Corrosion-resistant alloy seamless tube and processing technology thereof

By adding specific elements and processing to seamless steel pipes, a dense oxide film layer and passivation film are formed, which solves the problem of insufficient corrosion resistance and mechanical properties of seamless steel pipes in corrosive environments, and realizes the performance of seamless steel pipes in different environments. Long term use and high corrosion resistance.

CN118756038APending Publication Date: 2024-10-11ZHEJIANG YONGSHANG SPECIAL MATERIAL CO LTD
View PDF 0 Cites 0 Cited by

Patent Information

Application Number
CN202410750487.9
Authority / Receiving Office
CN · China
Patent Type
Applications(China)
Current Assignee / Owner
Filing Date
2024-06-12
Publication Date
2024-10-11

AI Technical Summary

Technical Problem

Existing seamless steel pipes have a short service life in corrosive environments, and it is difficult to ensure long-term corrosion resistance and mechanical properties. Especially in applications in different working environments, there is a problem of high corrosion sensitivity.

Method used

Corrosion-resistant alloy seamless pipes are made of specific composition, including 0.13~0.15% carbon, 0.8~1.1% chromium, 0.05~0.15% nickel, 0.5~0.7% manganese and other elements, and go through specific smelting and processing techniques, including smelting, Punching, rolling, cold drawing, quenching and passivation treatment to form a dense oxide film layer and passivation film to improve corrosion resistance and mechanical properties.

Benefits of technology

It achieves corrosion resistance and high mechanical strength for long-term use in corrosive environments. Through the combination of the oxide film layer and passivation film formed by chromium and nickel, the corrosion resistance and tensile resistance of seamless steel pipes are significantly improved. The problems of insufficient hardness and uneven internal structure after rapid quenching are avoided.

✦ Generated by Eureka AI based on patent content.

Smart Images

  • Figure BDA0004887742020000181
    Figure BDA0004887742020000181
  • Figure BDA0004887742020000191
    Figure BDA0004887742020000191
Patent Text Reader

Abstract

The invention relates to a corrosion-resistant alloy seamless tube and a processing technology thereof, and belongs to the related technical field of seamless tubes, and the corrosion-resistant alloy seamless tube comprises the following components in percentage by mass: 0.13-0.15% of carbon, 0.8-1.1% of chromium, 0.05-0.15% of nickel, 0.5-0.7% of manganese, 0.3-0.4% of silicon, 0.01-0.02% of phosphorus, 0.003-0.006% of sulfur, 0.02-0.1% of copper, 0.005-0.02% of titanium, and the balance of Fe and inevitable impurity elements. The corrosion-resistant alloy seamless pipe prepared by the steel pipe preparation process has excellent corrosion resistance and tensile property, and can be used for a long time in a corrosion environment.
Need to check novelty before this filing date? Find Prior Art

Description

Technical Field

[0001] The invention belongs to the technical field related to seamless pipes, and specifically relates to a corrosion-resistant alloy seamless pipe and a processing technology thereof. Background Art

[0002] Seamless steel pipes have high mechanical properties and are widely used in pipelines and structural components in the fields of petroleum, chemical, food, light industry, etc. Especially in recent years, more and more industries have adopted seamless steel pipes instead of solid round steel to manufacture mechanical parts, and the application environment of seamless steel pipes has become more and more extensive. Therefore, it is becoming more and more important to ensure the performance of seamless steel pipes in different environments.

[0003] Patent CN104197120A discloses a pressure-resistant and corrosion-resistant seamless steel pipe, including: a steel pipe body, a first anti-corrosion coating, a second anti-corrosion coating and an outer steel plate. The inner wall of the steel pipe body is coated with the first anti-corrosion coating. The patented technology mainly relies on the surface anti-corrosion coating to achieve corrosion resistance. The anti-corrosion coating is easy to fall off, and the anti-corrosion effect disappears. Patent CN106929639A discloses a quenching heat treatment process for shearing and slicing lead ingots in a cold granulator. The quenching liquid is prepared from polyalkylene glycol, dimethyl sulfoxide, polyvinyl alcohol, boric acid, copper sulfate, carboxymethyl cellulose, nano titanium dioxide, sodium lauryl sulfate, potassium nitrate, potassium sorbate and water. The quenching liquid provided by the patented technology has good corrosion resistance and aging resistance, but it cannot guarantee its long-term use in a corrosive environment.

[0004] Different working environments have different quality requirements for seamless steel pipes. Therefore, special smelting technology and processing technology are needed for seamless steel pipes. While ensuring the mechanical strength of the seamless steel pipe, the impact of corrosive substances on its surface is reduced and the corrosion sensitivity of the seamless steel pipe is reduced, thereby achieving long-term use of the seamless steel pipe in a corrosive environment. Summary of the invention

[0005] The object of the present invention is to provide a corrosion-resistant alloy seamless pipe having corrosion resistance and tensile resistance and capable of being used for a long time in a corrosive environment and a processing technology thereof.

[0006] In order to achieve the above object, the technical solution adopted by the present invention is as follows:

[0007] A corrosion-resistant alloy seamless pipe comprises the following components by mass percentage: 0.13-0.15% carbon, 0.8-1.1% chromium, 0.05-0.15% nickel, 0.5-0.7% manganese, 0.3-0.4% silicon, 0.01-0.02% phosphorus, 0.003-0.006% sulfur, 0.02-0.1% copper, 0.005-0.02% titanium, and the balance is Fe and unavoidable impurity elements.

[0008] Furthermore, the following components are included by mass percentage: 0.14% carbon, 1.0% chromium, 0.1% nickel, 0.6% manganese, 0.4% silicon, 0.01% phosphorus, 0.005% sulfur, 0.05% copper, 0.01% titanium, and the balance is Fe and unavoidable impurity elements.

[0009] A processing technology for a corrosion-resistant alloy seamless pipe comprises the following steps:

[0010] S1: Weigh all the components of the seamless steel pipe by weight, mix them, and then smelt them at 1460-1480°C, and then cast them into round billets at a casting temperature of 1220-1230°C;

[0011] S2: The round billet prepared in S1 is heated at 1230-1250°C for 4-5h, then pierced at 1200-1220°C and rolled into a steel pipe, the rolling temperature is 1050-1070°C, the tension reduction temperature is 880-900°C, and the final rolling temperature is 830-850°C;

[0012] S3: The steel pipe obtained in S2 is cold drawn at 1000-1150°C, sized at 580-610°C, straightened at 300-350°C, pickled, and then rinsed with water. The pickling solution is a sulfuric acid aqueous solution with a mass concentration of 10-20%. The pickling process lasts for 15-30 minutes and the pickling temperature is 35-40°C.

[0013] S4: The steel pipe treated by S3 is heated at 870-880°C, then kept warm for 1-1.5 hours, and then the steel pipe in the heat preservation is quenched with quenching liquid for 1-2 hours. The quenched steel pipe is tempered at 650-670°C, then kept warm for 1-2 hours, and finally straightened at 400-450°C;

[0014] S5: The steel pipe obtained in S4 is passivated with a passivation solution to obtain the corrosion-resistant alloy seamless pipe.

[0015] 4. The processing technology of a corrosion-resistant alloy seamless pipe according to claim 3 is characterized in that: the preparation method of the quenching liquid is:

[0016] A1: Mix 1-2 parts of propylene oxide, 2-4 parts of polyethylene glycol and 30-40 parts of water by weight, heat to 30-40°C, and stir for 10-15 minutes to obtain premixed solution A;

[0017] A2: Add 0.5-1 parts of polyurethane and 6-8 parts of polyacrylamide by weight into a reaction kettle equipped with a stirring device, and stir at 50-55° C. for 20-30 minutes to obtain a mixture;

[0018] A3: Heat the mixture obtained in A2 to 75-80°C, add 2-3 parts by weight of zinc nitrate, stir for 20-30 minutes, then add 1-3 parts of ethylene oxide, mix well, and obtain premixed solution B;

[0019] A4: The premixed liquid A obtained in A1 is added dropwise to the premixed liquid B prepared in A3, and 0.2-0.4 parts of carbon nanotube composite powder and 0.5-0.7 parts of chromic acid are added by weight. After stirring for 2-3 hours, the mixture is cooled to room temperature to obtain the quenching liquid.

[0020] Furthermore, the preparation method of the carbon nanotube composite powder is as follows: adding carboxylated double-walled carbon nanotubes and aluminum powder into deionized water to obtain a mixed solution A, ultrasonically treating the mixed solution A, and drying the mixed solution A to obtain the carbon nanotube composite powder, wherein the mass ratio of the carboxylated double-walled carbon nanotubes to the aluminum powder is 1:20 to 30.

[0021] Furthermore, the preparation method of the passivation solution is as follows: in parts by weight, 12 to 15 parts of sodium molybdate and 4 to 5 parts of zinc sulfate heptahydrate are added to 100 parts of water, mixed evenly, and stirred for 20 to 30 minutes to obtain a mixed solution B, and then 3 to 5 parts of ammonium fluorotitanate are slowly added to the mixed solution B, heated to 70 to 80° C., stirred for 1 to 2 hours, 2 to 4 parts of amino-modified nano-silica and 0.1 parts of silane coupling agent are added under stirring conditions, stirred for 5 to 10 minutes, and finally 200 to 300 parts of water are added, acid is added to adjust the pH to 4 to 5, mixed evenly, and a passivation solution is obtained.

[0022] Furthermore, the preparation method of the amino silicon dioxide is as follows: by weight, 10 parts of nano silicon dioxide are added to 50-60 parts of anhydrous ethanol, heated in a water bath to 70-80° C., then 0.3-0.5 parts of γ-aminopropyltriethoxysilane are added, the temperature is raised to boiling reflux and the reflux state is maintained for 5-6 hours, then the temperature is lowered, 80-100 parts of deionized water are added, centrifuged 3 times, the supernatant is discarded, filtered, and freeze-dried to obtain the amino silicon dioxide.

[0023] Furthermore, the passivation treatment time of the steel pipe in S5 is 30 to 40 minutes.

[0024] After adopting the above technical solution, the present invention has the following beneficial effects compared with the prior art:

[0025] 1. In the raw material components of the seamless steel pipe provided by the present invention, chromium and nickel can form dense chromium oxide and nickel oxide film layers to prevent further oxidation reactions and help improve the corrosion resistance of the material. By adjusting the contents of manganese, silicon, sulfur and phosphorus elements, the mechanical properties and corrosion tendency of the material can be improved. By properly controlling the contents of titanium and carbon, the lattice can be stabilized to improve the strength and corrosion resistance of the seamless steel pipe. The addition of copper can react with corrosive ions to prevent further corrosion. The pipe thus obtained has higher mechanical strength and good corrosion resistance.

[0026] 2. The quenching liquid provided by the present invention can not only improve the mechanical strength and corrosion resistance of the pipe, but also enhance the bonding strength between the passivation film and the pipe matrix, and further improve the corrosion resistance of the pipe. After the pipe is heated, the stress is relatively concentrated. It is difficult to evenly dissipate the heat in a short time when quenching it, and it is easy to form surface sudden cooling. The quenching liquid in the present invention has good viscosity and excellent hardenability. It can refine and improve the metallographic structure of the pipe. The cooling rate is slightly higher than the quenching oil and close to ordinary distilled water. The cooling rate is very slow, which can effectively avoid the risks of insufficient hardness, uneven internal organizational morphology, and easy cracking after ordinary rapid quenching, thereby improving the mechanical properties of the pipe. The content of random copolymers of ethylene oxide and propylene oxide in the quenching liquid is relatively small. Polyurethane can form a uniform and dense film layer by being used in combination with polyacrylamide and polyethylene glycol, effectively blocking corrosive media and improving the corrosion resistance of the alloy pipe body. By adding chromic acid to the quenching liquid, dirt on the steel surface can be removed to keep the pipe surface clean. The pipe surface can also be roughened to provide an adhesion surface basis for the passivation film. By adding carbon nanotube composite powder, the carboxylated double-walled carbon nanotubes are based on aluminum powder to achieve better dispersion performance. The carboxylated carbon nanotubes form bonds with the amino nano-silicon dioxide in the passivation film, and finally the passivation film is firmly adsorbed on the surface of the pipe matrix, thereby achieving high corrosion resistance of the alloy seamless pipe.

[0027] 3. The formation of passivation film on the surface of the pipe can effectively prevent the corrosive medium from damaging the internal metal, achieve corrosion protection for the pipe matrix, and show excellent corrosion resistance. DETAILED DESCRIPTION

[0028] The following will be combined with the embodiments of the present invention to clearly and completely describe the technical solutions of the present invention. Obviously, the described embodiments are only part of the embodiments of the present invention, rather than all the embodiments. The following description of at least one exemplary embodiment is actually only illustrative and is by no means intended to limit the present invention and its application or use. Based on the embodiments of the present invention, all other embodiments obtained by ordinary technicians in this field without creative work are within the scope of protection of the present invention.

[0029] The carboxylated double-walled carbon nanotubes involved in the following examples and comparative examples were purchased from Nanjing Saihongrui Biotechnology Co., Ltd.

[0030] Example 1: A corrosion-resistant alloy seamless pipe comprises the following components, by weight: 0.14 parts of carbon, 1.0 parts of chromium, 0.1 parts of nickel, 0.6 parts of manganese, 0.4 parts of silicon, 0.01 parts of phosphorus, 0.005 parts of sulfur, 0.05 parts of copper, 0.01 parts of titanium, and the balance being Fe and unavoidable impurity elements.

[0031] A processing technology for a corrosion-resistant alloy seamless pipe comprises the following steps:

[0032] S1: Weigh all components of the corrosion-resistant alloy seamless pipe by weight, mix them, smelt them at 1470°C, and then cast them into round billets at a casting temperature of 1220°C;

[0033] S2: The round billet prepared in S1 is heated at 1240°C for 5 hours, then pierced at 1210°C, and then rolled into a steel pipe at a rolling temperature of 1060°C, a tension reduction temperature of 900°C, and a final rolling temperature of 840°C;

[0034] S3: The steel pipe obtained in S2 is cold drawn at 1120°C, sized at 600°C, straightened at 320°C, and rinsed with water after pickling. The pickling solution is a sulfuric acid aqueous solution with a mass concentration of 15%. The pickling process lasts for 20 minutes at a temperature of 40°C.

[0035] S4: The steel pipe treated by S3 is heated at 880°C, then kept warm for 1.5 hours, and then the steel pipe in the heat preservation is quenched with quenching liquid for 1 hour. The quenched steel pipe is tempered at 660°C, then kept warm for 1.5 hours, and finally straightened at 420°C;

[0036] S5: The steel pipe obtained in S4 is passivated with a passivation solution for 30 minutes to obtain the corrosion-resistant alloy seamless pipe.

[0037] The preparation method of the quenching liquid is:

[0038] A1: Mix 2 parts of propylene oxide, 4 parts of polyethylene glycol and 35 parts of water by weight, heat to 40°C, and stir for 10 minutes to obtain premixed solution A;

[0039] A2: 0.5 parts of polyurethane and 7 parts of polyacrylamide were added into a reaction kettle equipped with a stirring device, and stirred at 55° C. for 20 minutes to obtain a mixture;

[0040] A3: Heat the mixture obtained in A2 to 80°C, add 2 parts of zinc nitrate by weight, stir for 30 minutes, then add 2 parts of ethylene oxide, mix well, and obtain premixed solution B;

[0041] A4: The premixed solution A obtained in A1 is added dropwise to the premixed solution B prepared in A3, and 0.3 parts of carbon nanotube composite powder and 0.6 parts of chromic acid are added by weight. After stirring for 3 hours, the mixture is cooled to room temperature to obtain the quenching solution.

[0042] The preparation method of carbon nanotube composite powder is as follows:

[0043] The preparation method of the carbon nanotube composite powder is as follows: adding carboxylated double-walled carbon nanotubes and aluminum powder into deionized water to obtain a mixed solution A, ultrasonically treating the mixed solution A, and drying the mixed solution to obtain the carbon nanotube composite powder, wherein the mass ratio of the carboxylated double-walled carbon nanotubes to the aluminum powder is 1:25.

[0044] The preparation method of the passivation solution is:

[0045] In parts by weight, 12 parts of sodium molybdate and 4 parts of zinc sulfate heptahydrate were added to 100 parts of water, mixed evenly, and stirred for 20 minutes to obtain a mixed solution B, and then 4 parts of ammonium fluorotitanate were slowly added to the mixed solution B, heated to 75°C, stirred for 1.5 hours, and 3 parts of amino-modified nano-silica and 0.1 parts of silane coupling agent were added under stirring conditions, stirred for 10 minutes, and finally 200 parts of water were added, acid was added to adjust the pH to 4, and mixed evenly to obtain a passivation solution.

[0046] The preparation method of amination silicon dioxide is:

[0047] By weight, 10 parts of nano-silica were added to 50 parts of anhydrous ethanol, heated to 75°C in a water bath, and then 0.4 parts of γ-aminopropyltriethoxysilane were added, the temperature was raised to boiling reflux and the reflux state was maintained for 6 hours, then the temperature was lowered, 80 parts of deionized water were added, centrifuged 3 times, the supernatant was discarded, and the remaining substances were filtered and freeze-dried in turn to obtain amino nano-silica.

[0048] Example 2: A corrosion-resistant alloy seamless pipe comprises the following components, by weight: 0.13 parts of carbon, 0.8 parts of chromium, 0.05 parts of nickel, 0.5 parts of manganese, 0.3 parts of silicon, 0.01 parts of phosphorus, 0.003 parts of sulfur, 0.02 parts of copper, 0.005 parts of titanium, and the remainder being Fe and unavoidable impurity elements.

[0049] A processing technology for a corrosion-resistant alloy seamless pipe comprises the following steps:

[0050] S1: Weigh all components of the corrosion-resistant alloy seamless pipe by weight, mix them, smelt them at 1460°C, and then cast them into round billets at a casting temperature of 1220°C;

[0051] S2: The round billet prepared in S1 is heated at 1230°C for 4 hours, then pierced at 1200°C, and then rolled into a steel pipe at a rolling temperature of 1050°C, a tension reduction temperature of 880°C, and a final rolling temperature of 830°C;

[0052] S3: The steel pipe obtained in S2 is cold drawn at 1000°C, sized at 580°C, straightened at 300°C, and rinsed with water after pickling. The pickling solution is a sulfuric acid aqueous solution with a mass concentration of 10%. The pickling process lasts for 15 minutes at a temperature of 35°C.

[0053] S4: The steel pipe treated by S3 is heated at 870°C, then kept warm for 1 hour, and then the steel pipe in the heat preservation is quenched with quenching liquid for 1 hour. The quenched steel pipe is tempered at 650°C, then kept warm for 1 hour, and finally straightened at 400°C;

[0054] S5: The steel pipe obtained in S4 is passivated with a passivation solution for 30 minutes to obtain the corrosion-resistant alloy seamless pipe.

[0055] The preparation method of the quenching liquid is:

[0056] A1: Mix 1 part of propylene oxide, 2 parts of polyethylene glycol and 30 parts of water by weight, heat to 30°C, and stir for 10 minutes to obtain premixed solution A;

[0057] A2: 0.5 parts of polyurethane and 6 parts of polyacrylamide were added into a reaction kettle equipped with a stirring device, and stirred at 50° C. for 20 minutes to obtain a mixture;

[0058] A3: Heat the mixture obtained in A2 to 75°C, add 2 parts by weight of zinc nitrate, stir for 20 minutes, then add 1 part of ethylene oxide, mix well, and obtain premixed solution B;

[0059] A4: The premixed solution A obtained in A1 is added dropwise to the premixed solution B prepared in A3, and 0.2 parts of carbon nanotube composite powder and 0.5 parts of chromic acid are added by weight. After stirring for 2 hours, the mixture is cooled to room temperature to obtain the quenching solution.

[0060] The preparation method of carbon nanotube composite powder is as follows:

[0061] Carboxylated double-walled carbon nanotubes and aluminum powder are added to deionized water to obtain a mixed solution A, and the mixed solution A is subjected to ultrasonic treatment and dried to obtain a carbon nanotube composite powder, wherein the mass ratio of the carboxylated double-walled carbon nanotubes to the aluminum powder is 1:20.

[0062] The preparation method of the passivation solution is:

[0063] In parts by weight, 12 parts of sodium molybdate and 4 parts of zinc sulfate heptahydrate were added to 100 parts of water, mixed evenly, and stirred for 20 minutes to obtain a mixed solution B, and then 3 parts of ammonium fluorotitanate were slowly added to the mixed solution B, heated to 70°C, stirred for 1 hour, 2 parts of amino-modified nano-silica and 0.1 parts of silane coupling agent were added under stirring, stirred for 5 minutes, and finally 200 parts of water were added, acid was added to adjust the pH to 5, mixed evenly, and a passivation solution was obtained.

[0064] The preparation method of amination silicon dioxide is:

[0065] By weight, 10 parts of nano-silica were added to 50 parts of anhydrous ethanol, heated to 70°C in a water bath, and then 0.3 parts of γ-aminopropyltriethoxysilane were added, the temperature was raised to boiling reflux and the reflux state was maintained for 5 hours, then the temperature was lowered, 80 parts of deionized water were added, centrifuged 3 times, the supernatant was discarded, and the remaining substances were filtered and freeze-dried in turn to obtain amino nano-silica.

[0066] Example 3: A corrosion-resistant alloy seamless pipe comprises the following components, by weight: 0.15 parts of carbon, 1.1 parts of chromium, 0.15 parts of nickel, 0.7 parts of manganese, 0.4 parts of silicon, 0.02 parts of phosphorus, 0.006 parts of sulfur, 0.1 parts of copper, 0.02 parts of titanium, and the remainder being Fe and unavoidable impurity elements.

[0067] A processing technology for a corrosion-resistant alloy seamless pipe comprises the following steps:

[0068] S1: Weigh all components of the corrosion-resistant alloy seamless pipe by weight, mix them, smelt them at 1480°C, and then cast them into round billets at a casting temperature of 1230°C;

[0069] S2: The round billet prepared in S1 is heated at 1250°C for 5 hours, then pierced at 1220°C, and then rolled into a steel pipe at a rolling temperature of 1070°C, a tension reduction temperature of 900°C, and a final rolling temperature of 850°C;

[0070] S3: The steel pipe obtained in S2 is cold drawn at 1150°C, sized at 610°C, straightened at 350°C, and rinsed with water after pickling. The pickling solution is a sulfuric acid aqueous solution with a mass concentration of 20%. The pickling process lasts for 30 minutes at a temperature of 40°C.

[0071] S4: The steel pipe treated by S3 is heated at 880°C, then kept warm for 1.5 hours, and then quenched with quenching liquid for 2 hours. The quenched steel pipe is tempered at 670°C, then kept warm for 2 hours, and finally straightened at 450°C;

[0072] S5: The steel pipe obtained in S4 is passivated with a passivation solution for 40 minutes to obtain the corrosion-resistant alloy seamless pipe.

[0073] The preparation method of the quenching liquid is:

[0074] A1: Mix 2 parts of propylene oxide, 4 parts of polyethylene glycol and 40 parts of water by weight, heat to 40°C, and stir for 15 minutes to obtain premixed solution A;

[0075] A2: Add 1 part of polyurethane and 8 parts of polyacrylamide, by weight, into a reaction kettle equipped with a stirring device, and stir at 55° C. for 30 minutes to obtain a mixture;

[0076] A3: Heat the mixture obtained in A2 to 80°C, add 3 parts of zinc nitrate by weight, stir for 30 minutes, then add 3 parts of ethylene oxide, mix well, and obtain premixed solution B;

[0077] A4: The premixed solution A obtained in A1 is added dropwise to the premixed solution B prepared in A3, and 0.4 parts of carbon nanotube composite powder and 0.7 parts of chromic acid are added by weight. After stirring for 3 hours, the mixture is cooled to room temperature to obtain the quenching solution.

[0078] The preparation method of carbon nanotube composite powder is as follows:

[0079] Carboxylated double-walled carbon nanotubes and aluminum powder are added to deionized water to obtain a mixed solution A, and the mixed solution A is subjected to ultrasonic treatment and dried to obtain a carbon nanotube composite powder, wherein the mass ratio of the carboxylated double-walled carbon nanotubes to the aluminum powder is 1:30.

[0080] The preparation method of the passivation solution is:

[0081] In parts by weight, 15 parts of sodium molybdate and 5 parts of zinc sulfate heptahydrate were added to 100 parts of water, mixed evenly, and stirred for 30 minutes to obtain a mixed solution B, and then 5 parts of ammonium fluorotitanate were slowly added to the mixed solution B, heated to 80°C, stirred for 2 hours, 4 parts of amino-modified nano-silica and 0.1 parts of silane coupling agent were added under stirring, stirred for 10 minutes, and finally 300 parts of water were added, acid was added to adjust the pH to 5, mixed evenly, and a passivation solution was obtained.

[0082] The preparation method of amination silicon dioxide is:

[0083] By weight, 10 parts of nano-silica were added to 60 parts of anhydrous ethanol, heated to 80°C in a water bath, and then 0.5 parts of γ-aminopropyltriethoxysilane were added. The temperature was raised to boiling reflux and the reflux state was maintained for 6 hours. The temperature was then lowered and added to 100 parts of deionized water. The mixture was centrifuged 3 times, the supernatant was discarded, and the remaining substances were filtered and freeze-dried in turn to obtain amino-modified nano-silica.

[0084] Example 4: A corrosion-resistant alloy seamless pipe comprises the following components, by weight: 0.13 parts of carbon, 0.9 parts of chromium, 0.08 parts of nickel, 0.6 parts of manganese, 0.34 parts of silicon, 0.013 parts of phosphorus, 0.004 parts of sulfur, 0.04 parts of copper, 0.008 parts of titanium, and the remainder being Fe and unavoidable impurity elements.

[0085] A processing technology for a corrosion-resistant alloy seamless pipe comprises the following steps:

[0086] S1: Weigh all components of the corrosion-resistant alloy seamless pipe by weight, mix them, smelt them at 1465°C, and then cast them into round billets at a casting temperature of 1223°C;

[0087] S2: The round billet prepared in S1 is heated at 1235°C for 4 hours, then pierced at 1205°C, and then rolled into a steel pipe at a rolling temperature of 1055°C, a tension reduction temperature of 885°C, and a final rolling temperature of 835°C;

[0088] S3: The steel pipe obtained in S2 is cold drawn at 1080°C, sized at 590°C, straightened at 310°C, and rinsed with water after pickling. The pickling solution is a sulfuric acid aqueous solution with a mass concentration of 12%. The pickling process lasts for 20 minutes at a temperature of 35°C.

[0089] S4: The steel pipe treated by S3 is heated at 870°C, then kept warm for 1.2 hours, and then the steel pipe in the heat preservation is quenched with quenching liquid for 1.2 hours. The quenched steel pipe is tempered at 655°C, then kept warm for 1 hour, and finally straightened at 410°C;

[0090] S5: The steel pipe obtained in S4 is passivated with a passivation solution for 30 minutes to obtain the corrosion-resistant alloy seamless pipe.

[0091] The preparation method of the quenching liquid is:

[0092] A1: By weight, 1.3 parts of propylene oxide, 2.5 parts of polyethylene glycol and 33 parts of water were mixed evenly, heated to 30°C, and stirred for 10 minutes to obtain premixed solution A;

[0093] A2: 0.7 parts of polyurethane and 6.5 parts of polyacrylamide were added into a reaction kettle equipped with a stirring device, and stirred at 50° C. for 20 minutes to obtain a mixture;

[0094] A3: Heat the mixture obtained in A2 to 75°C, add 2.8 parts of zinc nitrate by weight, stir for 25 minutes, then add 1.5 parts of ethylene oxide, mix well, and obtain premixed solution B;

[0095] A4: The premixed solution A obtained in A1 is added dropwise to the premixed solution B prepared in A3, and 0.2 parts of carbon nanotube composite powder and 0.5 parts of chromic acid are added by weight. After stirring for 2.5 hours, the mixture is cooled to room temperature to obtain the quenching solution.

[0096] The preparation method of carbon nanotube composite powder is as follows:

[0097] Carboxylated double-walled carbon nanotubes and aluminum powder are added to deionized water to obtain a mixed solution A, and the mixed solution A is subjected to ultrasonic treatment and dried to obtain a carbon nanotube composite powder, wherein the mass ratio of the carboxylated double-walled carbon nanotubes to the aluminum powder is 1:23.

[0098] The preparation method of the passivation solution is:

[0099] In parts by weight, 13 parts of sodium molybdate and 4.5 parts of zinc sulfate heptahydrate were added to 100 parts of water, mixed evenly, and stirred for 23 minutes to obtain a mixed solution B, and then 3.5 parts of ammonium fluorotitanate were slowly added to the mixed solution B, heated to 75°C, stirred for 1 hour, 2.5 parts of amino-modified nano-silica and 0.1 parts of silane coupling agent were added under stirring, stirred for 6 minutes, and finally 220 parts of water were added, acid was added to adjust the pH to 4, mixed evenly, and a passivation solution was obtained.

[0100] The preparation method of amination silicon dioxide is:

[0101] By weight, 10 parts of nano-silica were added to 53 parts of anhydrous ethanol, heated to 75°C in a water bath, and then 0.35 parts of γ-aminopropyltriethoxysilane were added. The temperature was raised to boiling reflux and maintained at reflux for 5 hours. The temperature was then lowered and added to 85 parts of deionized water. The mixture was centrifuged three times, the supernatant was discarded, and the remaining substances were filtered and freeze-dried in turn to obtain amino-modified nano-silica.

[0102] Example 5: A corrosion-resistant alloy seamless pipe comprises the following components, by weight: 0.15 parts of carbon, 1.0 parts of chromium, 0.13 parts of nickel, 0.7 parts of manganese, 0.4 parts of silicon, 0.018 parts of phosphorus, 0.005 parts of sulfur, 0.08 parts of copper, 0.015 parts of titanium, and the remainder being Fe and unavoidable impurity elements.

[0103] A processing technology for a corrosion-resistant alloy seamless pipe comprises the following steps:

[0104] S1: Weigh all components of the corrosion-resistant alloy seamless pipe by weight, mix them, smelt them at 1475°C, and then cast them into round billets at a casting temperature of 1228°C;

[0105] S2: The round billet prepared in S1 is heated at 1238°C for 5 hours, then pierced at 1218°C, and then rolled into a steel pipe at a rolling temperature of 1065°C, a tension reduction temperature of 895°C, and a final rolling temperature of 845°C;

[0106] S3: The steel pipe obtained in S2 is cold drawn at 1145°C, sized at 605°C, straightened at 340°C, and rinsed with water after pickling. The pickling solution is a sulfuric acid aqueous solution with a mass concentration of 18%. The pickling process lasts for 25 minutes at a temperature of 40°C.

[0107] S4: The steel pipe treated with S3 is heated at 880°C, then kept warm for 1.4 hours, and then quenched with quenching liquid for 1.8 hours. The quenched steel pipe is tempered at 665°C, then kept warm for 2 hours, and finally straightened at 445°C;

[0108] S5: The steel pipe obtained in S4 is passivated with a passivation solution for 40 minutes to obtain the corrosion-resistant alloy seamless pipe.

[0109] The preparation method of the quenching liquid is:

[0110] A1: 1.8 parts of propylene oxide, 3.5 parts of polyethylene glycol and 38 parts of water were mixed evenly by weight, heated to 40°C, and stirred for 14 minutes to obtain premixed solution A;

[0111] A2: 0.9 parts of polyurethane and 7.5 parts of polyacrylamide were added into a reaction kettle equipped with a stirring device, and stirred at 55° C. for 28 minutes to obtain a mixture;

[0112] A3: Heat the mixture obtained in A2 to 80°C, add 2.8 parts of zinc nitrate by weight, stir for 28 minutes, then add 2.5 parts of ethylene oxide, mix well, and obtain premixed solution B;

[0113] A4: The premixed solution A obtained in A1 is added dropwise to the premixed solution B prepared in A3, and 0.4 parts of carbon nanotube composite powder and 0.7 parts of chromic acid are added by weight. After stirring for 3 hours, the mixture is cooled to room temperature to obtain the quenching solution.

[0114] The preparation method of carbon nanotube composite powder is as follows:

[0115] Carboxylated double-walled carbon nanotubes and aluminum powder are added to deionized water to obtain a mixed solution A, and the mixed solution A is subjected to ultrasonic treatment and dried to obtain a carbon nanotube composite powder, wherein the mass ratio of the carboxylated double-walled carbon nanotubes to the aluminum powder is 1:28.

[0116] The preparation method of the passivation solution is:

[0117] In parts by weight, 14 parts of sodium molybdate and 4.8 parts of zinc sulfate heptahydrate were added to 100 parts of water, mixed evenly, and stirred for 28 minutes to obtain a mixed solution B, and then 4.5 parts of ammonium fluorotitanate were slowly added to the mixed solution B, heated to 80°C, stirred for 2 hours, 3.5 parts of amino-modified nano-silica and 0.1 parts of silane coupling agent were added under stirring, stirred for 9 minutes, and finally 280 parts of water were added, acid was added to adjust the pH to 5, mixed evenly, and a passivation solution was obtained.

[0118] The preparation method of amination silicon dioxide is:

[0119] By weight, 10 parts of nano-silica were added to 58 parts of anhydrous ethanol, heated to 80°C in a water bath, and then 0.5 parts of γ-aminopropyltriethoxysilane were added. The temperature was raised to boiling reflux and the reflux state was maintained for 6 hours. The temperature was then lowered and added to 95 parts of deionized water. The mixture was centrifuged three times, the supernatant was discarded, and the remaining substances were filtered and freeze-dried in turn to obtain amino-modified nano-silica.

[0120] Comparative Example 1: The difference between Comparative Example 1 and Example 1 is that manganese in the raw material composition of a corrosion-resistant alloy seamless pipe is replaced by silicon;

[0121] A corrosion-resistant alloy seamless pipe comprises the following components by weight percentage: 0.14 parts of carbon, 1.0 parts of chromium, 0.1 parts of nickel, 1 parts of silicon, 0.01 parts of phosphorus, 0.005 parts of sulfur, 0.05 parts of copper, 0.01 parts of titanium, and the balance is Fe and unavoidable impurity elements.

[0122] Comparative Example 2: The difference between Comparative Example 2 and Example 1 is that the quenching liquid in S5 is water.

[0123] Comparative Example 3: The difference between Comparative Example 3 and Example 1 is that no carbon nanotube composite powder and chromic acid are added in the preparation of the quenching liquid: The preparation method of the quenching liquid is as follows:

[0124] A1: Mix 2 parts of propylene oxide, 4 parts of polyethylene glycol and 35 parts of water by weight, heat to 40°C, and stir for 10 minutes to obtain premixed solution A;

[0125] A2: 0.5 parts of polyurethane and 7 parts of polyacrylamide were added into a reaction kettle equipped with a stirring device, and stirred at 55° C. for 20 minutes to obtain a mixture;

[0126] A3: Heat the mixture obtained in A2 to 80°C, add 2 parts of zinc nitrate by weight, stir for 30 minutes, then add 2 parts of ethylene oxide, mix well, and obtain premixed solution B;

[0127] A4: The premixed solution A obtained in A1 is added dropwise to the premixed solution B prepared in A3, and the mixture is stirred at the temperature for 3 hours, and then cooled to room temperature to obtain the quenching solution.

[0128] Comparative Example 4: The difference between Comparative Example 4 and Example 1 is that no amino-modified nano-silica is added in the preparation of the passivation solution;

[0129] The preparation method of the passivation solution is:

[0130] In parts by weight, 12 parts of sodium molybdate and 4 parts of zinc sulfate heptahydrate were added to 100 parts of water, mixed evenly, and stirred for 20 minutes to obtain a mixed solution B, and then 4 parts of ammonium fluorotitanate were slowly added to the mixed solution B, heated to 75°C, stirred for 1.5 hours, 0.1 parts of silane coupling agent were added under stirring, stirred for 10 minutes, and finally 200 parts of water were added, acid was added to adjust the pH to 4, mixed evenly, and a passivation solution was obtained.

[0131] Comparative Example 5: The difference between Comparative Example 5 and Example 1 is that no carbon nanotube composite powder and chromic acid are added in the preparation of the quenching liquid, and no amino-treated nano-silica is added in the preparation of the passivation liquid.

[0132] The seamless steel pipes of the embodiments and comparative examples were subjected to performance testing. According to the method described in the national industry standard "GB / T10125-2021", the neutral salt spray resistance of the seamless steel pipes was tested. The test cycle was one month. The tensile strength was the tensile strength before corrosion. The test was performed according to the ASTM standard. The tensile strength and corrosion resistance rate of the seamless steel pipes prepared in the embodiments and comparative examples are shown in Table 1.

[0133]

[0134]

[0135] The corrosion rate of the seamless steel pipes in Examples 1 to 5 is low and the tensile strength is high, indicating that the corrosion-resistant alloy seamless pipes prepared in the present invention have excellent corrosion resistance and excellent tensile resistance.

[0136] Comparative Example 1: The difference between Comparative Example 1 and Example 1 is that manganese in the raw material composition of a corrosion-resistant alloy seamless pipe is replaced by silicon, and the corrosion rate of the seamless steel pipe prepared in Comparative Example 1 is higher than the corrosion rate of the seamless steel pipe prepared in Example 1. At the same time, the tensile strength of the seamless steel pipe prepared in Comparative Example 1 is lower than the tensile strength of the seamless steel pipe prepared in Example 1, indicating that the use of manganese improves the corrosion resistance and tensile resistance of the seamless steel pipe.

[0137] Comparative Example 2: The difference between Comparative Example 2 and Example 1 is that the quenching liquid in S5 is water.

[0138] The corrosion rate of the seamless steel pipe prepared in Comparative Example 2 is higher than that of the seamless steel pipe prepared in Example 1. At the same time, the tensile strength of the seamless steel pipe prepared in Comparative Example 2 is lower than that of the seamless steel pipe prepared in Example 1, indicating that the type and use of quenching liquid affect the corrosion resistance and tensile resistance of the seamless steel pipe.

[0139] Comparative Example 3: The difference between Comparative Example 3 and Example 1 is that, in the preparation of the quenching liquid, no carbon nanotube composite powder and chromic acid are added, and the corrosion rate of the seamless steel pipe prepared in Comparative Example 3 is higher than the corrosion rate of the seamless steel pipe prepared in Example 1, indicating that the carbon nanotube composite powder and chromic acid can improve the corrosion resistance of the seamless steel pipe.

[0140] Comparative Example 4: The difference between Comparative Example 4 and Example 1 is that, in the preparation of the passivating solution, no amino nano-silica is added. The corrosion rate of the seamless steel pipe prepared in Comparative Example 4 is higher than the corrosion rate of the seamless steel pipe prepared in Example 1, indicating that amino nano-silica can improve the corrosion resistance of the seamless steel pipe.

[0141] Comparative Example 5: The difference between Comparative Example 5 and Example 1 is that no carbon nanotube composite powder and chromic acid are added in the preparation of the quenching liquid, and no amino-treated nano-silica is added in the preparation of the passivation liquid.

[0142] The corrosion rate of the seamless steel pipe prepared in Comparative Example 5 is higher than the corrosion rate of the seamless steel pipe prepared in Example 1. At the same time, the corrosion rate of the seamless steel pipe prepared in Comparative Example 5 is higher than the corrosion rate of the seamless steel pipe prepared in Comparative Examples 3 and 4, indicating that the use of carbon nanotube composite powder and chromic acid as a composition together with amino-treated nano-silica can synergistically improve the corrosion resistance of the seamless steel pipe.

[0143] The above description is only a preferred specific implementation manner of the present invention, but the protection scope of the present invention is not limited thereto. Any technician familiar with the technical field can make equivalent replacements or changes according to the technical scheme and inventive concept of the present invention within the technical scope disclosed by the present invention, which should be covered by the protection scope of the present invention.

Claims

1. A corrosion-resistant alloy seamless pipe, characterized in that: Calculated by mass percentage, it includes the following components: 0.13-0.15% carbon, 0.8-1.1% chromium, 0.05-0.15% nickel, 0.5-0.7% manganese, 0.3-0.4% silicon, 0.01-0.02% phosphorus, 0.003-0.006% sulfur, 0.02-0.1% copper and 0.005-0.02% titanium, and the balance is Fe and unavoidable impurity elements.

2. The corrosion-resistant alloy seamless pipe according to claim 1, characterized in that: In terms of mass percentage, it includes the following components: 0.14% carbon, 1.0% chromium, 0.1% nickel, 0.6% manganese, 0.4% silicon, 0.01% phosphorus, 0.005% sulfur, 0.05% copper and 0.01% titanium, and the balance is Fe and unavoidable impurity elements.

3. A processing technology for a corrosion-resistant alloy seamless pipe as claimed in any one of claims 1 to 2, characterized in that: The following steps are involved: S1: Weigh all the components of the seamless steel pipe by weight, mix them, and then smelt them at 1460-1480° C., and then cast them into round billets at a casting temperature of 1220-1230° C.; S2: The round billet prepared in S1 is heated at 1230-1250°C for 4-5h, then pierced at 1200-1220°C and rolled into a steel pipe, the rolling temperature is 1050-1070°C, the tension reduction temperature is 880-900°C, and the final rolling temperature is 830-850°C; S3: The steel pipe obtained in S2 is cold drawn at 1000-1150°C, sized at 580-610°C, straightened at 300-350°C, pickled, and then rinsed with water. The pickling solution is a sulfuric acid aqueous solution with a mass concentration of 10-20%. The pickling process lasts for 15-30 minutes and the pickling temperature is 35-40°C. S4: The steel pipe treated by S3 is heated at 870-880°C, then kept warm for 1-1.5 hours, and then the steel pipe in the heat preservation is quenched with quenching liquid for 1-2 hours. The quenched steel pipe is tempered at 650-670°C, then kept warm for 1-2 hours, and finally straightened at 400-450°C; S5: The steel pipe obtained in S4 is passivated with a passivation solution to obtain the corrosion-resistant alloy seamless pipe.

4. The processing technology of a corrosion-resistant alloy seamless pipe according to claim 3 is characterized in that: The preparation method of the quenching liquid is: A1: Mix 1-2 parts of propylene oxide, 2-4 parts of polyethylene glycol and 30-40 parts of water by weight, heat to 30-40°C, and stir for 10-15 minutes to obtain premixed solution A; A2: Add 0.5-1 parts of polyurethane and 6-8 parts of polyacrylamide by weight into a reaction kettle equipped with a stirring device, and stir at 50-55° C. for 20-30 minutes to obtain a mixture; A3: Heat the mixture obtained in A2 to 75-80°C, add 2-3 parts by weight of zinc nitrate, stir for 20-30 minutes, then add 1-3 parts of ethylene oxide, mix well, and obtain premixed solution B; A4: The premixed liquid A obtained in A1 is added dropwise to the premixed liquid B prepared in A3, and 0.2-0.4 parts of carbon nanotube composite powder and 0.5-0.7 parts of chromic acid are added by weight. After stirring for 2-3 hours, the mixture is cooled to room temperature to obtain the quenching liquid.

5. The processing technology of a corrosion-resistant alloy seamless pipe according to claim 4 is characterized in that: The preparation method of the carbon nanotube composite powder comprises the following steps: adding carboxylated double-walled carbon nanotubes and aluminum powder into deionized water to obtain a mixed solution A, ultrasonically treating the mixed solution A, and drying the mixed solution to obtain the carbon nanotube composite powder, wherein the mass ratio of the carboxylated double-walled carbon nanotubes to the aluminum powder is 1:20-30.

6. The processing technology of a corrosion-resistant alloy seamless pipe according to claim 3 is characterized in that: The preparation method of the passivation solution is as follows: in parts by weight, 12 to 15 parts of sodium molybdate and 4 to 5 parts of zinc sulfate heptahydrate are added to 100 parts of water, the mixture is evenly mixed, and the mixture is fully stirred for 20 to 30 minutes to obtain a mixed solution B, and then 3 to 5 parts of ammonium fluorotitanate are slowly added to the mixed solution B, the mixture is heated to 70 to 80° C., and the mixture is fully stirred for 1 to 2 hours. Under stirring conditions, 2 to 4 parts of amino-modified nano-silicon dioxide and 0.1 part of a silane coupling agent are added, and the mixture is stirred for 5 to 10 minutes. Finally, 200 to 300 parts of water are added, acid is added to adjust the pH value to 4 to 5, and the mixture is evenly mixed to obtain the passivation solution.

7. The processing technology of a corrosion-resistant alloy seamless pipe according to claim 6 is characterized in that: The preparation method of the amino silicon dioxide is as follows: by weight, 10 parts of nano silicon dioxide are added to 50-60 parts of anhydrous ethanol, heated in a water bath to 70-80° C., then 0.3-0.5 parts of γ-aminopropyltriethoxysilane are added, the temperature is raised to boiling reflux and the reflux state is maintained for 5-6 hours, then the temperature is lowered, the mixture is added to 80-100 parts of deionized water, centrifuged for 3 times, the supernatant is discarded, filtered, and freeze-dried to obtain the amino silicon dioxide.

8. The processing technology of a corrosion-resistant alloy seamless pipe according to claim 3 is characterized in that: The passivation treatment time of the steel pipe in S5 is 30 to 40 minutes.