A high-strength and tough nitride film and its preparation method and application
By designing a combination of a high-strength toughness (TiaAlbNbcTadXe) N-type nitride film and a SiO2 substrate, the measurement error problem caused by deformation of the resonant sensor in precision processing is solved, and the clamping force test with high accuracy and stability is achieved.
Patent Information
- Application Number
- CN202411237607.1
- Authority / Receiving Office
- CN · China
- Patent Type
- Patents(China)
- Current Assignee / Owner
- Filing Date
- 2024-09-05
- Publication Date
- 2024-12-03
- Estimated Expiration
- 2044-09-05
AI Technical Summary
The deformation caused by the large clamping force during the precision machining of the existing resonant sensors affects the sensor's induction accuracy and test repeatability, and the bonding ability with the SiO2 substrate is insufficient, resulting in measurement errors.
(TiaAlbNbcTadXe)N type high-strength tough nitride film is used as electrode material, and is prepared by component design and magnetron cosputtering technology. The nanohardness is ≥20 GPa, the toughness H3/E2 value is ≥0.15, and it is good with the a-SiO2 substrate. Combined.
Improves the strength and toughness of the nitride film and its binding force with the SiO2 substrate, reduces the deformation of the sensor, enhances the stability and accuracy of measurement, and realizes a high-strength and high-toughness resonant sensor suitable for clamping force testing. .
Smart Images

Figure CN118756097B_ABST
Abstract
Description
Technical Field
[0001] The present application relates to the technical field of nitride thin films, and in particular to a high-strength and toughness nitride thin film and a preparation method and application thereof. Background Art
[0002] With the development trend of industrial automation and digitalization, the related systems and products combining automated tooling with intelligent sensors are one of the urgent needs. The development and application of intelligent sensors for precision machining industries are gradually gaining attention, such as new energy vehicle manufacturing, aerospace, marine and other industrial heavy equipment products. Its tooling fixtures require intelligent sensors to monitor and sense various physical parameters in real time in terms of clamping force maintenance and positioning, to confirm that its clamping force can maintain a stable state and safety, to adapt to processing objects of different shapes and sizes, and to improve production efficiency and product quality. This places high demands on the mechanical response time, accuracy, repeatability and other parameters of the sensor.
[0003] Resonant sensors have obvious advantages in mechanical response time, accuracy, repeatability and other parameters. The principle is to use the inverse piezoelectric effect of piezoelectric materials to produce a resonant fundamental frequency of a fixed frequency. When subjected to external force, the resonant frequency changes and is proportional to the strength of the external force, thereby calculating the value of the external force. However, during precision machining, tooling fixtures usually require a large clamping force to maintain machining stability, which causes the sensor to deform to a certain extent and further affects the electrode layer. At present, the electrodes of resonant sensors are mainly soft metals with excellent conductivity such as gold and silver. Their deformation under force will cause changes in the overall frequency of the sensor, thereby causing measurement errors, resulting in a decrease in the sensor's sensing accuracy and test repeatability.
[0004] It should be noted that the information disclosed in this background technology section is only intended to deepen the understanding of the overall background technology of the present invention, and should not be regarded as an admission or suggestion in any form that the information constitutes the prior art known to those skilled in the art. Summary of the invention
[0005] The first problem to be solved by the present invention is to provide a nitride film having both strength and toughness and good bonding with a-SiO2 film substrate in view of the current state of the prior art.
[0006] The second problem to be solved by the present invention is to provide a method for preparing the high-strength and toughness nitride film of the first aspect.
[0007] The third problem to be solved by the present invention is to provide a resonant sensor using the high-strength and toughness nitride film of the first aspect as an electrode material.
[0008] The fourth problem to be solved by the present invention is to provide a clamping device for testing the clamping force using the resonant sensor of the third aspect.
[0009] To achieve the above objectives, this application adopts the following technical solutions:
[0010] In the first aspect, the present application provides a high-strength and tough nitride film, the composition of which is expressed as (Ti a Al b Nb c Ta d X e )N , wherein a=10-30, b=10-30, c=10-30, d=10-30, e=0-20, |(a+b)-(c+d)| ≤ 15, and a+b+c+d+e=100, X is one or two of Hf, Zr, V, Cr, and Mo. The present invention designs the composition of the thin film system to make the (Ti a Al b Nb c Ta d X e )N system film nanohardness ≥ 20 GPa, toughness H 3 / E 2 Value ≥ 0.15.
[0011] Furthermore, the mismatch between the (2×11×1) supercell on the (200) plane of the film and the (√3R30×8×5) supercell on the (0-58) plane of the a-SiO2 single crystal (i.e., the AT-cut type of a-quartz) is δ ≤ 3%, (Ti a Al b Nb c Ta d X e ) The interface bonding strength of N / a-SiO2 is above 3.5 N. Based on the above performance characteristics, the film can be well bonded to the SiO2 substrate.
[0012] In a second aspect, the present application provides a method for preparing the nitride film according to the first aspect, comprising the following steps:
[0013] S1 Prepare target material: Select target material containing Ti a Al b Nb c Ta d X e Single target with full element composition, where X is one or two of Hf, Zr, V, Cr, and Mo;
[0014] S2: preparing a substrate and a mask: fixing the mask onto the substrate to prepare for sputtering deposition;
[0015] S3 Sputtering deposited thin films:
[0016] S31 Pre-vacuum to 0.8×10 -1 -1.5×10 -1 Pa, and continue to evacuate to 2.0×10 -6 -3.0×10 -6 Pa, a mixed gas of protective gas and N2 is introduced as the working gas, and the ratio of the protective gas and N2 flow rate is adjusted to ensure (Ti a Al b Nb c Ta d X e ) The nitrogen content in the N-nitride system film reaches saturation;
[0017] S32: Turn on the negative bias voltage to clean the substrate; turn off the bias voltage, adjust the sputtering power to 50-100 W, and pre-sputter the target material to remove nitrides and contaminants on the target surface;
[0018] S33 uses RF power or DC pulse power for sputtering, with a sputtering power of 100-800 W and a substrate temperature of 20-550 °C. After sputtering, a deposited (Ti a Al b Nb c Ta d X e )N nitride thin film samples.
[0019] Furthermore, in step S1, the target material may be a plurality of alloy targets containing one or more components of Ti, Al, Nb, Ta, and X, and the size of the target material may be 2 inches, 8 inches, or 10 inches.
[0020] Furthermore, in step S2, the thickness of the substrate is 10 μm-1000 μm, and the material of the substrate can be selected from AT or SC cut single crystal a-SiO2, or the (002) surface of AlN and AlSCN materials for toughening electrode applications.
[0021] Furthermore, in step S2, the substrate is pretreated: first, ultrasonically treated with acetone for 30-50 min, then ultrasonically treated with alcohol for 10-30 min, washed in deionized water, ultrasonically cleaned for 10-30 min, then ultrasonically cleaned in alcohol for 10-30 min, all at a temperature of 20°C, and finally dried in a vacuum drying oven at a temperature of 100-140°C.
[0022] Furthermore, in step S2, the mask can be used for positive or reverse photolithography.
[0023] Furthermore, in step S31, the protective gas is argon gas, and argon ions bombard the target material to cause the target material to sputter; while nitrogen gas is used for reactive sputtering to form a nitride film.
[0024] Furthermore, in step S32, the magnitude of the negative bias voltage is 12-22 V, the cleaning time is 3-10 min, the working gas pressure is 0.5-1 Pa, and the pre-sputtering time is 10-30 min.
[0025] In a third aspect, the present invention provides a resonant sensor, comprising a resonant chip and a chip frame, wherein the resonant chip is a high-strength and tough nitride film of the first aspect described above, and electrode patterns are directly prepared on the upper and lower surfaces of an a-SiO2 substrate using a mask or a photolithography process.
[0026] Furthermore, the resonant chip and the chip frame may be connected by gluing or laser melting.
[0027] In a fourth aspect, the present invention provides a clamping device, comprising a pressure plate and a hydraulic cylinder, wherein the pressure plate applies force to a workpiece under the drive of the hydraulic cylinder to fix the workpiece on a mounting platform, and a sensor mounting groove is provided on the pressure plate, in which the resonant sensor of the third aspect is installed, and the resonant sensor is used to measure the clamping force of the clamping device on the workpiece.
[0028] Furthermore, the first end of the pressing plate is transmission-connected to the output end of the hydraulic cylinder, the second end of the pressing plate applies force to the workpiece, and the sensor mounting groove is arranged at the top position of the pressing plate close to the second end.
[0029] Furthermore, the distance between the force center point of the pressure plate and the center point of the sensor installation groove is between 5-60 mm.
[0030] The beneficial effects of the present invention are:
[0031] 1. In terms of element selection in the film composition, Ti, Al, Nb, and Ta are all strong nitride-forming elements. At the same time, the strength orientations of their nitride chemical bonds are different. The multi-component nitrides formed can achieve complementary advantages of chemical bonds with different strength orientations, thereby achieving the strengthening and toughening of the multi-component nitrides. At the same time, there are differences in the lattice constants of the above-mentioned nitrides. After adjusting the composition, the lattice mismatch between some crystal planes of the multi-component nitrides and the AT-cut of a-SiO2 can be reduced, thereby improving the film-based bonding. In addition, the introduction of the X element can further provide the freedom of composition regulation on the basis of the above advantages, so that the overall strength and toughness of the nitride and the film-based bonding are further optimized;
[0032] 2. The present invention adopts N2 reactive magnetron co-sputtering method to carry out (Ti a Al b Nb c Ta d X e )N thin film preparation, the method is easy to control the composition, the film is relatively uniform, the performance of the equipment is very stable, the repeatability is strong, and it is very suitable for large-scale production; the film performance can be optimized by controlling the sputtering power, substrate bias, substrate temperature and other parameters; the elements are evenly distributed during the magnetron sputtering process, which is very suitable for the preparation of multi-component nitride films;
[0033] 3. The present invention installs the resonant sensor at the top position of the clamping device pressure plate, and uses this position to measure the clamping force to obtain a stable, accurate and highly linear value. BRIEF DESCRIPTION OF THE DRAWINGS
[0034] Figure 1 According to Example 1 of the present application, it is shown that (Ti 19 Al 18 Nb 23 Ta 22 V 18 ) Surface SEM morphology of N film;
[0035] Figure 2 According to Example 1 of the present application, it is shown that (Ti 19 Al 18 Nb 23 Ta 22 V 18 )TEM morphology of the interface between N thin film electrode and a-SiO2 substrate;
[0036] Figure 3 According to Example 1 of the present application, it is shown that (Ti 19 Al 18 Nb 23 Ta 22 V 18 )N nanoindentation loading and unloading curves of thin film electrode;
[0037] Figure 4 According to Example 1 of the present application, it is shown that (Ti 19 Al 18 Nb 23 Ta 22 V 18 ) Scratch test results of N thin film electrode;
[0038] Figure 5 According to the embodiments and comparative examples of the present application, a schematic structural diagram of a chip body prepared is shown;
[0039] Figure 6 According to the embodiments and comparative examples of the present application, a schematic structural diagram of a prepared resonant sensor is shown;
[0040] Figure 7 Shows Figure 6 Sectional view of section AA;
[0041] Figure 8 Shows Figure 6 A schematic diagram of the coordination structure of the first frame, the second frame and the resonant chip;
[0042] Fig. 9 Shows Figure 6 Schematic diagram of the structure of the upper and lower surfaces of the resonant chip;
[0043] Fig.10 According to the embodiments and comparative examples of the present application, a schematic structural diagram of a clamping device is shown;
[0044] Fig.11 According to Example 1 of the present application, a graph of force-frequency test results of a clamping device equipped with a resonant sensor is shown;
[0045] In the figure, 100, clamping device; 101, pressure plate; 102, fastener; 103, hydraulic cylinder; 104, pressure hole; 105, sensor mounting groove; 200, resonant sensor; 210, chip frame; 211, first frame; 211a, chip slot; 212, second frame; 220, resonant chip; 221, chip body; 221a, SiO2 substrate; 221b, (Ti a Al b Nb c Ta d X e )N film; 222, a first electrode; 223, a second electrode; 231, a first adhesive area; 232, a second adhesive area. DETAILED DESCRIPTION
[0046] The following is a more detailed description of the technical features and advantages of the present application in combination with embodiments, comparative examples and drawings, so that the advantages and features of the present application can be more easily understood by those skilled in the art, thereby making a clearer and more definite definition of the protection scope of the present invention. Example 1
[0047] S1. Prepare the target: select a 4-inch alloy target containing five elements: Ti, Al, Nb, Ta, and V. The TiAlNbTaV alloy target contains five elements: Ti, Al, Nb, Ta, and V, and the atomic ratio is Ti:Al:Nb:Ta:V=19:18:23:22:18 at.%. The target has a diameter of 4 inches and a thickness of 3 mm.
[0048] S2: Prepare substrate: In this embodiment, AT-cut single crystal SiO2 is used as the substrate, the substrate thickness is 100 μm, and it is covered with an organic mask;
[0049] S3 Sputtering (Ti a Al b Nb c Ta d X e )N Thin Film Electrode Chip:
[0050] S31 Close the vacuum chamber of the magnetron sputtering equipment, turn on the mechanical pump, and start the pre-vacuum state of the vacuum chamber. Wait until the pressure reaches 1.0×10 -1 Pa, open the molecular pump and the plug valve, and further evacuate the air pressure to 2.5×10 -6 Pa, based on the goal of preparing a nitride film in an embodiment of the present invention, a mixed working gas of argon and nitrogen is introduced, and the argon flow rate is set to 20 sccm, and the nitrogen flow rate is set to 40 sccm, that is, Ar:N2=1:2 in the working gas.
[0051] S32 Close the sample stage valve and evaporation source valve, turn on the 15V substrate negative bias, clean the substrate, turn off the bias, adjust the sputtering power to 100 W, pre-sputter the target for 20 minutes to remove the nitride on the target surface;
[0052] S33 The sample stage was continuously rotated, and the sample stage valve and evaporation valve were opened for sputtering. The sputtering power was 300 W, the substrate temperature was 27 °C, and the sputtering time was 1400 s. After the sputtering was completed, the chip sample with the nitride thin film electrode was taken out. The upper and lower surfaces of the chip sample were both deposited with 300 nm thick (Ti a Al b Nb c Ta d X e )N film. See Figure 5 , is a cross-sectional view of the chip body 221 obtained by the preparation, and 300 nm thick (Ti) is deposited on the upper and lower surfaces of the SiO2 substrate 221a respectively. a Al b Nb c Ta d X e )N film 221b, forming the chip body 221.
[0053] S4 Sensor preparation: Use an adhesive method to connect the chip body 221 prepared in S3 and the chip frame to make a resonant sensor 200. Figure 6-9, is a schematic diagram of the structure of the resonant sensor 200, which includes a chip frame 210 and a resonant chip 220, and the chip frame 210 is arranged around the periphery of the resonant chip 220. The first electrode 222 and the second electrode 223 are respectively arranged on the upper and lower surfaces of the chip body 221 prepared in step S3 to form the resonant chip 220, and then the resonant chip 220 is installed in the chip frame 210 by gluing to form the resonant sensor 200. Specifically, the chip frame 210 includes a first frame 211 and a second frame 212, and the first frame 211 / the second frame 212 are respectively provided with a chip card slot 211a, and the resonant chip 220 is clamped in the above-mentioned chip card slot 211a, and then fixed by the first adhesive area 231, and then the first frame 211 is covered on the second frame 212, and fixed by the second adhesive area 232. When the first electrode 222 and the second electrode 223 of the resonant chip 220 are connected to the oscillation circuit, the chip body 221 generates a fixed resonant fundamental frequency due to the inverse piezoelectric effect. When an external force acts on the chip frame 210, the stress will be further transmitted to the chip body 221, causing its vibration frequency to change. The external force value can be derived according to the force-frequency change relationship, thereby realizing the external force perception test;
[0054] S5 sensor installation: Fig.10The resonant sensor 200 prepared by S4 is installed on the clamping device 100 shown. The clamping device 100 specifically includes two parts: a pressure plate 101 and a hydraulic cylinder 103. The first end of the pressure plate 101 can be connected to the output end of the hydraulic cylinder 103 through a fastener 102. The second end of the pressure plate 101 directly applies force to the workpiece. The pressure plate 101 is driven by the hydraulic cylinder 103 to pressurize the workpiece to achieve the clamping and fixing of the workpiece. In some embodiments, a pressure hole 104 can be opened at the second end of the pressure plate 101, and a pressure head (not shown in the figure) can be detachably installed in the pressure hole 104. The pressure head is used to clamp the workpiece. The detachable installation method can replace the pressure head when it is worn out; illustratively, the pressure head can be installed in the pressure hole 104 by threaded connection. A sensor mounting groove 105 is provided at the top of the second end of the pressing plate 101 near the pressure hole 104, and the resonant sensor 200 prepared in the above S4 is installed in the sensor mounting groove 105. The shape of the sensor mounting groove 105 matches the shape of the chip frame 210, and the chip frame 210 of the resonant sensor and the sensor mounting groove 105 can be fixedly connected by gluing or welding. When the hydraulic cylinder 103 is working, it drives the pressing plate 101 to press down and applies force to the workpiece through the pressure head. At the same time, the pressing plate 101 will be deformed due to the upward reaction force of the workpiece and further act on the resonant sensor 200, and the resonant sensor 200 will then output the corresponding clamping force value to realize pressure perception. In order to ensure the accuracy of the clamping force detection, the distance between the force center point of the pressing plate 101 and the center point of the sensor mounting groove 105 is between 5-60 mm. In this embodiment, the distance X between the center point of the sensor installation groove 105 and the center point of the pressure hole 104 (ie, the force center point of the pressure plate 101 ) is between 30 mm.
[0055] The preparation methods of Examples 2 and 3 are basically the same as those of Example 1, except that the target material composition or ratio is different. The atomic ratio of Example 2 is Ti:Al:Nb:Ta:V=18:17:21:21:23 at.%; and the atomic ratio of Example 3 is Ti:Al:Nb:Ta:Zr=22:21:24:23:10 at.%.
[0056] Example 4
[0057] S1. Prepare the target: select two alloy targets of equal atomic ratio TiAl alloy and equal atomic ratio NbTa alloy, both of which are 4 inches and 3 mm thick.
[0058] S2: Prepare substrate: In this embodiment, an AT-cut single crystal SiO2 substrate with a thickness of 100 μm and covered with an organic mask is selected;
[0059] S3 Sputtering (Ti a Al b Nb c Ta d X e )N thin film electrode:
[0060] S31 Close the vacuum chamber of the magnetron sputtering equipment, turn on the mechanical pump, and start the pre-vacuum state of the vacuum chamber. Wait until the pressure reaches 1.0×10 -1 Pa, open the molecular pump and the plug valve, and further evacuate the air pressure to 2.5×10 -6 Pa, based on the goal of preparing a nitride film in an embodiment of the present invention, a mixed working gas of argon and nitrogen is introduced, and the argon flow rate is set to 20 sccm, and the nitrogen flow rate is set to 40 sccm, that is, Ar:N2=1:2 in the working gas.
[0061] S32 Close the sample stage valve and the evaporation source valve, turn on the 15V substrate negative bias, clean the substrate, turn off the bias, adjust the sputtering power of the two targets to 100 W, pre-sputter the targets for 20 minutes to remove the nitride on the target surface;
[0062] S33: Continue to rotate the sample stage, open the sample stage valve and the evaporation valve for sputtering, adjust the sputtering power of the two targets to 300 W, the substrate temperature to 27 °C, the sputtering time to 1400 s, and perform reactive co-sputtering. After the sputtering is completed, take out the chip sample with the nitride thin film electrode deposited thereon.
[0063] S4 Sensor preparation: Use the gluing method to connect the chip sample prepared in S3 to the chip frame to make a resonant sensor. Figure 5 As shown;
[0064] S5 sensor installation location: Fig.10 The resonant sensor prepared by S4 is installed on the clamping device shown, and the distance from the center point of the sensor installation groove 105 to the center point of the top pressure hole 104 is 30 mm. Example 5
[0065] S1 Prepare the target materials: select two alloy targets of TiAl alloy with equal atomic ratio and NbTa alloy with equal atomic ratio, and select one Cr target. All three targets are 4 inches in size and 3 mm in thickness.
[0066] S2: Prepare substrate: In this embodiment, an AT-cut single crystal SiO2 substrate with a thickness of 100 μm and covered with an organic mask is selected;
[0067] S3 Sputtering (Ti a Al b Nb c Tad X e )N thin film electrode:
[0068] S31 Close the vacuum chamber of the magnetron sputtering equipment, turn on the mechanical pump, and start the pre-vacuum state of the vacuum chamber. Wait until the pressure reaches 1.0×10 -1 Pa, open the molecular pump and the plug valve, and further evacuate the air pressure to 2.5×10 -6 Pa, based on the goal of preparing a nitride film in an embodiment of the present invention, a mixed working gas of argon and nitrogen is introduced, and the argon flow rate is set to 20 sccm, and the nitrogen flow rate is set to 40 sccm, that is, Ar:N2=1:2 in the working gas.
[0069] S32 Close the sample stage valve and the evaporation source valve, turn on the 15V substrate negative bias, clean the substrate, turn off the bias, adjust the sputtering power of the three targets to 100 W, pre-sputter the targets for 20 minutes to remove the nitride on the target surface;
[0070] S33: Continue to rotate the sample stage, open the sample stage valve and the evaporation valve for sputtering, adjust the sputtering power of the TiAl alloy target and the NbTa alloy target to 300 W, adjust the power of the Cr target to 100 W, set the substrate temperature to 27 °C, and the sputtering time to 1400 s for reactive co-sputtering. After the sputtering is completed, take out the chip sample with the nitride thin film electrode deposited thereon.
[0071] S4 Sensor preparation: Use the gluing method to connect the chip prepared in S3 and the frame to make a resonant sensor. Its structure is as shown in the attached figure. Figure 5 As shown;
[0072] S5 sensor installation location: Fig.10 The resonant sensor prepared by S4 is installed on the clamping device shown, and the distance from the center point of the sensor installation groove 105 to the center point of the top pressure hole 104 is 30 mm. Example 6
[0073] S1 Prepare the target: select two alloy targets of equal atomic ratio TiAl alloy and equal atomic ratio NbTa alloy, and select one V target. All three targets have a diameter of 4 inches and a thickness of 3 mm.
[0074] S2: Prepare substrate: In this embodiment, an AT-cut single crystal SiO2 substrate with a thickness of 100 μm and covered with an organic mask is selected;
[0075] S3 Sputtering (Ti a Al b Nb c Ta d X e)N thin film electrode:
[0076] S31 Close the vacuum chamber of the magnetron sputtering equipment, turn on the mechanical pump, and start the pre-vacuum state of the vacuum chamber. Wait until the pressure reaches 1.0×10 -1 Pa, open the molecular pump and the plug valve, and further evacuate the air pressure to 2.5×10 -6 Pa, based on the goal of preparing a nitride film in an embodiment of the present invention, a mixed working gas of argon and nitrogen is introduced, and the argon flow rate is set to 20 sccm, and the nitrogen flow rate is set to 40 sccm, that is, Ar:N2=1:2 in the working gas.
[0077] S32 Close the sample stage valve and the evaporation source valve, turn on the 15V substrate negative bias, clean the substrate, turn off the bias, adjust the sputtering power of the three targets to 100 W, pre-sputter the targets for 20 minutes to remove the nitride on the target surface;
[0078] S33: Continue to rotate the sample stage, open the sample stage valve and the evaporation valve for sputtering, adjust the sputtering power of the TiAl alloy target to 300 W, the sputtering power of the NbTa alloy target to 200 W, and the sputtering power of the V target to 200 W. The substrate temperature is 27 °C, the sputtering time is 1400 s, and reactive co-sputtering is performed. After the sputtering is completed, take out the chip sample with the nitride thin film electrode deposited thereon.
[0079] S4 Sensor preparation: Use the gluing method to connect the chip sample prepared in S3 to the frame to make a resonant sensor. Figure 5 As shown;
[0080] S5 sensor installation location: Fig.10 The resonant sensor prepared by S4 is installed on the clamping device shown, and the distance from the center point of the sensor installation groove 105 to the center point of the top pressure hole 104 is 30 mm.
[0081] Comparative Example 1
[0082] S1 Prepare the target: select two alloy targets of equal atomic ratio TiAl alloy and equal atomic ratio NbTa alloy, and select one V target. All three targets have a diameter of 4 inches and a thickness of 3 mm.
[0083] S2: Prepare substrate: In this embodiment, an AT-cut single crystal SiO2 substrate with a thickness of 100 μm and covered with an organic mask is selected;
[0084] S3 Sputtering (Ti a Al b Nb c Ta d X e)N thin film electrode:
[0085] S31 Close the vacuum chamber of the magnetron sputtering equipment, turn on the mechanical pump, and start the pre-vacuum state of the vacuum chamber. Wait until the pressure reaches 1.0×10 -1 Pa, open the molecular pump and the plug valve, and further evacuate the air pressure to 2.5×10 -6 Pa, based on the purpose of preparing a nitride film of the present invention, a mixed working gas of argon and nitrogen is introduced, and the argon flow rate is set to 20 sccm, and the nitrogen flow rate is set to 40 sccm, that is, Ar:N2=1:2 in the working gas.
[0086] S32 Close the sample stage valve and the evaporation source valve, turn on the 15V substrate negative bias, clean the substrate, turn off the bias, adjust the sputtering power of the three targets to 100 W, pre-sputter the targets for 20 minutes to remove the nitride on the target surface;
[0087] S33: Continue to rotate the sample stage, open the sample stage valve and the evaporation valve for sputtering, adjust the sputtering power of the TiAl alloy target to 300 W, the sputtering power of the NbTa alloy target to 200 W, and the sputtering power of the V target to 300 W. The substrate temperature is 27 °C, the sputtering time is 1400 s, and reactive co-sputtering is performed. After the sputtering is completed, take out the chip sample with the nitride thin film electrode deposited.
[0088] S4 Sensor preparation: Use the gluing method to connect the chip sample prepared in S3 to the frame to make a resonant sensor. Figure 5 As shown;
[0089] S5 sensor installation location: Fig.10 The resonant sensor prepared by S4 is installed on the clamping device shown, and the distance from the center point of the sensor installation groove 105 to the center point of the top pressure hole 104 is 30 mm.
[0090] The preparation parameters of Comparative Example 2 are the same as those of Example 1, except that the distance from the center point of the sensor mounting groove 105 to the center point of the top pressure hole 104 is located at 70 mm.
[0091] Table 1 lists the composition, preparation parameters and performance data of the film samples prepared in various embodiments and comparative examples.
[0092] Table 1 Preparation parameters and performance data of each group of samples
[0093] Sample No. <![CDATA[(Ti a Al b Nb c Ta d X e )N x ]]> <![CDATA[Ar:N2]]> Nanohardness (GPa) Mismatch (%) Membrane-substrate bonding strength (N) Installation position (mm) Force frequency linearity (%) Example 1 <h2 style=";text-align:left;direction:ltr"><![CDATA[(Ti <h2 style=";text-align:left;direction:ltr"> 19 <h2 style=";text-align:left;direction:ltr"> Al<h2 style=";text-align:left;direction:ltr"> 18 <h2 style=";text-align:left;direction:ltr"> Nb<h2 style=";text-align:left;direction:ltr"> 23 <h2 style=";text-align:left;direction:ltr"> Ta<h2 style=";text-align:left;direction:ltr"> 22 <h2 style=";text-align:left;direction:ltr"> V<h2 style=";text-align:left;direction:ltr"> 18 <h2 style=";text-align:left;direction:ltr"> )N]]><h2 style=";text-align:left;direction:ltr"> 1:2 33.07 1.71 3.85 30 99.85 Example 2 <h2 style=";text-align:left;direction:ltr"><![CDATA[(Ti <h2 style=";text-align:left;direction:ltr"> 18 <h2 style=";text-align:left;direction:ltr"> Al<h2 style=";text-align:left;direction:ltr"> 17 <h2 style=";text-align:left;direction:ltr"> Nb<h2 style=";text-align:left;direction:ltr"> 21 <h2 style=";text-align:left;direction:ltr"> Ta<h2 style=";text-align:left;direction:ltr"> 21 <h2 style=";text-align:left;direction:ltr"> V<h2 style=";text-align:left;direction:ltr"> 23 <h2 style=";text-align:left;direction:ltr"> )N]]><h2 style=";text-align:left;direction:ltr"> 1:2 29.44 2.39 3.65 30 99.30 Example 3 <h2 style=";text-align:left;direction:ltr"><![CDATA[(Ti <h2 style=";text-align:left;direction:ltr"> 22 <h2 style=";text-align:left;direction:ltr"> Al<h2 style=";text-align:left;direction:ltr"> 21 <h2 style=";text-align:left;direction:ltr"> Nb<h2 style=";text-align:left;direction:ltr"> 24 <h2 style=";text-align:left;direction:ltr"> Ta<h2 style=";text-align:left;direction:ltr"> 23 <h2 style=";text-align:left;direction:ltr"> Zr<h2 style=";text-align:left;direction:ltr"> 10 <h2 style=";text-align:left;direction:ltr"> )N]]><h2 style=";text-align:left;direction:ltr"> 1:2 32.51 1.56 3.78 30 99.62 Example 4 <h2 style=";text-align:left;direction:ltr"><![CDATA[(Ti <h2 style=";text-align:left;direction:ltr"> 24 <h2 style=";text-align:left;direction:ltr"> Al<h2 style=";text-align:left;direction:ltr"> 23 <h2 style=";text-align:left;direction:ltr"> Nb<h2 style=";text-align:left;direction:ltr"> 26 <h2 style=";text-align:left;direction:ltr"> Ta<h2 style=";text-align:left;direction:ltr"> 27 <h2 style=";text-align:left;direction:ltr"> )N]]><h2 style=";text-align:left;direction:ltr"> 1:2 29.07 2.15 3.66 30 99.32 Example 5 <h2 style=";text-align:left;direction:ltr"><![CDATA[(Ti <h2 style=";text-align:left;direction:ltr"> 22 <h2 style=";text-align:left;direction:ltr"> Al<h2 style=";text-align:left;direction:ltr"> 21 <h2 style=";text-align:left;direction:ltr"> Nb<h2 style=";text-align:left;direction:ltr"> 24 <h2 style=";text-align:left;direction:ltr"> Ta<h2 style=";text-align:left;direction:ltr"> 25 <h2 style=";text-align:left;direction:ltr"> Cr8)N]]><h2 style=";text-align:left;direction:ltr"> 1:2 30.15 2.42 3.64 30 99.18 Example 6 <h2 style=";text-align:left;direction:ltr"><![CDATA[(Ti <h2 style=";text-align:left;direction:ltr"> 22 <h2 style=";text-align:left;direction:ltr"> Al<h2 style=";text-align:left;direction:ltr"> 23 <h2 style=";text-align:left;direction:ltr"> Nb<h2 style=";text-align:left;direction:ltr"> 16 <h2 style=";text-align:left;direction:ltr"> Ta<h2 style=";text-align:left;direction:ltr"> 15 <h2 style=";text-align:left;direction:ltr"> V<h2 style=";text-align:left;direction:ltr"> 24 <h2 style=";text-align:left;direction:ltr"> )N]]><h2 style=";text-align:left;direction:ltr"> 1:2 28.73 2.93 3.54 30 99.06 Comparative Example 1 <h2 style=";text-align:left;direction:ltr"><![CDATA[(Ti <h2 style=";text-align:left;direction:ltr"> 19 <h2 style=";text-align:left;direction:ltr"> Al<h2 style=";text-align:left;direction:ltr"> 19 <h2 style=";text-align:left;direction:ltr"> Nb<h2 style=";text-align:left;direction:ltr"> 15 <h2 style=";text-align:left;direction:ltr"> Ta<h2 style=";text-align:left;direction:ltr"> 17 <h2 style=";text-align:left;direction:ltr"> V<h2 style=";text-align:left;direction:ltr"> 30 <h2 style=";text-align:left;direction:ltr"> )N]]><h2 style=";text-align:left;direction:ltr"> 1:2 27.18 3.42 2.93 30 98.51 Comparative Example 2 <h2 style=";text-align:left;direction:ltr"><![CDATA[(Ti <h2 style=";text-align:left;direction:ltr"> 19 <h2 style=";text-align:left;direction:ltr"> Al<h2 style=";text-align:left;direction:ltr"> 18 <h2 style=";text-align:left;direction:ltr"> Nb<h2 style=";text-align:left;direction:ltr"> 23 <h2 style=";text-align:left;direction:ltr"> Ta<h2 style=";text-align:left;direction:ltr"> 22 <h2 style=";text-align:left;direction:ltr"> V<h2 style=";text-align:left;direction:ltr"> 18 <h2 style=";text-align:left;direction:ltr"> )N]]><h2 style=";text-align:left;direction:ltr"> 1:2 33.07 1.71 3.85 70 97.24
[0094] Take Example 1 as an example, please refer to Figure 1 , for the preparation of (Ti 19 Al18 Nb 23 Ta 22 V 18 )Surface SEM morphology of N thin film electrode. The surface micromorphology of the thin film electrode was observed using a field emission scanning electron microscope (FE-SEM, S-4800, HITACHI, Tokyo, Japan).
[0095] The target materials and thin film elemental compositions in all the embodiments and comparative examples were quantitatively characterized using a Phenom ProX electron microscope energy spectrometer.
[0096] The Ti 19 Al 18 Nb 23 Ta 22 V 18 ) The interface morphology between N and a-SiO2, such as Figure 2 As shown, the interface is relatively flat, which reflects good interface bonding to a certain extent.
[0097] The lattice mismatch in each embodiment and comparative example is calculated based on the first principle (Ti a Al b Nb c Ta d X e )N thin film stable lattice values and a-SiO2 lattice values are calculated.
[0098] The mechanical properties of the thin film electrodes in the examples and comparative examples were tested using a nanoindentation device (MTS G200), wherein the loading and unloading curves of the thin film in Example 1 are as follows: Figure 3 As shown, its nanohardness can be calculated to be 33.07 GPa, and its H 3 / E 2 The value is 0.0325.
[0099] The membrane-substrate bonding strength of the thin film electrodes in the examples and comparative examples was tested using a scratch tester (CSM Revetest), wherein the results in Example 1 are as follows: Figure 4 As shown, the membrane-base bonding strength can be measured to be 3.85N.
[0100] The structural diagram of the resonant sensor is shown in Figure 5 As shown, the resonant sensors in the embodiments and comparative examples are prepared according to this structure.
[0101] The schematic diagram of the installation position of the resonant sensor in the embodiment and the comparative example on the clamping device pressure plate is as follows: Figure 6 shown.
[0102] The frequency acquisition was performed using a frequency-counting power supply when the clamping device in all the comparative examples was loaded, wherein the force-frequency curve results in Example 1 are as follows: Fig.11 As shown, its force-frequency linearity reaches 99.85%.
[0103] The above descriptions are merely embodiments of the present application and are not intended to limit the patent scope of the present application. Any equivalent structure or equivalent process transformation made using the contents of the present invention specification and drawings, or directly or indirectly applied in other related technical fields, are also included in the patent protection scope of the present application.
Claims
1. A high-strength and tough nitride film, characterized in that: The composition expression of the film is: (Ti a Al b Nb c Ta d X e )N, wherein a=10-30, b=10-30, c=10-30, d=10-30, e=0-20, |(a+b)-(c+d)| ≤ 15, and a+b+c+d+e=100, X is one or two of V, Hf, Zr, Cr, Mo; the film has a nanohardness ≥20 GPa and a toughness H 3 / E 2 Value ≥ 0.15; The mismatch between the (2×11×1) supercell on the (200) plane and the (√3R30×8×5) supercell on the (0-5 8) plane of the a-SiO2 single crystal is δ ≤3%. a Al b Nb c Ta d X e )The interface bonding strength of N / a-SiO2 is above 3.5N.
2. The method for preparing a high-strength and tough nitride film according to claim 1, characterized in that: The following steps are involved: S1 Prepare target material: Select target material containing Ti a Al b Nb c Ta d X e Single target with full element composition; S2: preparing a substrate and a mask: fixing the mask onto the substrate to prepare for sputtering deposition; S3 Sputtering deposition of thin film: Use RF power or DC pulse power to perform alloy target N2 reactive sputtering or co-sputtering to prepare thin film, the sputtering power is 100-800 W, and after sputtering, the deposited (Ti a Al b Nb c Ta d X e )N nitride thin film samples.
3. The method for preparing a high-strength and tough nitride film according to claim 2, characterized in that: In step S3, a single target containing all-component alloys is selected for N2 reactive sputtering, or multiple targets containing one or more components are used for N2 reactive co-sputtering.
4. The method for preparing a high-strength and tough nitride film according to claim 2, characterized in that: In step S2, the thickness of the substrate is 10 μm-1000 μm, and the material of the substrate is a-SiO2 single crystal AT cut, or a-SiO2 single crystal SC cut with a mismatch adjusted within a composition range to within 3.5%, or (002) surface of AlN and AlSCN materials based on toughened electrode applications within a composition range.
5. A resonant sensor, comprising a resonant chip and a chip frame, characterized in that: The high-strength and toughness nitride film according to claim 1 is directly deposited on the upper and lower surfaces of the SiO2 substrate using a mask or a photolithography process to prepare electrode patterns to form the resonant chip.
6. The resonant sensor according to claim 5, characterized in that: The resonant chip and the chip frame are connected by gluing or laser melting.
7. A clamping device, comprising a pressing plate and a hydraulic cylinder, wherein the pressing plate applies force to a workpiece under the drive of the hydraulic cylinder to fix the workpiece on a mounting platform, characterized in that: The pressing plate is provided with a sensor installation groove, in which a resonant sensor as claimed in any one of claims 5 to 6 is installed, and the resonant sensor is used to measure the clamping force of the clamping device on the workpiece.
8. The clamping device according to claim 7, characterized in that: The first end of the pressing plate is transmission-connected to the output end of the hydraulic cylinder, the second end of the pressing plate applies force to the workpiece, and the sensor mounting groove is arranged at the top position of the pressing plate close to the second end.
9. The clamping device according to claim 8, characterized in that: The distance between the force center point of the pressure plate and the center point of the sensor installation slot is between 5-60 mm.
Citation Information
Patent Citations
Piezoelectric thin film, piezoelectric material, and fabrication method of piezoelectric thin film and piezoelectric material, and piezoelectric resonator
CN101325240A
TiAlMoNbW high-entropy alloy nitride film and preparation process thereof
CN114645254A
High-entropy alloy electrode, preparation method, gas sensor and application thereof
CN117468060A
Method for optimizing superconducting transition temperature of NbN film on Si substrate at room temperature and application thereof
CN117684125A
TiAlNbTaV high-entropy alloy target material as well as preparation method and application thereof
CN118048570A