Method for repairing slag line of slag pouring surface of 120-ton converter by adopting repairing material
By raising the slag dumping surface of the converter and sintering the repair material, the problem of thinning of the lining at the slag line on the slag dumping surface is solved, a more balanced lining thickness and higher corrosion resistance are achieved, and the service life of the converter is extended. and reduce costs.
Patent Information
- Application Number
- CN202410861912.1
- Authority / Receiving Office
- CN · China
- Patent Type
- Applications(China)
- Current Assignee / Owner
- Filing Date
- 2024-06-28
- Publication Date
- 2024-10-11
AI Technical Summary
During the production process of the top-bottom combined blowing converter, the slag line on the slag pouring surface is corroded by high-temperature molten steel and highly oxidizing slag, resulting in thinning of the furnace lining. There are maintenance requirements such as slag splashing to protect the furnace, dry and wet gunning methods, and refractory brick patching. This method has the problems of high cost, high labor intensity, non-uniformity and safety risks. It is difficult for the existing method to effectively solve the actual situation of thin furnace lining thickness at the slag line on the slag pouring surface.
Use pig iron or repairing sand to raise the middle area of the slag dumping surface of the converter, change the relative height of the slag line, and add an appropriate amount of repairing material according to the degree of erosion for sintering, control the thickness of the slag line, and improve its Corrosion resistance.
It achieves balanced maintenance of the slag line on the slag pouring surface, increases the service life of the furnace lining, reduces production costs, avoids furnace leakage accidents, extends the economic life of the converter, and reduces manufacturing costs.
Smart Images

Figure CN118755901A_ABST
Abstract
Description
Technical Field
[0001] The invention belongs to the technical field of steel smelting, and in particular relates to a method for filling a slag line on a slag pouring surface of a 120-ton converter by using supplementary furnace charge. Background Art
[0002] During the production process of the top and bottom double-blown converter, the lining is affected by factors such as high-temperature molten steel, converter slag and oxidizing gases, rapid cooling and heating of the furnace temperature, and mechanical impact, which causes the lining refractory to be eroded, damaged and thinned; when the converter lining becomes thinner, the molten steel is easy to melt through and leak furnace accidents occur. On the contrary, the thicker the working lining of the converter, the longer and safer it is. When the converter smelting reaches the end point, the conventional operation will swing the converter to a certain angle (+76°~+86°) to the slag pouring surface for temperature measurement, sampling or slag discharge. Under the joint erosion of high-temperature molten steel and highly oxidizing slag, as the age of the furnace increases, two arc-shaped areas with faster erosion (usually called slag lines on the slag pouring surface) are formed on the left and right sides of the slag pouring surface below the furnace cap. This part becomes a weak point for the safe use of the lining and is one of the parts of the converter lining that need to be maintained. In view of the problem of rapid erosion of the slag line on the slag pouring surface, in actual production, the following methods can be used to maintain the slag line on the slag pouring surface: 1. Slag splashing protection: The slag line is covered and soaked by high-temperature, highly oxidizing molten slag during slag pouring and temperature measurement sampling, which causes the lining erosion rate to be much more serious than other parts. Especially when the converter is operating with less slag and low iron-steel ratio, due to the small amount of splashing slag and the strong oxidation of the final slag, the slag phase has a low melting point. Splashing protection alone can no longer meet the requirements of the thickness of the slag splashing layer and the corrosion resistance of the converter lining. 2. Dry and wet gunning method: There are problems such as high cost of raw materials, increased labor intensity, chilled furnace lining, uneven gunning position, non-bonding of gunning materials, thin gunning layer, and gunning materials are not resistant to corrosion. 3. Refractory brick patching: Due to the long converter body, heavy refractory bricks, high working environment temperature, high labor intensity, large patching gaps and poor adhesion, the refractory brick patching method cannot be operated normally. This method of slag patching is rarely used in actual production. 4. The method of using refractory materials to fill the slag line: The staff needs to stand in the scrap steel bucket and throw the refractory materials to the slag line by hand. This is an operation in a high-altitude and high-temperature environment, which poses a safety risk. In addition, due to factors such as the instability of manual input, this method of filling the slag line is rarely used in actual production.
[0003] After long-term practice summary, in actual production, the slag line of the slag pouring surface is generally maintained by combining slag splashing protection with dry and wet gunning, but it still fails to effectively solve the actual situation that the thickness of the lining at the slag line is relatively thin. Therefore, it is particularly necessary to study a reliable method for maintaining the lining at the slag line of the 120-ton converter slag pouring surface. Summary of the invention
[0004] The object of the present invention is to provide a method for filling the slag line of the slag pouring surface of a 120-ton converter by using supplementary charge.
[0005] The object of the present invention is achieved in this way. A method for using supplementary furnace charge to fill the slag line of the slag pouring surface of a 120-ton converter is to use pig iron or supplementary furnace sand to fill the middle large surface area of the converter slag pouring surface to control the relative height between the slag line area and the slag pouring surface, and then according to the degree of erosion of the slag line area of the slag pouring surface, an appropriate amount of supplementary furnace charge is added for filling and sintering.
[0006] When the existing furnace protection means are used for the slag pouring surface of the converter, the relative heights of the slag lines on both sides of the slag pouring surface are higher than other parts, that is, the slag lines on both sides are high, and the middle large surface is low. The furnace protection materials will fall down under the action of gravity during maintenance, and cannot play a good furnace protection role, causing the slag line parts of the slag pouring surface to form weak points in the working of the converter lining, failing to meet the requirements of balanced lining, and restricting the improvement of furnace life. In order to solve the problem of high relative heights of the slag lines on both sides of the slag pouring surface and difficulty in maintenance, the present invention uses pig iron or other refractory materials to raise the middle large surface of the converter slag pouring surface, and the slag lines on both sides become relatively low. Then, according to the degree of erosion of the slag line parts of the slag pouring surface, an appropriate amount of filling materials are added for spreading and sintering, thereby meeting the process requirements of controlling the thickness of the working lining at the slag line parts of the slag pouring surface, improving the corrosion resistance of the slag line parts, and realizing balanced operation of the working lining of the converter.
[0007] The present invention changes the height of the slag line of the slag pouring surface according to the degree of erosion of the large surface of the slag pouring surface or the thickness of the slag line that needs to be patched. When the slag line of the slag pouring surface needs to be patched with patching charge, pig iron or furnace sand is normally added to maintain the slag surface molten pool / furnace body / furnace cap. When the inclination angle of the converter is shaken to 80-125° in front of the furnace, it can meet the requirement that the middle part of the converter slag pouring surface is high and the slag lines on both sides are low. At this time, the patching charge can only flow from the high middle part of the slag pouring surface to the low part of the slag line. The height can be regulated according to the required patching thickness. After the slag line height is determined, the patching charge is added for patching and sintered for a certain time, thereby realizing normal maintenance of the two slag lines, increasing the thickness of the slag line and improving the corrosion resistance.
[0008] The present invention changes the relative height of the slag line of the slag pouring surface by padding the height of the large surface of the slag pouring surface, so that the large surface in the middle of the slag pouring surface is high and the slag line parts on both sides are low, and the slag line parts are changed from a high position to a low position, and then the weak points of the lining at the slag line of the slag pouring surface are patched with furnace charge to thicken the weak points of the lining, thereby meeting the process requirement of controlling the thickness of the working lining at the slag line of the slag pouring surface, avoiding leakage accidents at the slag line part, realizing balanced operation of the working lining of the converter, effectively improving the economic life of the converter, and reducing the manufacturing cost.
[0009] The beneficial effects of the present invention are: 1. The method of the present invention can control the thickness of the slag line of the slag pouring surface more conveniently and flexibly, can better maintain the slag line of the slag pouring surface, ensure the balanced operation of the working lining of the converter, and thus increase the service life of the lining.
[0010] 2. When the slag line cannot be repaired due to special reasons, the method of the present invention can completely replace the dry and wet methods of repairing the slag line, thereby ensuring the stable and smooth operation of the furnace condition, and can also increase the thickness of the slag line on the slag pouring surface, thereby reducing production costs.
[0011] 3. The method of the present invention is simple and reliable, easy to promote and apply, and can also make up for other weak points of the slag pouring surface when spreading the slag line, providing technical support for the maintenance of the converter slag line. BRIEF DESCRIPTION OF THE DRAWINGS
[0012] Figure 1 The actual erosion of the lining at the slag line of the converter slag pouring surface before the use of supplementary materials; Figure 2 This is a picture showing that the erosion degree of the lining at the slag line of the converter pouring surface has been significantly improved after the slag line was filled with supplementary materials; Figure 3 This is a picture showing that the erosion of the lining at the slag line of the converter pouring surface has been effectively controlled after the slag line is filled with filler material; Figure 4 This is a site view of the 120t converter in Example 1 when the slag line of the slag pouring surface is filled with filler material and the slag line of the molten pool and the furnace body; Figure 5 This is a diagram of dismantling a 120t converter in Example 1 when the slag line of the slag pouring surface is filled with supplementary charge and the furnace age reaches 12197 heats; Figure 6 This is a site photo of the 120t converter in Example 1 when using supplementary charge to fill the slag line of the slag pouring surface molten pool. DETAILED DESCRIPTION
[0013] The present invention is further described below in conjunction with the embodiments, but the present invention is not limited in any way. Any changes or substitutions made based on the teachings of the present invention belong to the protection scope of the present invention.
[0014] The present invention adopts a method for filling the slag line of the slag pouring surface with supplementary furnace charge. Pig iron or supplementary furnace sand is used to fill the middle large surface area of the converter slag pouring surface to control the relative height between the slag line area and the slag pouring surface. Then, according to the erosion degree of the slag line area of the slag pouring surface, an appropriate amount of supplementary furnace charge is added for filling and sintering.
[0015] Among them, the specific method of using pig iron to pad the slag surface is as follows: after the steel is tapped, 2 to 3 tons of pig iron are used to pad the slag surface, and the soaking time is ≥1min. After the next furnace is tapped, the furnace is shaken to 85° for the slag surface and soaked for ≥120s.
[0016] The amount of pig iron used is about 2t and cannot exceed 3t; the C content of the final slag of the supplementary furnace converter needs to be controlled at 0.06%~0.10%; the final temperature needs to be less than 1670℃; the binary basicity is controlled at 2.8~3.5; the amount of slag retained should be greater than 4t.
[0017] When using pig iron to pad the slag surface, the converter angle should be shaken to 60°~65° when padding the furnace cap area, and the converter angle should be shaken to 53°~58° when padding the scrap steel impact area and below; when the pig iron for filling the furnace is poured into the furnace, the converter should be shaken down until all the pig iron is covered with slag, and soaked for about 1 minute before the splashing slag can be shaken up. After the pig iron padding is completed for the second furnace, the slag should not be splashed too dry into particles, and should have appropriate fluidity. After the slag splashing is completed, the gun should be lifted and the converter should be shaken down to cover the slag on the surface of the pig iron. After confirming that the conditions for entering the furnace are met, molten iron and scrap steel can be added.
[0018] After the pig iron is used to pad the slag surface, after each batch of steel is produced, the converter is directly shaken to 85°~90° towards the slag surface without splashing slag. After soaking for about 20 seconds, shake off the splashing slag. If seasoning is needed, appropriate material can be added to adjust the slag system.
[0019] When using pig iron to pad the slag surface, if there are pits at the bottom of the furnace, pig iron is needed to pad the bottom of the furnace to match the slag surface, and pig iron can be directly added after steel is discharged. After adding, shake the converter backward to 50°, then shake it straight, and leave it for about 1 minute to lower the gun to splash slag. The lowest gun position for slag splashing is not less than 1 meter. If there is no rush to enter the furnace for blowing after the slag splashing is over, it can be left still first, and when it is needed, shake the furnace back and forth to confirm before entering.
[0020] The specific method of using the filling furnace sand to fill the slag surface is as follows: 1.6 to 4 tons of filling furnace sand is used to fill the slag surface, and the sintering time is 40 to 120 minutes; When the amount of supplementary furnace sand is 1.6-2.4 tons, the sintering time is 40 to 60 minutes; when the amount of supplementary furnace sand is 2.4 to 3.2 tons, the sintering time is 60 to 90 minutes; when the amount of supplementary furnace sand is 3.2 to 4 tons, the sintering time is 90 to 120 minutes.
[0021] When using furnace sand to pad the slag surface, the scrap steel in the furnace must be melted completely. The furnace seat of the furnace must be completed within 10 minutes from the completion of steel output to the spreading of the furnace sand. After the furnace sand is spread, oxygen-assisted heating must be used in time.
[0022] According to the erosion position of the slag line on the slag pouring surface, the depth of the slag line is controlled, and an appropriate amount of supplementary charge and a furnace shaking angle are added to spread it; when the erosion position is close to the molten pool, the amount of supplementary charge is less and the furnace shaking angle is 115°-120°; when the erosion position is close to the furnace cap, the amount of supplementary charge is more and the furnace shaking angle is 120°-125°.
[0023] The present invention will be further described below by taking a 120t E# converter in an operating area of Kunming Iron and Steel Plant as an example.
[0024] Example 1 In production, when it is necessary to use supplementary furnace materials to fill the slag line of the slag pouring surface, according to the erosion of the converter slag pouring surface and the shutdown time of the converter, it is determined to use pig iron or supplementary furnace sand to fill the middle large surface of the converter slag pouring surface to control the relative height between the slag line and the slag pouring surface. Then, according to the erosion degree of the slag line of the slag pouring surface, add appropriate amount of supplementary furnace materials for filling and sintering, so as to increase the thickness of the furnace lining at the slag line of the slag pouring surface.
[0025] 1. When the shutdown time is short and the large area of the slag pouring surface is not seriously eroded, pig iron is used to fill the middle large area of the converter slag pouring surface to control the relative height between the slag line and the slag pouring surface.
[0026] The specific method of using pig iron to pad the slag surface is as follows: after the steel is tapped, use 2 to 3 tons of pig iron to pad the slag surface, the soaking time is ≥1min, and after the next furnace is tapped, shake the furnace until the slag surface is 85° and soak for ≥120s.
[0027] When using pig iron to fill the slag surface to control the relative height of the slag line, the following points should be noted: 1. The amount of pig iron used should not be too much, about 2 tons is appropriate, and no more than 3 tons. Self-produced cast iron or bar rolling heads are preferred for furnace replenishment.
[0028] 2. The final slag of the converter must meet the following conditions: (1) The final C content must be between 0.06% and 0.10%; (2) The final temperature must be less than 1670°C; (3) The binary basicity must be between 2.8 and 3.5; (4) The amount of slag left should be greater than 4 tons.
[0029] 3. When pig iron is used to pad the slag surface, the furnace master shall, according to the actual situation of the slag surface and the slag accumulation at the bottom of the furnace during the shift, shake the converter angle to 60°~65° when padding the furnace cap area, and shake the converter angle to 53°~58° when padding the scrap steel impact area and the position below. When the pig iron for the furnace is poured into the furnace, the converter is shaken down until all the pig iron is covered with slag, and soaked for about 1 minute before the splashing slag can be shaken up. After the pig iron padding is completed for the second furnace, the slag cannot be splashed too dry into particles when splashing, and it should have appropriate fluidity. After the slag splashing is completed, the furnace master will command the converter to shake down to cover the slag on the surface of the pig iron. Only after confirming that the conditions for entering the furnace are met can molten iron and scrap steel be added. If the conditions for entering the furnace are not met, corresponding measures should be taken (adding materials, shaking the furnace or splashing slag again).
[0030] 4. After the pig iron pad is used to fill the slag surface, after each batch of steel is produced, shake the converter directly to the slag surface to an angle of 85°~90° without splashing slag. Soak it for about 20 seconds and then shake it to splash slag. If seasoning is needed, add appropriate amount of material to adjust the slag system.
[0031] 5. If there are pits at the bottom of the furnace and pig iron is needed to pad the bottom of the furnace to match the slag pouring surface, add pig iron directly after tapping the steel. After adding, shake the converter backward to 50°, then shake it straight, leave it for about 1 minute, and then lower the gun to splash the slag. The lowest gun position for slag splashing should not be lower than 1 meter. After the slag splashing is over, if you are not in a hurry to enter the furnace for blowing, you can leave it still and shake the furnace back and forth to confirm when you need to enter the furnace.
[0032] Pig iron resources are abundant. After melting, it becomes molten steel. The slag surface protection of the furnace is effective quickly and takes a short time, only 3-5 minutes. However, it is greatly affected by the operation level of the furnace master and the quality of the pig iron pad. After melting, it affects the uniformity of the molten steel, and its corrosion resistance is weaker than that of the furnace sand protection. Therefore, a high frequency of furnace protection is required.
[0033] 2. When the furnace is shut down for a long time and the large area of the slag pouring surface is severely eroded, the converter is repaired with furnace sand pads. The middle large surface of the slag pouring surface is used to control the relative height between the slag line and the slag pouring surface. It takes a long time to pad the middle large surface of the slag pouring surface with filling sand, which can be completed in 40-120 minutes. The efficiency is low. It takes a long time to pad the middle large surface of the slag pouring surface, and then add filling materials to sinter the slag line of the slag pouring surface. However, the filling sand used to pad the middle large surface of the slag pouring surface is resistant to the erosion of high-temperature molten steel and high-oxidation slag, and is not easy to fall off, which is conducive to improving the corrosion resistance of the filling materials spread at the slag line of the slag pouring surface. In actual production, the shutdown time is more than 40 minutes, and the large surface of the slag pouring surface is generally padded with filling sand. If the height of the large surface of the slag pouring surface meets the filling slag line, the filling materials are generally used to fill the slag line of the slag pouring surface.
[0034] The specific method of using furnace sand to pad the slag surface is as follows: use 1.6 to 4 tons of furnace sand to pad the slag surface, and the sintering time is 40 to 120 minutes.
[0035] When using furnace sand to fill the slag surface to control the relative height of the slag line, the following points should be noted: 1. The supervisor shall carry out converter maintenance according to the issued furnace repair plan, and those that are not completed shall be assessed according to relevant management regulations; 2. The furnace seat for the repair must be notified to the converter furnace master two furnaces of steel before the repair (especially the furnace seat for over-refining). The converter furnace master should keep the scrap steel in good heat balance to ensure that the scrap steel in the furnace is melted completely when the repair is made; 3. The furnace seat of the repair furnace must be completed within 10 minutes from the completion of steel production to the spreading of the repair furnace sand; the oxygen hose must be prepared in advance, and oxygen auxiliary heating should be used in time after the repair furnace sand is spread; 4. When the amount of supplementary sand is 1.6-2.4 tons, the sintering time is 40-60 minutes; when the amount of supplementary sand is 2.4-3.2 tons, the sintering time is 60-90 minutes; when the amount of supplementary sand is 3.2-4 tons, the sintering time is 90-120 minutes. (From the start of supplementary sand to the lower gun blowing is one supplementary furnace time, the furnace master is responsible); 5. During the first to third batches of steel, one of the shift supervisors and deputy supervisors must be on site to monitor safety and prevent people from crossing on both sides. The furnace shaker wears protective clothing and positions the ladle in advance. During the steel-out process, the small observation door is closed. The furnace shaker controls the angle of the furnace according to the rhythm of the steel-out time, and drives the ladle car according to the command of the furnace master. The furnace master wears protective clothing and observes the steel-out process at the front door of the furnace, and closes the slide plate.
[0036] The furnace sand repair and furnace protection uses magnesium carbon refractory materials, which requires high temperature and other conditions. The furnace protection time is relatively long, about 2 hours, but the corrosion resistance is better. Therefore, combining the advantages and disadvantages of the two, we use pig iron to maintain the slag pouring surface according to the actual situation during the production process to prevent the furnace condition of the slag pouring surface from deteriorating; if the furnace condition is seriously eroded and the converter can meet a longer maintenance time, we will use the furnace sand repair and furnace protection; finally, the ideal relative height of the slag line is achieved.
[0037] 3. According to the erosion position of the slag line on the slag pouring surface, control the depth of the slag line, add appropriate amount of supplementary materials and the angle of the furnace for supplementary materials ( Figure 4 and Figure 6 ); When the erosion position is close to the molten pool, the amount of supplementary charge is less and the furnace shaking angle is 115°-120°; when the erosion position is close to the furnace cap, the amount of supplementary charge is more and the furnace shaking angle is 120°-125°.
[0038] Figure 1-3It is the actual plane cross-sectional view of the lining laser thickness gauge, indicating the lining thickness of the converter when it is upright; the thinner the lining thickness, the more serious the lining erosion is, and the more likely the risk of steel leakage during operation is; conversely, the thicker the lining is, the less erosion is, and the safer the working lining is; the colors of the thickness of the converter working lining from thick to thin are: blue→light green→green→yellow→orange→red. The horizontal axis represents the converter angle, and the vertical axis represents the converter depth, among which, A: 0° line represents the center line of the steel-outlet surface, -180° and 180 degrees are overlapping lines, representing the center line of the slag pouring surface; -90° is the left ear axis, and 90° is the right ear axis; -90°~90° is the steel-outlet surface, -90°~-180° is the left slag pouring surface, and 90°~180° is the right slag pouring surface; B: 0~2.2m is the converter cap, 2.2~6.7m is the furnace body, and 6.7~8m is the furnace bottom; C: -45° is the left slag line of the steel-outlet surface, 45° is the right slag line of the steel-outlet surface, -135° is the left slag line of the slag pouring surface, and 135° is the right slag line of the slag pouring surface.
[0039] In this embodiment, it can be seen from the actual erosion of the lining before the slag line of the converter slag pouring surface is filled with supplementary materials ( Figure 1 ), the four slag lines of the converter all show orange → red areas, indicating that the erosion is relatively serious. The slag line on the left side of the steel tapping surface is 0.414~0.502m, the slag line on the right side of the steel tapping surface is 0.448~0.515m, the slag line on the left side of the slag pouring surface is 0.432~0.498m, and the slag line on the right side of the slag pouring surface is 0.446~0.499m. The thinnest thickness of the lining at the east slag line is 0.38252m, and the color is red, which has entered the safety warning range of the converter leakage furnace; By changing the relative height of the slag line on the slag pouring surface and using the filling charge to fill the gap, the thickness of the slag line on the slag pouring surface increased significantly. The slag line on the left side of the steel tapping surface was 0.559-0.855m, the slag line on the right side of the steel tapping surface was 0.604-0.883m, the slag line on the left side of the slag pouring surface was 0.456-0.700m, the slag line on the right side of the slag pouring surface was 0.482-0.659m, and the thinnest part was 0.41487m ( Figure 2 ), the thickness of the thinnest part of the slag line on the slag pouring surface increased by 0.03235m, and the improvement effect was obvious.
[0040] After changing the relative height of the slag line on the slag pouring surface again, the slag line on the left side of the steel tapping surface is 0.635~0.991m, the slag line on the right side of the steel tapping surface is 0.683~0.993m, the slag line on the left side of the slag pouring surface is 0.564~0.765m, the slag line on the right side of the slag pouring surface is 0.574~0.1066m, and the thinnest part is 0.52766m ( Figure 3 ), the slag line position of the slag pouring surface is relative to Figure 2The thickness at the thinnest point increases by 0.11279m, relative to Figure 1 It increases by 0.14514m. It can be seen that the thickness of the slag line on the slag pouring surface increases, the furnace protection effect is obvious, the working lining runs evenly, and the furnace life can be controlled and improved.
[0041] After the method of the present invention was used to fill the slag line on the slag pouring surface, 338 furnace steel data were collected. The average thickness of the furnace lining increased by 17 cm, and the thickness of the corroded slag line increased by 14.5 cm. The corrosion resistance of the slag line was greatly improved, and the service life of the furnace lining was improved. Until the furnace age reached 12197 furnaces, there was no leakage accident in the converter, and the thickness of the remaining bricks at the slag line of the slag pouring surface was measured after the furnace was dismantled. About 20 cm ( Figure 5 ).
[0042] After adopting the method of the present invention for filling the slag surface and slag line, the slag surface and slag line lining of the converter are significantly improved, greatly improving the economic life of the converter, from the original 11,000 furnaces to 15,000 furnaces. The economic benefits are as follows: based on the masonry cost of each set of converter of 2.3 million yuan, the cost of each furnace of steel spread to the original furnace age is 209.09 yuan. After the furnace filling process method is changed, 4,000 furnaces can be added, and the actual economic benefits are: 2300000÷15000×(15000-11000)=613333.33 yuan The consumption of supplementary materials is reduced from 1.13kg / t to 0.83kg / t. The economic benefits are as follows: the supplementary materials are calculated at 3,000 yuan / t, and the average steel output is 117.3t / furnace, so the actual economic benefits are: 15000×117.3×(1.13-0.83)×3000÷1000=1583550 yuan The direct economic benefits totaled 2.197 million yuan, and the frequency of furnace refilling was greatly reduced, which not only reduced the labor intensity of employees, but also increased the converter operation rate and reduced safety hazards.
Claims
1. The 120-ton converter adopts the method of filling the slag line on the slag surface with supplementary charge. It is characterized in that The method comprises the following steps: using pig iron or furnace sand to fill the middle large surface of the converter slag pouring surface to control the relative height between the slag line and the slag pouring surface; and then adding a proper amount of furnace filler material for spreading and sintering according to the erosion degree of the slag line of the slag pouring surface.
2. The method according to claim 1, It is characterized in that in, The specific method of using pig iron to pad the slag surface is as follows: after the steel is tapped, use 2 to 3 tons of pig iron to pad the slag surface, the soaking time is ≥1min, and after the next furnace is tapped, shake the furnace until the slag surface is 85° and soak for ≥120s.
3. The method according to claim 2, It is characterized in that The amount of pig iron used is about 2t and cannot exceed 3t; the C content of the final slag of the supplementary furnace converter needs to be controlled at 0.06%~0.10%; the final temperature needs to be less than 1670℃; the binary basicity is controlled at 2.8~3.5; the amount of slag retained should be greater than 4t.
4. The method according to claim 2, It is characterized in that When using pig iron to pad the slag surface, the converter angle should be shaken to 60°~65° when padding the furnace cap area, and the converter angle should be shaken to 53°~58° when padding the scrap steel impact area and below; when the pig iron for filling the furnace is poured into the furnace, the converter should be shaken down until all the pig iron is covered with slag, and soaked for about 1 minute before the splashing slag can be shaken up. After the pig iron padding is completed for the second furnace, the slag should not be splashed too dry into particles, and should have appropriate fluidity. After the slag splashing is completed, the gun should be lifted and the converter should be shaken down to cover the slag on the surface of the pig iron. After confirming that the conditions for entering the furnace are met, molten iron and scrap steel can be added.
5. The method according to claim 2, It is characterized in that After the pig iron is used to pad the slag surface, after each batch of steel is produced, the converter is directly shaken to 85°~90° towards the slag surface without splashing slag. After soaking for about 20 seconds, shake off the splashing slag. If seasoning is needed, appropriate material can be added to adjust the slag system.
6. The method according to claim 2, It is characterized in that When using pig iron to pad the slag surface, if there are pits at the bottom of the furnace, pig iron is needed to pad the bottom of the furnace to match the slag surface, and pig iron can be directly added after steel is discharged. After adding, shake the converter backward to 50°, then shake it straight, and leave it for about 1 minute to lower the gun to splash slag. The lowest gun position for slag splashing is not less than 1 meter. If there is no rush to enter the furnace for blowing after the slag splashing is over, it can be left still first, and when it is needed, shake the furnace back and forth to confirm before entering.
7. The method according to claim 2, It is characterized in that The specific method of using the filling furnace sand to fill the slag surface is as follows: 1.6 to 4 tons of filling furnace sand is used to fill the slag surface, and the sintering time is 40 to 120 minutes; When the amount of supplementary furnace sand is 1.6-2.4 tons, the sintering time is 40 to 60 minutes; when the amount of supplementary furnace sand is 2.4 to 3.2 tons, the sintering time is 60 to 90 minutes; when the amount of supplementary furnace sand is 3.2 to 4 tons, the sintering time is 90 to 120 minutes.
8. The method according to claim 7, It is characterized in that When using furnace sand to pad the slag surface, the scrap steel in the furnace must be melted completely. The furnace seat of the furnace must be completed within 10 minutes from the completion of steel output to the spreading of the furnace sand. After the furnace sand is spread, oxygen-assisted heating must be used in time.
9. The method according to claim 1, It is characterized in that According to the erosion position of the slag line on the slag pouring surface, the depth of the slag line is controlled, and an appropriate amount of supplementary charge and a furnace shaking angle are added to spread it; when the erosion position is close to the molten pool, the amount of supplementary charge is less and the furnace shaking angle is 115°-120°; when the erosion position is close to the furnace cap, the amount of supplementary charge is more and the furnace shaking angle is 120°-125°.