A method for reducing the wear rate of foot roller by using alloy powder and thermal processing technology

The laser cladding process using alloy powder to form a self-lubricating film on the surface of the foot roller has solved the problem of high wear rate of foot rollers in continuous casting production lines of steel plants, significantly extending service life and reducing costs.

CN118756136BActive Publication Date: 2024-11-05长沙瑞华新材料科技有限公司
View PDF 0 Cites 0 Cited by

Patent Information

Application Number
CN202411207830.1
Authority / Receiving Office
CN · China
Patent Type
Patents(China)
Current Assignee / Owner
Filing Date
2024-08-30
Publication Date
2024-11-05
Estimated Expiration
2044-08-30

AI Technical Summary

Technical Problem

Existing technologies are insufficient to effectively reduce the wear rate of foot rollers in continuous casting production lines of steel plants, resulting in short service life and affecting the dimensional accuracy and safety of steel billets.

Method used

By using alloy powder and hot processing technology, a self-lubricating film is formed on the surface of the foot roller through laser cladding, which reduces friction and thus reduces wear rate.

Benefits of technology

The laser cladding layer has a diameter reduction of only 0.35~0.42 mm within 39 days, a wear rate of 1/3~1/2 of the existing technology, a cost of 3/4~4/5 of the welding wire cost, a cladding efficiency of 1.5~2.1 times that of the existing technology, and no straightening and internal hole repair processes are required.

✦ Generated by Eureka AI based on patent content.

Smart Images

  • Figure CN118756136B_ABST
    Figure CN118756136B_ABST
Patent Text Reader

Abstract

The invention discloses a method for reducing the wear rate of a foot roller by utilizing alloy powder and a heat treatment process, and relates to the technical field of foot roller optimization of a continuous casting production line in a steel plant. Specifically, a thin film is formed on the surface of a workpiece by a special phase in a cladding layer, and the self-lubricating ability of the thin film is used to reduce the friction force, thereby reducing the wear rate of the foot roller. The alloy powder used comprises the following components: C: 0.08-0.10wt%; Cr: 13.0-13.3wt%; Ni: 2.4-2.7wt%; Mo: 1.2-1.4wt%; Mn0.7-0.9wt%; Cu: 8.4-8.5wt%; Sn: 1.1-1.2wt%; Nb: 0.14-0.16wt%; B: 0.6-1.0wt%; Si: 0.7-0.8wt%; P: 0.1-0.2wt%; and Fe is the remainder. The invention combines laser cladding technology with heat treatment technology, which not only improves the service life of the foot roller of the continuous casting production line, but also saves consumables and reduces processing procedures.
Need to check novelty before this filing date? Find Prior Art

Description

Technical Field

[0001] The invention relates to the technical field of foot roller optimization for a continuous casting production line in a steel plant, and specifically to a method for reducing the wear rate of a foot roller by utilizing alloy powder and a thermal processing process. Background Art

[0002] The foot roller is an indispensable and important mechanical component of the continuous casting production line of the steel plant. It is located below the crystallizer of the steel plant. The temperature of the steel billet it contacts is as high as 1300~1500 degrees Celsius. Although the inner hole and outer cylindrical surface of the foot roller are cooled by water in real time, due to the high contact temperature and the influence of the bulging force, the service life of the foot roller of the continuous casting production line is only between 7 and 30 days. The main reasons for the failure of the foot roller are wear and cracks. Wear will cause dimensional deviation of the steel billet, and cracks will cause the risk of water leakage and breakage of the foot roller. For the alloy layer represented by 414N material, improving its wear resistance will inevitably deteriorate its cold and hot fatigue ability, that is, aggravate the tendency of cracking. Therefore, the development of wear-reducing materials that meet the working conditions of the foot roller is imminent. Unlike wear-resistant materials, wear-reducing materials are not based on wear-resistant elements or elements that increase hardness, and do not sacrifice cold and hot fatigue and toughness. It is to increase self-lubrication and reduce friction to reduce wear. In addition, since the diameter of the foot roller is less than 150 mm and the wall thickness is between 10 and 20 mm, the laser cladding technology with low dilution rate and small thermal deformation is more suitable for strengthening and repairing the surface of the foot roller than the existing open arc welding and submerged arc welding technologies.

[0003] The Chinese patent with patent number CN109967913B discloses a flux-cored welding wire for laser cladding of continuous casting rollers. The laser cladding strengthening material used in this invention patent is a stainless steel flux-cored welding wire, which does not contain the self-lubricating and anti-friction components such as Cu, Sn, Mo, and P described in the patent application of the present invention, nor does it describe the reduction of wear rate, and there is no related heat treatment process. Therefore, this invention patent is inconsistent with the direction described in the patent of the present invention. The Chinese patent with patent number CN116713637B discloses a flux-cored welding wire for surfacing and adding materials to the continuous casting rollers of the fan-shaped segments. The composition of the flux-cored welding wire is 1Cr13Ni3Mo1NbVTiN, and its composition is characterized by the combination of micro-alloy elements Nb, V, Ti and Mo, N elements. Its main purpose is to increase the anti-tempering stability, high temperature wear resistance and cold and hot fatigue resistance of the continuous casting rollers of the fan-shaped segments, and the patent does not mention the consideration of friction reduction.

[0004] In addition, Chinese patents CN110539101A and CN109014654B respectively disclose an open arc self-shielded flux-cored welding wire for surfacing of continuous casting machine sector-shaped continuous casting rollers and a submerged arc surfacing flux-cored solder and process for composite (re)manufacturing of continuous casting rollers. The alloy compositions provided in the above two patents are mainly for solving surfacing forming, and there is no mention of reducing the wear rate.

[0005] Therefore, based on the above problems, we need a method to reduce the wear rate of the foot roller by using alloy powder and hot working process. Summary of the invention

[0006] The purpose of the present invention is to provide a method for reducing the wear rate of the foot roller by using alloy powder and hot processing technology, forming a thin film on the surface of the workpiece through the special phase in the cladding layer, and using the self-lubricating ability of the film to achieve the purpose of reducing friction, thereby reducing the wear rate of the foot roller, so as to solve the problems raised in the above background technology.

[0007] To achieve the above object, the present invention provides the following technical solutions:

[0008] A method for reducing the wear rate of a foot roller by using alloy powder and a thermal processing process comprises the following steps:

[0009] Step 1: performing laser cladding operation on the surface of the substrate of the foot roller, the laser cladding hot processing process material includes alloy powder, and the composition of the alloy powder is: C: 0.08~0.10wt%, Cr: 13.0~13.3wt%, Ni: 2.4~2.7wt%, Mo: 1.2~1.4wt%, Mn: 0.7~0.9wt%, Cu: 8.4~8.5wt%, Sn: 1.1~1.2wt%, Nb: 0.14~0.16wt%, B: 0.6~1.0wt%, Si: 0.7~0.8wt%, P: 0.1~0.2wt%, and Fe is the balance;

[0010] Step 2: Place the foot roller workpiece after laser cladding in a 1180~1195℃ resistance furnace, keep it warm for 100~120min, and then take it out of the furnace and air cool it to room temperature;

[0011] Step 3: Then place the workpiece back in the resistance furnace, heat it to 280~310℃ at a heating rate of 2.7~3.2℃ / min, keep it warm for 235~255min, and finally cool it to room temperature. The hardness of the cladding layer after heat treatment is between 38~43HRC, which is the qualified standard.

[0012] As a further solution of the present invention: the parameters of the laser cladding operation include: selecting a fiber laser with a power of 3500~4000w and a power density of 218~250w / mm 2 , linear speed is 22~24mm / s.

[0013] As a further solution of the present invention: in the step 1, laser cladding operation is performed on the substrate surface of the foot roller in a continuous spiral overlapping manner.

[0014] As a further solution of the present invention: the overlapping rate of the continuous spiral overlap is 50% to 55% in the length direction of the light spot.

[0015] As a further solution of the present invention: the single-side thickness of the laser cladding is 1.8-2.2 mm.

[0016] Compared with the prior art, the beneficial effects of the present invention are as follows: the present invention forms a thin film on the surface of the workpiece through the special phase in the cladding layer, and uses the self-lubricating ability of the thin film to achieve the purpose of reducing friction, thereby reducing the wear rate of the foot roller. After the surface of the foot roller of the continuous casting production line is processed according to the alloy powder and hot processing technology provided by the present invention, the diameter reduction is only 0.35~0.42 mm after 39 days of operation, and the wear rate of the workpiece with the same specification is 1 / 3~1 / 2 of the existing open arc welding technology. Laser cladding can achieve the expected effect in a single single-side two-mm case, without the primer and transition layer of the prior art, the consumables cost is 3 / 4~4 / 5 of the welding wire cost, and the cladding efficiency is 1.5~2.1 times that of the prior art; the thermal deformation of laser cladding is small, and there is no straightening and inner hole repair process of the prior art, and the comprehensive cost is 0.81~0.94 times that of the prior art. BRIEF DESCRIPTION OF THE DRAWINGS

[0017] Figure 1 This is a physical picture of the surface state of the foot roller when it is 39 days online according to Example 2 provided by the present invention;

[0018] Figure 2 This is a physical picture of the surface state of the foot roller 39 days after it was put into production based on the processing technology of open arc welding. The arrows show the worn lines;

[0019] Figure 3 The binary alloy phase diagram calculated by JMATPRO software according to Example 2 provided by the present invention; wherein, LIQUID: liquid phase; FERRITE: ferrite phase; AUSTENNITE: austenite phase; M (C, N): carbonitride phase; CU: copper phase; M23C6: carbide phase; LAVES: Laves phase (intermetallic compound phase); G_PHASE: G phase (intermetallic compound phase);

[0020] Figure 4 A schematic diagram of heat treatment drawn according to the heat treatment system route provided by the patent of this invention. DETAILED DESCRIPTION

[0021] The following will be combined with the drawings in the embodiments of the present invention to clearly and completely describe the technical solutions in the embodiments of the present invention. Obviously, the described embodiments are only part of the embodiments of the present invention, not all of the embodiments. Based on the embodiments of the present invention, all other embodiments obtained by ordinary technicians in this field without creative work are within the scope of protection of the present invention.

[0022] See also Figure 1-Figure 4 , a method for reducing the wear rate of a foot roller by using alloy powder and a hot working process, wherein the composition of the alloy powder used in the hot working process is: C: 0.08~0.10wt%; Cr: 13.0~13.3wt%; Ni: 2.4~2.7wt%; Mo: 1.2~1.4wt%; Mn: 0.7~0.9wt%; Cu: 8.4~8.5wt%; Sn: 1.1~1.2wt%; Nb: 0.14~0.16wt%; B: 0.6~1.0wt%; Si: 0.7~0.8wt%; P: 0.1~0.2wt%; Fe is the balance.

[0023] Furthermore, the thermal processing technology matching the alloy powder includes a laser cladding process and a cladding layer heat treatment process. The parameters of the laser cladding operation are: a fiber laser with a power of 3500~4000w and a power density of 218~250w / mm 2 The line speed is 22~24mm / s, the overlap rate is 50%~55% of the spot length direction, the cladding single-side thickness is 1.8~2.2mm, and the laser cladding operation is carried out on the substrate surface of the foot roller in a continuous spiral overlap manner.

[0024] Furthermore, the heat treatment process of the cladding layer is as follows: the workpiece after laser cladding is placed in a resistance furnace at 1180~1195℃, kept at this temperature for 100~120min, and then the workpiece is taken out of the furnace and air-cooled to room temperature. Then the workpiece is placed in the resistance furnace again, heated to 280~310℃ at a heating rate of 2.7~3.2℃ / min, kept at this temperature for 235~255min, and finally taken out of the furnace and cooled to room temperature. The hardness of the cladding layer after heat treatment is between 38~43HRC, which is the qualified standard.

[0025] Further explanation on the selection of alloy composition and setting of heat treatment process:

[0026] 1. The overall idea of ​​alloy design

[0027] The purpose of reducing friction is achieved by dispersing and precipitating the Cu-Sn-Mo-P phase on the lath martensite matrix, and the wear rate of the foot roller laser cladding layer is reduced by reducing friction. The design route is divided into four steps:

[0028] (1) The four elements C, Cr, Ni and Mo combine to form a martensitic matrix structure, ensuring the oxidation resistance, corrosion resistance and thermal strength of the foot roller. When the C content is higher than 0.1wt%, the oxidation resistance and corrosion resistance of martensitic steel are insufficient, and the cladding layer is prone to cracking. When it is lower than 0.08wt%, the hardness and thermal strength of martensite are insufficient. When the Cr content is higher than 12.5%, the oxidation resistance of the cladding layer is guaranteed, but with the continuous increase of Cr content, the ferrite phase in the cladding layer continues to increase, and the tendency of brittle cracking increases, so the Cr content is best between 13.0 and 13.3wt%. The Ni content is designed to increase the proportion of high-temperature austenite phase. Too high Ni content (>2.7wt%) is prone to thermal cracking during laser cladding, and too low Ni content (<2.4wt%) is prone to insufficient martensite phase. Mo plays the role of thermal strength and self-lubricating and friction reduction in this solution. When Mo is lower than 1.2wt%, the hardness, thermal strength and self-lubricating properties are insufficient. When it is higher than 1.4wt%, the overlap area of ​​the cladding layer is prone to wear.

[0029] (2) The combination of Cu-Sn-Mo-P four elements plays a role in lubrication and friction reduction during the service life of the workpiece. Since the melting points of Cu and Sn are lower than those of steel, they can easily form a self-lubricating and friction-reducing layer on the surface of the iron-based material. Cu has good thermal conductivity, which prevents the heat accumulation generated when the foot roller contacts the high-temperature steel billet, causing overheating cracks. When the Cu content is lower than 8.4wt% and the Sn content is lower than 1.1wt%, the friction reduction effect is insufficient. When the Cu content is higher than 8.5wt% and the Sn content is higher than 1.2wt%, the laser cladding is not formed, and the cladding layer is prone to defects such as pores. P promotes the dispersion of Cu and Sn elements in the alloy system. When P is higher than 0.2wt%, it is easy to cause hot brittleness effect. When it is lower than 0.1wt%, Cu and Sn elements are easy to agglomerate. In addition, Mo combined with Cu and Sn elements can effectively reduce the thickness of the high-temperature oxide film, so that the service life of the foot roller can be further improved.

[0030] (3) The combination of B and Nb elements mainly plays the role of reducing (controlling) the carbon content and improving the grain boundary strength. When the B element is lower than 0.6wt%, not only the carbon content needs to be increased, but also the foot roller is prone to form cracks during service. When the B element is higher than 1.0wt%, the cold cracking tendency is serious. When the Nb content is lower than 0.14wt%, the foot roller is prone to overlap corrosion during the laser cladding process, especially in the second half of the foot roller. When the Nb content is higher than 0.16wt%, the risk of intergranular corrosion of the cladding layer will increase.

[0031] (4) Mn and Si elements. Mn and Si elements are not only indispensable alloying elements in steel materials, but also play the role of removing pores caused by P elements. When the content of Mn and Si is lower than 0.7wt%, there are more phosphorus pores in the cladding layer. When the content of Mn is higher than 0.9wt% and the content of Si is higher than 0.8wt%, thermal cracks are easily generated during laser cladding.

[0032] 2. Selection of laser cladding parameters

[0033] Laser cladding parameters are determined according to the composition and characteristics of the alloy powder, which will not be discussed in detail here.

[0034] 3. Description of heat treatment process system

[0035] The phase transition process of alloy powder from molten state to room temperature is as follows Figure 3 As shown in the figure, since laser cladding is a thermal processing technology with rapid heating and cooling and the alloy powder provided by this solution has a complex composition, it is necessary to adjust the microstructure of the laser cladding layer according to the phase diagram after the laser cladding is completed. Therefore, the foot roller workpiece is heated to 1180~1195℃ and kept warm for 100~120min. The purpose is to homogenize the workpiece. As can be seen from the phase diagram, too high a temperature will easily lead to coarsening of the cladding layer structure, and too low a temperature will easily generate a ferrite brittle phase. When the workpiece is kept warm for 100~120min, in order to fully burn through the workpiece and prevent the temperature of the workpiece surface and core from being inconsistent, resulting in cracks in the subsequent cooling process. Since the thickness of the cladding layer is only two millimeters and the hardenability of this alloy is good, air cooling is selected. Water cooling and oil cooling are prone to cracks in actual processing. "Put the workpiece back in the resistance furnace, heat it to 280~310℃ at a heating rate of 2.7~3.2℃ / min, keep it warm for 235~255min, and finally take it out of the furnace and cool it to room temperature." The purpose of this step is to slowly precipitate the Cu-Sn-Mo-P compound and disperse it in the lath martensite matrix structure, but not all of it, but to partially dissolve the four elements Cu, Sn, Mo, and P in the martensite. This method can extend the service life of the foot roller. Therefore, the heat treatment temperature is selected to be a lower temperature "280~310℃" and a longer time "235~255min". The heat treatment system is as follows Figure 4 shown.

[0036] Example 1

[0037] A method for reducing the wear rate of a foot roller by using alloy powder and a hot working process. The composition of the alloy powder used in the hot working process is: C: 0.08wt%; Cr: 13.0wt%; Ni: 2.4wt%; Mo: 1.2wt%; Mn: 0.7wt%; Cu: 8.4wt%; Sn: 1.1wt%; Nb: 0.14wt%; B: 0.6wt%; Si: 0.7wt%; P: 0.1wt%; Fe is the balance.

[0038] Laser cladding process matching alloy powder: 3500w fiber laser with power density of 218w / mm 2 The line speed is 22mm / s, the overlap rate is 50% in the direction of the spot length, the cladding single-side thickness is 1.8mm, and the laser cladding operation is carried out on the substrate surface of the foot roller in a continuous spiral overlap manner.

[0039] The heat treatment process matching the alloy powder is as follows: the workpiece after laser cladding is placed in a resistance furnace at 1180°C, kept at this temperature for 100 minutes, and then air-cooled to room temperature. The workpiece is then placed in the resistance furnace again, heated to 280°C at a heating rate of 2.7°C / min, kept at this temperature for 235 minutes, and finally cooled to room temperature. The hardness of the cladding layer after heat treatment is 41.0HRC.

[0040] After the foot roller was put into the production line for testing for 39 days, the diameter reduction of the foot roller temporarily taken off the line was measured, as shown in Table 1.

[0041] Table 1: Diameter reduction of the foot roller tested according to the solution provided in Example 1

[0042]

[0043] Example 2

[0044] A method for reducing the wear rate of a foot roller by using alloy powder and a hot working process. The composition of the alloy powder used in the hot working process is: C: 0.09wt%; Cr: 13.2wt%; Ni: 2.6wt%; Mo: 1.3wt%; Mn: 0.8wt%; Cu: 8.45wt%; Sn: 1.15wt%; Nb: 0.15wt%; B: 0.8wt%; Si: 0.75wt%; P: 0.15wt%; Fe is the balance.

[0045] Laser cladding process matching alloy powder: Use fiber laser with power of 3500~4000w and power density of 234w / mm 2The line speed is 23 mm / s, the overlap rate is 53% of the spot length direction, the cladding single-side thickness is 2.0 mm, and the laser cladding operation is carried out on the substrate surface of the foot roller in a continuous spiral overlap manner.

[0046] The heat treatment process matching the alloy powder is as follows: the workpiece after laser cladding is placed in a resistance furnace at 1187°C, kept at this temperature for 110 minutes, and then air-cooled to room temperature. The workpiece is then placed in the resistance furnace again, heated to 295°C at a heating rate of 2.9°C / min, kept at this temperature for 245 minutes, and finally cooled to room temperature. The hardness of the cladding layer after heat treatment is 42.8HRC.

[0047] After the foot roller was put into the production line for testing for 39 days, the diameter reduction of the foot roller temporarily taken off the line was measured, as shown in Table 2.

[0048] Table 2: Diameter reduction of the foot roller tested according to the solution provided in Example 2

[0049]

[0050] Example 3

[0051] A method for reducing the wear rate of a foot roller by using alloy powder and a hot working process. The composition of the alloy powder used in the hot working process is: C: 0.10wt%; Cr: 13.3wt%; Ni: 2.7wt%; Mo: 1.4wt%; Mn: 0.9wt%; Cu: 8.5wt%; Sn: 1.2wt%; Nb: 00.16wt%; B: 1.0wt%; Si: 0.8wt%; P: 0.2wt%; Fe is the balance.

[0052] Laser cladding process matching alloy powder: use fiber laser with power of 3500~4000w and power density of 250w / mm 2 The line speed is 24 mm / s, the overlap rate is 55% of the spot length direction, the cladding single-side thickness is 2.2 mm, and the laser cladding operation is carried out on the substrate surface of the foot roller in a continuous spiral overlap manner.

[0053] The heat treatment process route that matches the alloy powder is: place the workpiece after laser cladding in a resistance furnace at 1195℃, keep it warm for 120 minutes, then take it out of the furnace and air cool it to room temperature. Then put the workpiece back into the resistance furnace, heat it to 310℃ at a heating rate of 3.2℃ / min, keep it warm for 255 minutes, and finally take it out of the furnace and cool it to room temperature. The hardness of the cladding layer after heat treatment is 40.5HRC.

[0054] After the foot roller was put into the production line for testing for 39 days, the diameter reduction of the foot roller temporarily taken off the line was measured, as shown in Table 3.

[0055] Table 3: Diameter reduction of the foot roller tested according to the solution provided in Example 3

[0056]

[0057] It is obvious to those skilled in the art that the present invention is not limited to the details of the above exemplary embodiments, and that the present invention can be implemented in other specific forms without departing from the spirit or basic features of the present invention. Although this specification is described in accordance with the implementation modes, not every implementation mode includes only one technical solution. This description of the specification is only for the sake of clarity. Those skilled in the art should regard the specification as a whole. The technical solutions in each embodiment can also be appropriately combined to form other implementation modes that can be understood by those skilled in the art.

Claims

1. A method for reducing the wear rate of a foot roller by using alloy powder and a thermal processing process, characterized in that: The specific steps include: Step 1: performing laser cladding operation on the surface of the substrate of the foot roller, the laser cladding hot processing process material includes alloy powder, and the composition of the alloy powder is: C: 0.08~0.10wt%, Cr: 13.0~13.3wt%, Ni: 2.4~2.7wt%, Mo: 1.2~1.4wt%, Mn: 0.7~0.9wt%, Cu: 8.4~8.5wt%, Sn: 1.1~1.2wt%, Nb: 0.14~0.16wt%, B: 0.6~1.0wt%, Si: 0.7~0.8wt%, P: 0.1~0.2wt%, and Fe is the balance; Step 2: Place the foot roller workpiece after laser cladding in a 1180~1195℃ resistance furnace, keep it warm for 100~120min, and then take it out of the furnace and air cool it to room temperature; Step 3: Then place the workpiece back in the resistance furnace, heat it to 280~310℃ at a heating rate of 2.7~3.2℃ / min, keep it warm for 235~255min, and finally cool it to room temperature. The hardness of the cladding layer after heat treatment is between 38~43HRC, which is the qualified standard.

2. The method of reducing the wear rate of the foot roller by using alloy powder and hot working process according to claim 1, characterized in that: The parameters of the laser cladding operation include: using a fiber laser with a power of 3500~4000w and a power density of 218~250w / mm 2 , linear speed is 22~24mm / s.

3. The method of reducing the wear rate of the foot roller by using alloy powder and hot working process according to claim 1, characterized in that: In the step 1, laser cladding is performed on the surface of the base material of the foot roller in a continuous spiral overlapping manner.

4. The method of reducing the wear rate of the foot roller by using alloy powder and hot working process according to claim 3, characterized in that: The overlapping rate of the continuous spiral overlap is 50% to 55% in the length direction of the light spot.

5. A method for reducing the wear rate of a foot roller by using alloy powder and hot working process according to any one of claims 1 to 4, characterized in that: The single-side thickness of the laser cladding is 1.8-2.2 mm.