers in the embodiments show high suspension (96.5%-98.3%) in both oil-based and water-based environments, which means that the fluid loss reducers can effectively maintain the suspension state of solid particles in the drilling fluid, enhance the sand carrying capacity of the drilling fluid, and reduce the sand settling problem in the wellbore. The pH value of each embodiment is moderate (8.0-8.6), indicating that these fluid loss reducers can work stably under neutral to slightly alkaline conditions, reduce the risk of corrosion to drilling equipment and well walls, and help maintain the chemical stability of the drilling fluid. Experimental data show that the fluid loss reducers in the embodiments show lower filtration rate, higher thermal stability and better suspension in both oil-based and water-based, showing their excellent performance in oil-based environments. These characteristics are particularly important for complex downhole environments with high temperature and high pressure. In addition, these fluid loss reducers also maintain good performance in water-based drilling fluids and have balanced performance in oil-based or water-based fluids, demonstrating their wide adaptability in different base fluids.

[0079] In addition, the performance of Comparative Examples 1-4 in oil-based and water-based is significantly different. Among them, the filtrate reducer of Comparative Example 1 performs poorly in oil-based and has a high filtration rate (27.1 mL / 30 min), indicating that it is difficult to effectively reduce the filtration loss in an oil-based environment, increasing the risk of formation fluid invasion. Although the filter cake thickness is thin (1.5 mm), other performance indicators, such as thermal stability and suspension, are poor (85.3%), resulting in its overall weak performance in an oil-based environment. In water-based, the filtrate reducer of Comparative Example 1 performs well, with a significantly reduced filtration rate (13.5 mL / 30 min), showing a good filtration loss reduction effect, and effectively reducing the filtration loss of water-based drilling fluid. Other performance indicators are also ideal, such as high suspension (97.5%) and thin filter cake (1.2 mm), all of which indicate that the filtrate reducer can maintain good performance in a water-based environment. The filtrate reducer of Comparative Example 2 performs well in the oil base, with a low filtration rate (9.5 mL / 30 min), effectively reducing the filtration loss of the oil-based drilling fluid, showing a good filtration loss reduction ability. Other properties such as filter cake thickness (1.3 mm) and suspension (96.6%) are also excellent, indicating that the filtrate reducer is stable and excellent in the oil-based environment. The filtrate reducer of Comparative Example 2 performs poorly in the water base, with a high filtration rate (21.4 mL / 30 min), indicating that it is not ideal in the water-based environment and cannot effectively reduce the filtration loss. The thick filter cake thickness (1.7 mm) and low suspension (87.1%) further illustrate that the comprehensive performance of the filtrate reducer in the water-based environment is poor. The filtrate reducer of Comparative Example 3 performs poorly in the oil base, with a high filtration rate (24.6 mL / 30 min), showing that the filtration loss in the oil-based environment is large and it is difficult to effectively control the filtration loss. Although the filter cake thickness is slightly thin (1.3 mm), the suspension is low (91.7%), the thermal stability is also insufficient, and the overall performance is poor. The filter loss reducer of Comparative Example 3 performs well in water-based, with a medium filter loss rate (13.7 mL / 30 min), which can reduce the filter loss to a certain extent, but the effect is not as good as that of Comparative Example 1. Other properties such as suspension (93.4%) and filter cake thickness (1.4 mm) perform well, indicating that the filter loss reducer can maintain relatively stable performance in a water-based environment. The filter loss reducer of Comparative Example 4 performs well in oil-based, with a medium filter loss rate (11.2 mL / 30 min), which can control the filter loss in an oil-based environment to a certain extent. Other properties such as filter cake thickness (1.3 mm) and suspension (89.2%) perform well, but fail to reach the optimal level, and the overall performance is slightly lower than that of Comparative Example 2. The filtrate reducer of Comparative Example 4 performed poorly in water-based environment, with a high filtration rate (19.6 mL / 30 min), and could not effectively control the filtration loss, resulting in poor filtration effect. The thick filter cake thickness (1.5 mm) and low suspension (87.8%) further indicate that the comprehensive performance of the filtrate reducer in water-based environment is poor.In summary, in combination with the preparation methods of the embodiments and comparative examples, comparative example 1 performs well in water-based, but performs poorly in oil-based. Compared with Example 1, it can be seen that the addition of polar wax helps the filtration performance of the filtrate reducer in the oil-based; comparative example 2 performs well in the oil-based, but performs poorly in the water-based. Compared with Example 1, it can be seen that the addition of lignin helps the filtration performance of the filtrate reducer in the water-based; comparative example 3 performs poorly in the oil-based, but is acceptable in the water-based. Compared with Example 1, it can be seen that there is too little polar wax and the performance of the filtrate reducer in the oil-based is poor; comparative example 4 performs well in the oil-based, but performs poorly in the water-based. Compared with Example 1, it can be seen that there is too much polar wax and the performance of the filtrate reducer in the water-based is poor.

[0080] It is worth noting that the materials grafted with lignin and maleic anhydride are more water-based. Lignin itself has a certain hydrophilicity, especially when it contains polyhydroxyl and aromatic groups. Maleic anhydride grafting will introduce more polar groups (such as carboxylic acid groups), further increasing the hydrophilicity of the material. Therefore, the materials grafted with lignin and maleic anhydride show better solubility and dispersibility in a water-based environment and are suitable for use in a water-based system. The materials grafted with lignin and polar wax are more oil-based. Polar waxes usually have long-chain hydrocarbon groups, which increase the hydrophobicity of the material and make it more stable in an oil-based environment. Although polar waxes have a certain polarity, after grafting with lignin, the hydrophobicity of the overall material is relatively high, which is suitable for use in an oil-based system. Therefore, the materials grafted with lignin and polar wax show better compatibility and stability in an oil-based environment and are suitable for use in an oil-based system. Therefore, the embodiment grafts polar wax with lignin, and then grafts maleic anhydride on this polymer, which can create a dual-purpose material with good performance in both oil-based and water-based environments. The long-chain hydrocarbon group of the polar wax increases the hydrophobicity of the material, making the grafted lignin more stable and easier to disperse in an oil-based environment. The polar part in the polar wax can interact with water to a certain extent, providing limited hydrophilicity. Maleic anhydride introduces a carboxylic acid group, which significantly improves the hydrophilicity and solubility of the material in water, and can also play a role in the oil base. Therefore, after maleic anhydride grafting, the material has both hydrophilicity and hydrophobicity, allowing it to perform well in both water-based and oil-based environments. This double-layer grafted structure can be used as an effective surfactant or surfactant. At the oil-water interface, the polar wax part can be compatible with the oil base, while the maleic anhydride part can be compatible with water, thereby stabilizing the oil-water interface and preventing phase separation. This property is very useful for applications such as emulsifiers and dispersants. Since the material can perform well in both oil-based and water-based, it has a wide range of applications. It can be used as a multifunctional additive (the polar wax in the embodiment uses oxidized polyethylene wax), suitable for oil-based and water-based drilling fluids, coatings, inks, drug delivery systems, etc. The introduction of polar wax enhances the stability of the material under high temperature and pressure, especially in oil-based environments. This allows the material to maintain its functionality under harsh conditions, while the hydrophilic groups of maleic anhydride ensure its durability and effectiveness in water-based environments. In oil-based drilling fluids, polar wax can effectively reduce fluid loss and improve filter cake quality, while maleic anhydride grafting can provide similar benefits in water-based drilling fluids. This dual grafting strategy improves both fluid loss control and rheological properties of the material in different base fluids.

[0081] The specific implementation methods described above further illustrate the objectives, technical solutions and beneficial effects of the present invention in detail. It should be understood that the above description is only a specific implementation method of the present invention and is not intended to limit the scope of protection of the present invention. Any modifications, equivalent substitutions, improvements, etc. made within the spirit and principles of the present invention should be included in the scope of protection of the present invention.

Claims

1. A maleic anhydride grafted polymer fluid loss reducer, characterized in that: The composition comprises the following components by weight: 5-8 parts of unsaturated acid anhydride, 2-3 parts of polyethylene glycol, 30-50 parts of lignin, 25-35 parts of polar wax, 2-5 parts of nano silicon dioxide, 0.7-1 parts of initiator and 170-190 parts of organic solvent; wherein the unsaturated acid anhydride is maleic anhydride; The maleic anhydride grafted polymer fluid loss reducer is prepared by the following process: S1: dissolving or dispersing lignin and polar wax in an organic solvent to form a uniform solution or suspension, slowly adding an initiator under stirring conditions, and heating the reaction mixture until all raw material components are fully reacted to obtain solution I; S2: adding unsaturated acid anhydride to solution I, adjusting the reaction temperature, maintaining the stirring speed, and waiting for all raw material components to fully react to obtain solution II; S3: dissolving polyethylene glycol in an organic solvent to form a uniform solution, then adding unsaturated acid anhydride, slowly adding an initiator under stirring, and heating the mixture until all raw material components are fully reacted to obtain solution III; S4: Mixing solution II and solution III under stirring conditions at 500-900 rpm, slowly adding nano-silicon dioxide, maintaining the stirring conditions for 10-30 minutes, and drying and crushing the obtained product to obtain the maleic anhydride grafted polymer fluid loss reducer.

2. A maleic anhydride grafted polymer fluid loss reducer as claimed in claim 1, characterized in that: The maleic anhydride grafted polymer fluid loss reducer uses benzoyl peroxide as an initiator and toluene as an organic solvent.

3. A maleic anhydride grafted polymer fluid loss reducer as claimed in claim 1, characterized in that: The weight ratio of polar wax to lignin is between 0.3 and 1.

4. A maleic anhydride grafted polymer fluid loss reducer as claimed in claim 1, characterized in that: The polar wax is a polar wax with a size of 500-3000 Daltons, and the lignin is a lignin with a size of 20000-50000 Daltons.

5. The maleic anhydride grafted polymer fluid loss reducer according to claim 1, characterized in that: The preparation temperature range of solution I is 80-90 degrees Celsius, the stirring speed is 500-900 rpm, and the reaction time is 3-6 hours; the reaction temperature range of solution II is 60-80 degrees Celsius, the stirring speed is 500-900 rpm, and the reaction time is 2-4 hours; the reaction temperature range of solution III is 60-80 degrees Celsius, the stirring speed is 500-900 rpm, and the reaction time is 3-5 hours.