Phosphorus-doped TiO2 / elemental phosphorus heterojunction composite film photoelectrode and preparation method and application thereof

By using black phosphorus as the doping source on the TiO2 nanofiber film to form a phosphorus-doped TiO2/phosphorus elemental heterojunction composite film photoelectrode, the problems of complicated preparation methods and limited doping amount in the existing technology are solved, and the efficiency is significantly improved. Photoelectrocatalytic performance, suitable for photoelectrocatalytic hydrogen production, nitrogen fixation, CO2 conversion and other fields.

CN118756221APending Publication Date: 2024-10-11SHAANXI UNIV OF SCI & TECH
View PDF 0 Cites 0 Cited by

Patent Information

Application Number
CN202410953258.7
Authority / Receiving Office
CN · China
Patent Type
Applications(China)
Current Assignee / Owner
Filing Date
2024-07-16
Publication Date
2024-10-11

AI Technical Summary

Technical Problem

In the existing technology, the preparation method of TiO2 photoelectrocatalyst is complicated and the doping amount is limited, resulting in limited improvement in photoelectrocatalytic performance.

Method used

Using a titanium metal sheet as the substrate, a TiO2 nanofiber film is grown through hydrothermal and pickling calcination methods, and combined with black phosphorus under high temperature and high pressure conditions to form a phosphorus-doped TiO2/phosphorus elemental heterojunction composite film photoelectrode, using the black phosphorus' Highly active phosphorus atoms are doped and coated in TiO2 to build a one-dimensional core-shell structure to improve light absorption and electron-hole separation efficiency.

Benefits of technology

The preparation process has been simplified, the photoelectrocatalytic performance has been improved, the photocurrent density and visible light response range have been enhanced, and the material can be recycled, making it suitable for photoelectrocatalytic hydrogen production, nitrogen fixation, CO2 conversion and other fields.

✦ Generated by Eureka AI based on patent content.

Smart Images

  • Figure HDA0004947820940000011
    Figure HDA0004947820940000011
  • Figure HDA0004947820940000012
    Figure HDA0004947820940000012
  • Figure HDA0004947820940000013
    Figure HDA0004947820940000013
Patent Text Reader

Abstract

The invention provides a phosphorus-doped TiO2 / phosphorus elementary substance heterojunction composite film photoelectrode and a preparation method and application thereof.The preparation method comprises the steps that 1, a titanium metal sheet is immersed in a NaOH solution to be subjected to a hydrothermal reaction, washing and drying are conducted after the reaction is finished, then the titanium metal sheet is placed in a hydrochloric acid solution to be acidified, the acidified titanium metal sheet is calcined, and the titanium metal sheet is obtained; growing a TiO2 nanofiber film on the titanium metal sheet in situ; and (2) putting the titanium metal sheet on which the TiO2 nanofiber film grows in situ, excessive black phosphorus and iodine into a quartz tube, vacuumizing the quartz tube, sealing, calcining, cooling to room temperature, and washing and drying the titanium metal sheet to obtain the phosphorus-doped TiO2 / phosphorus elementary substance heterojunction composite film photoelectrode. The method can solve the problems that in the prior art, a preparation method is complex, and the phosphorus doping amount is limited.
Need to check novelty before this filing date? Find Prior Art

Description

Technical Field

[0001] The present invention belongs to the technical field of photoelectrochemical nanomaterial preparation, and specifically relates to a phosphorus-doped TiO2 / phosphorus element (P-TiO2 / P) heterojunction composite thin film photoelectrode and a preparation method and application thereof. Background Art

[0002] The energy utilization method of converting solar energy into hydrogen energy reduces human dependence on fossil fuels and avoids carbon dioxide emissions. It is regarded as an effective measure to solve the current energy shortage and environmental pollution. This technology shows great development potential and prospects. Since Fujishima and Honda discovered the phenomenon of photoelectrocatalytic decomposition of water to produce hydrogen on single-crystal TiO2 electrodes in 1972, solar photoelectrocatalytic technology using semiconductor nanomaterials as photoelectrodes has become a research hotspot. However, due to the low solar energy utilization rate caused by the wide bandgap of TiO2 and the high recombination rate of photogenerated electron-hole pairs, the photoelectric conversion efficiency of semiconductor catalysts is seriously restricted. Therefore, seeking easy-to-implement methods to improve photoelectrocatalytic performance has become the focus of attention in this field.

[0003] Among the many methods to broaden the photoresponse range of TiO2 and improve the efficiency of electron-hole separation, element doping and forming semiconductor heterojunctions are two effective measures. Black phosphorus, as an emerging single-element direct bandgap semiconductor material, has attracted widespread attention from scientists since it was successfully exfoliated in 2014. The unique two-dimensional lamellar structure gives black phosphorus good photoelectric conversion properties, significant anisotropy and high carrier mobility, making it show great potential in the fields of photoelectricity, photothermal, energy storage, catalysis, etc. Tetsuro Majima et al. designed a two-dimensional Z-type photocatalytic structure based on BP / BiVO4, which can achieve photocatalytic water splitting without bias. Zhu et al. composited two non-metallic two-dimensional materials, BP nanosheets and g-C3N4 nanosheets, and the prepared photocatalyst had photocatalytic hydrogen production performance under visible light and near-infrared light. Further characterization proved that the high separation and transmission efficiency of photogenerated carriers of the composite material gave it good photocatalytic activity.

[0004] Chinese patent CN109411740A discloses a phosphorus-doped bronze phase titanium dioxide nanowire array and its preparation and application. The method uses sodium hypophosphite as a phosphorus source, and by placing it together with a titanium sheet in a tubular furnace for heat treatment, phosphorus is doped into the bronze phase titanium dioxide nanowire array to obtain a self-supporting lithium-ion battery negative electrode that does not require the addition of any binder and conductive agent and has excellent electrochemical performance. The method is to react under high temperature and normal pressure conditions, the phosphorus atom doping amount is low, and heteroatoms are easily introduced using sodium hypophosphite as a phosphorus source. At the same time, the reaction cannot produce a phosphorus coating layer.

[0005] It can be seen from the existing literature that the research on P and TiO2 in photoelectrocatalysis mainly focuses on doping TiO2 with sodium hypophosphite or red phosphorus as the phosphorus source, and forming a heterostructure with red phosphorus and black phosphorus to improve the absorption of visible light by TiO2 and improve the efficiency of photogenerated electron and hole separation. The current catalyst preparation method has complex steps, limited doping amount, and limited performance improvement. It can be seen that there is an urgent need to develop a simple preparation method for P-doped TiO2 photoelectrode materials with efficient photoelectrocatalytic performance. Summary of the invention

[0006] The purpose of the present invention is to provide a phosphorus-doped TiO2 / phosphorus single substance heterojunction composite thin film photoelectrode and its preparation method and application, so as to solve the problems of complex preparation method and limited doping amount in the prior art.

[0007] The present invention is achieved through the following technical solutions:

[0008] The present invention provides a method for preparing a phosphorus-doped TiO2 / phosphorus single substance heterojunction composite thin film photoelectrode, comprising:

[0009] (1) immersing a titanium metal sheet in a NaOH solution for a hydrothermal reaction, washing and drying the titanium metal sheet after the reaction, and then placing the titanium metal sheet in a hydrochloric acid solution for acidification. The acidified titanium metal sheet is calcined to in-situ grow a TiO2 nanofiber film on the titanium metal sheet;

[0010] (2) A titanium metal sheet with an in-situ grown TiO2 nanofiber film, excess black phosphorus and iodine are placed in a quartz tube, the quartz tube is evacuated and sealed, and calcined. After cooling to room temperature, the titanium metal sheet is washed and dried to obtain a phosphorus-doped TiO2 / phosphorus single-element heterojunction composite thin film photoelectrode.

[0011] Preferably, before step (1), the method further comprises the following steps: immersing the titanium metal sheet in a mixed acid for surface polishing, wherein the mixed acid is a mixed aqueous solution of HF and HNO 3 .

[0012] Preferably, the concentration of NaOH in the NaOH solution is 1 to 4.5 mol / L.

[0013] Preferably, in step (1), the temperature of the hydrothermal reaction is 180-210° C. and the time is 24-48 hours.

[0014] Preferably, in step (1), the calcination temperature is 450-700°C.

[0015] Preferably, in step (2), the preparation method of black phosphorus is: fully mixing red phosphorus, tin powder and iodine particles, and encapsulating the mixture into a quartz tube under vacuum conditions; and calcining the quartz tube to obtain black phosphorus crystals.

[0016] Furthermore, the mass ratio of red phosphorus, tin powder and iodine is 20:2:1.

[0017] Preferably, in step (2), the calcination temperature is 550-650° C. and the calcination time is 3-6 hours.

[0018] The present invention provides a phosphorus-doped TiO2 / phosphorus single substance heterojunction composite thin film photoelectrode obtained by the preparation method as described above, which is a one-dimensional core-shell structure, wherein the inner core layer is phosphorus-doped TiO2 and the outer shell layer is phosphorus single substance.

[0019] The present invention provides an application of the phosphorus-doped TiO2 / phosphorus single substance heterojunction composite thin film photoelectrode in photoelectrocatalytic hydrogen production, nitrogen fixation or CO2 conversion.

[0020] Compared with the prior art, the present invention has the following beneficial effects:

[0021] The present invention uses titanium metal sheet as raw material, and prepares a TiO2 nanofiber film with titanium metal sheet as substrate through hydrothermal, acid washing and calcination processes. The preparation is prepared by a relatively mild hydrothermal method. The titanium metal sheet is used as both substrate and titanium source to simplify the preparation steps. At the same time, the titanium substrate is a good conductor, so that the product TiO2 nanofiber film and the titanium substrate are directly and firmly connected. The photoelectrocatalytic material is not easy to fall off during use, and it is convenient to reuse; the generated TiO2 nanofiber has an extremely high ordered arrangement structure and extremely low agglomeration. Black phosphorus is mixed and calcined with the TiO2 nanofiber film to form a P-TiO2 / P heterojunction composite film material. The reaction mechanism of black phosphorus and TiO2 nanofiber can be summarized as follows: under high temperature and high pressure environment, black phosphorus powder undergoes sublimation, thermal decomposition and other processes to generate phosphorus vapor; high temperature phosphorus vapor reacts with TiO2, and highly active P atoms enter the TiO2 lattice or gap to achieve doping; then, as the temperature decreases, excess phosphorus is deposited on the outside of the TiO2 nanofiber to form a P coating layer. The addition of I2 in high-temperature solid-phase reactions can make the high-temperature sublimated reactants transfer between the high-temperature zone and the low-temperature zone, making them evenly distributed in the tube, improving the uniformity and efficiency of the reaction. The P-TiO2 / P heterojunction composite thin film material has a one-dimensional core-shell structure, with the inner core layer being P-doped TiO2 and the outer shell being single-substance P. The P coating layer not only closely combines with the nanofibers to form a heterostructure, but also protects the TiO2 nanofibers from phase change at high temperatures. On the one hand, when P atoms are doped into TiO2, the Ti-OP bonds formed and the impurity energy levels introduced significantly enhance the light absorption capacity of TiO2 and capture sunlight more effectively; on the other hand, the single-substance P coating layer closely contacts the TiO2 core to form a heterojunction, enhancing visible light absorption and accelerating the separation and transmission of photogenerated electrons and holes at the interface. Due to the two-dimensional layered structure and large specific surface area of ​​black phosphorus, the phosphorus vapor generated after sublimation and thermal decomposition under high temperature and high pressure is more active than red phosphorus, which makes the TiO2 film prepared with black phosphorus as the doping source have a higher photocurrent density. Compared with other doping and heterojunction construction methods, since the present invention uses black phosphorus as a phosphorus source, phosphorus atoms with high activity under high temperature and high pressure conditions significantly increase the doping amount, and will not introduce heteroatoms to form defects, and one-step method simultaneously completes phosphorus doping and phosphorus single substance coating, and the prepared composite thin film photoelectrode is in-situ generated on a titanium metal sheet, and can be directly used as an electrode, and does not need to be connected to a conductive substrate through an adhesive, which greatly improves the electron transport capacity of the semiconductor and the conductive substrate. The construction of doping and heterojunction can effectively improve stability and catalytic performance, and can be recycled after simple cleaning after use. The preparation method of the present invention has simple equipment, low raw material price, wide source, safety and non-toxicity, simple preparation process, safe and easy operation, and can be mass-produced.

[0022] Furthermore, before the hydrothermal reaction, the oxides and oil stains on the surface of the titanium sheet are cleaned with a mixed acid, which can improve the cleanliness of the surface of the titanium sheet and facilitate the hydrothermal reaction.

[0023] Furthermore, the calcination temperature in step (2) does not exceed 650° C. to prevent excessive doping of black phosphorus, which would lead to excessive defects in the TiO2 crystal and introduce more electron-hole recombination centers.

[0024] The P-doped TiO2 and P single-element heterojunction composite thin film photoelectrode prepared by the present invention has the advantages of recyclability, excellent photoelectrocatalytic performance, a wide spectral response range (with visible light response), and low cost. It has great application value in the field of photoelectric energy conversion and can be used for photoelectrocatalytic hydrogen production, nitrogen fixation, and CO2 conversion. BRIEF DESCRIPTION OF THE DRAWINGS

[0025] In order to more clearly illustrate the embodiments of the present invention or the technical solutions in the prior art, the drawings required for use in the embodiments or the description of the prior art will be briefly introduced below. Obviously, the drawings described below are some embodiments of the present invention. For ordinary technicians in this field, other drawings can be obtained based on these drawings without paying creative work.

[0026] Figure 1 Digital photos of the TiO2 nanofiber film (a) and the P-TiO2 / P heterojunction composite film (b) prepared in Example 1 of the present invention;

[0027] Figure 2 The XRD diagram of the P-TiO2 / P heterojunction composite film prepared in Example 1 of the present invention;

[0028] Figure 3 SEM images of the TiO2 nanofiber film (a) and the P-TiO2 / P heterojunction composite film (b) prepared in Example 1 of the present invention;

[0029] Figure 4 Transient photocurrent-time curve of the P-TiO2 / P and P-TiO2(NaH2PO2) heterojunction composite thin film prepared in Example 2 of the present invention under simulated sunlight conditions;

[0030] Figure 5 TEM image of the P-TiO2 / P heterojunction composite film prepared in Example 2 of the present invention;

[0031] Figure 6 This is the element distribution diagram of the P-TiO2 / P heterojunction composite film prepared in Example 2 of the present invention;

[0032] Figure 7This is a hydrogen production performance curve of the P-TiO2 / P heterojunction composite film prepared in Example 3 of the present invention;

[0033] Figure 8 The transient photocurrent-time curves of the P-TiO2 / P and P-TiO2 / P(RP) heterojunction composite films prepared in Example 3 of the present invention under simulated sunlight and visible light conditions. DETAILED DESCRIPTION

[0034] The following describes the embodiments of the present invention through specific examples, and those skilled in the art can easily understand other advantages and effects of the present invention from the contents disclosed in this specification. The present invention can also be implemented or applied through other different specific embodiments, and the details in this specification can also be modified or changed in various ways based on different viewpoints and applications without departing from the spirit of the present invention.

[0035] It should be noted that the process equipment or devices not specifically specified in the following embodiments are all conventional equipment or devices in the art.

[0036] It should be noted that the terms "include" and "have" and any variations thereof are intended to cover non-exclusive inclusions. For example, a process, method, system, product or device that includes a series of steps or units is not necessarily limited to those steps or units clearly listed, but may include other steps or units that are not clearly listed or inherent to these processes, methods, products or devices. Moreover, unless otherwise specified, the numbering of each method step is only a convenient tool for identifying each method step, and is not intended to limit the order of arrangement of each method step or to define the scope of the present invention. Changes or adjustments in their relative relationships should also be regarded as the scope of the present invention without substantially changing the technical content.

[0037] The method for preparing the P-TiO2 / P heterojunction composite thin film photoelectrode of the present invention adopts the following steps:

[0038] (1) immersing a titanium metal sheet in a mixed acid for surface polishing; placing the polished titanium metal sheet in a NaOH solution for hydrothermal reaction, washing and drying after the reaction, and then immersing in a hydrochloric acid solution for acidification; placing the acidified titanium metal sheet in a muffle furnace for calcination, and in-situ growing a TiO2 nanofiber film on the titanium metal sheet;

[0039] (2) fully mixing red phosphorus, tin powder and iodine particles, and encapsulating the mixture into a quartz tube under vacuum conditions; then, placing the quartz tube in a muffle furnace and calcining it under certain heating and cooling conditions to obtain black black phosphorus (BP) crystals with a metallic luster;

[0040] (3) A titanium metal sheet with an in-situ grown TiO2 nanofiber film, a certain amount of black phosphorus (excess) and iodine are placed in a quartz tube by using a vacuum sealing method; the quartz tube is evacuated and sealed, and then placed in a muffle furnace for calcination. After cooling to room temperature, it is washed and dried to obtain a P-TiO2 / P heterojunction composite thin film photoelectrode.

[0041] In step (1) of the above method of the present invention, the mixed acid is a mixed aqueous solution of HF and HNO3, and the volume ratio of HF, HNO3 and H2O is preferably 1:4:5.

[0042] The NaOH solution preparation method adopted by the present invention is as follows: dissolving NaOH in a mixed solution of water and ethylene glycol, and stirring to fully dissolve it; wherein the volume ratio of water to ethylene glycol in the mixed solution is 1:(1-3), and the concentration of NaOH in the mixed solution is 1-4.5 mol / L.

[0043] In step (1) of the present invention, the hydrothermal reaction temperature is 180-210°C, and the hydrothermal reaction time is 24-48h; the concentration of the hydrochloric acid solution for acidification is 0.75-1.75wt%; the calcination temperature in the muffle furnace is 450-700°C, more preferably 500-600°C, and the insulation time is preferably 4h.

[0044] In step (2) of the above method of the present invention, the mass ratio of the red phosphorus, tin powder and iodine is preferably 20:2:1.

[0045] In step (3) of the above method of the present invention, two Ti metal sheets (5×40 mm) with TiO2 nanofiber films grown thereon are placed in a quartz tube, and the amount of BP added is 0.4 to 3 mg, and the amount of I2 added is 0.5 to 2 mg. As the amount of BP added increases, the P doping amount and the thickness of the P single substance coating layer both increase, and the absorption of visible light and the electron-hole separation efficiency of the electrode are both improved; however, an excessively thick P coating layer will reduce the absorption of sunlight by the TiO2 nanofibers, and instead reduce the photoelectric catalytic performance.

[0046] In step (3) of the above method of the present invention, the calcination temperature in the muffle furnace is 550-650° C., preferably 600-620° C., and the insulation time in the muffle furnace is 3-6 hours.

[0047] Embodiment 1:

[0048] (1) Cut titanium sheet (Ti sheet) into thin sheets of 20×40×0.2 mm and immerse them in mixed acid (HF:HNO3:H2O=1:4:5) for surface polishing. Dissolve 15g NaOH in a mixture of 25mL water and 75mL ethylene glycol and stir to fully dissolve it. Put the polished Ti sheet into the mixture for hydrothermal reaction and keep it at 200℃ for 24h. After the reaction, wash and dry it with water and ethanol, and soak it in 1.2wt% hydrochloric acid solution for 24h. Put the acidified Ti sheet into a muffle furnace and calcine it at 500℃ for 4h to form a TiO2 nanofiber film (Ti / TiO2) on the Ti substrate.

[0049] (2) 400 mg of red phosphorus (RP), 40 mg of tin (Sn) powder and 20 mg of iodine (I2) particles were fully mixed and the mixture was encapsulated in a quartz tube under vacuum conditions. The temperature was raised from room temperature to 620°C at a rate of 2°C / min and kept at this temperature for 5 hours. Afterwards, the temperature was lowered to 485°C at a rate of 0.5°C / min and kept at this temperature for 4 hours. Finally, the temperature was slowly lowered to 120°C at a rate of 1°C / min and cooled to room temperature in the furnace to obtain black black phosphorus (BP) crystals with a metallic luster.

[0050] (3) Two Ti sheets (5×40 mm) with TiO2 nanofiber films grown on them and 1 mg BP were placed in a quartz tube, and 0.5 mg I2 was added. The quartz tube was evacuated and sealed, and then placed in a muffle furnace and heated to 600°C for calcination for 3 h. After cooling to room temperature, the tube was washed and dried to form a P-TiO2 / P heterojunction composite thin film photoelectrode on the Ti substrate.

[0051] like Figure 1 The following are digital photos of the TiO2 nanofiber film (a) and the P-TiO2 / P heterojunction composite film (b) prepared in this example. It can be seen from the figure that the color of the prepared TiO2 nanofiber film changes from metallic color to blue after the vacuum sealed tube high temperature solid phase reaction, indicating that the P-TiO2 / P heterojunction composite film photoelectrode significantly enhances the absorption of visible light, which is beneficial to improve the utilization rate of sunlight in the photoelectrocatalytic process. Figure 2 It can be seen from the XRD spectrum shown that the prepared P-TiO2 / P heterojunction composite film is anatase phase TiO2 (PDF 21-1272). Apart from this, no other significant characteristic peaks are observed, which may be due to the relatively low doping and loading of P. Figure 3The microscopic morphology of the TiO2 nanofiber film (a) and the P-TiO2 / P heterojunction composite thin film photoelectrode (b) observed by scanning electron microscopy. As shown in Figure (a), the diameter of the TiO2 nanofiber is about 30nm, the length is several microns, the fiber surface is smooth, and the fibers grow randomly and intertwine to form a TiO2 network structure, forming a large number of micropores; as shown in Figure (b), the morphology of the nanofibers after BP doping changes significantly, showing a short rod shape, which can provide more active sites for photoelectrocatalytic reactions. The experimental results show that under the conditions of 300W xenon lamp irradiation and AM1.5 G filter simulating sunlight, the photocurrent density of the P-TiO2 / P heterojunction composite thin film photoelectrode of the present invention reaches 121.8μA·cm under the bias voltage of 0.8V (vs.RHE). -2 , which is 5.6 times the photocurrent density of pure TiO2 nanofiber film.

[0052] Embodiment 2:

[0053] (1) Cut the titanium sheet into 30×60×0.2 mm thin slices and immerse them in a mixed acid (HF:HNO3:H2O=1:4:5) for surface polishing. Dissolve 6 g of NaOH in a mixture of 25 mL of water and 50 mL of ethylene glycol and stir to fully dissolve it. Put the polished Ti sheet into the mixture for hydrothermal reaction and keep it at 180°C for 30 h. After the reaction, wash and dry it with water and ethanol, and soak it in a 1wt% hydrochloric acid solution for 24 h. Put the acidified Ti sheet into a muffle furnace and calcine it at 600°C for 4 h to form a TiO2 nanofiber film (Ti / TiO2) on the Ti substrate.

[0054] (2) 300 mg of red phosphorus (RP), 30 mg of tin (Sn) powder and 15 mg of iodine (I2) particles were fully mixed and the mixture was encapsulated in a quartz tube under vacuum conditions. The temperature was raised from room temperature to 620°C at a rate of 2°C / min and kept at this temperature for 5 h. Afterwards, the temperature was lowered to 485°C at a rate of 0.5°C / min and kept at this temperature for 4 h. Finally, the temperature was slowly lowered to 120°C at a rate of 1°C / min and then cooled to room temperature in the furnace to obtain black BP crystals with a metallic luster.

[0055] (3) Two Ti sheets (5×40 mm) with TiO2 nanofiber films grown thereon and 2 mg of BP were placed in a quartz tube, and 1.2 mg of I2 was added. The quartz tube was evacuated and sealed, and then placed in a muffle furnace and heated to 620°C for calcination for 4 h. After cooling to room temperature, it was washed and dried to form a P-TiO2 / P heterojunction composite thin film photoelectrode on the Ti substrate.

[0056] Comparative Example 1

[0057] In order to compare the effects of different phosphorus sources and different doping methods on the photoelectrocatalytic performance of composite thin film photoelectrodes, composite thin film samples were prepared by the method of doping in a tube furnace. Two Ti sheets with TiO2 nanofiber films grown thereon prepared in Example 2 and 0.5 g of sodium hypophosphite were placed in a tube furnace, nitrogen was introduced for protection, the sodium hypophosphite was located upstream of the airflow, and the Ti sheet was located downstream of the airflow. The temperature was raised to 450°C and kept for 3 hours to obtain a phosphorus-doped TiO2 nanofiber film, recorded as P-TiO2 (NaH2PO2).

[0058] like Figure 4 As shown in the figure, under the conditions of 300W xenon lamp irradiation and AM1.5G filter simulating sunlight, the photocurrent density of the P-TiO2 / P heterojunction composite thin film photoelectrode of Example 2 of the present invention reaches 80.4μA·cm at a bias voltage of 0.7V (vs.RHE). -2 , which is 3.7 times the photocurrent density of pure TiO2 nanofiber film. The photocurrent density of P-TiO2 (NaH2PO2) composite film photoelectrode under the same test conditions is 40.1μA·cm -2 , which is significantly lower than that of the P-TiO2 / P sample. This may be because the present invention significantly increases the P doping amount under high temperature and high pressure conditions by sealing the tube, and the coating layer formed by the deposition of excess P atoms further improves the light absorption and electron-hole separation efficiency, resulting in a higher photocurrent density.

[0059] Figure 5 The figure shows the microscopic morphology of the P-TiO2 / P sample of Example 2 observed by transmission electron microscopy. As can be seen from Figure (a), the length of the TiO2 nanowire is about 450nm, the diameter is about 55nm, and it presents a hollow tubular structure with rich mesopores on the surface. These mesopores provide more active sites for surface reactions, making it easier for water molecules and hydroxyl groups on the surface to be adsorbed. As can be seen from Figures (b) and (c), the sample has good crystallinity, and the lattice fringes at a crystal plane spacing of 0.35nm correspond to the (101) plane of the rutile phase TiO2; the external amorphous layer is a phosphorus coating layer, and it has been measured that the thickness of the phosphorus outer shell layer is about 1.7nm. SEAD analysis confirmed that the diffraction rings correspond to the TiO2 (101) crystal plane. Figure 6 The distribution of elements in the P-TiO2 / P sample is shown. As can be seen from the figure, Ti, O and P elements are all uniformly distributed. TEM results show that the prepared catalyst is a core-shell structure nanowire with P-doped TiO2 as the inner core layer and P single substance as the outer shell layer. This structure can enhance the visible light absorption of the photoelectric catalyst and improve the separation efficiency of photogenerated electrons and holes.

[0060] Embodiment three:

[0061] (1) Cut the titanium sheet into thin sheets of 50×50×0.2 mm and immerse them in a mixed acid (HF:HNO3:H2O=1:4:5) for surface polishing. Dissolve 4g NaOH in a mixture of 25mL water and 25mL ethylene glycol and stir to fully dissolve it. Put the polished Ti sheet into the mixture for hydrothermal reaction and keep it at 210℃ for 24h. After the reaction, wash and dry it with water and ethanol, and soak it in a 0.75wt% hydrochloric acid solution for 24h. Put the acidified Ti sheet into a muffle furnace and calcine it at 500℃ for 4h to obtain a TiO2 nanofiber film.

[0062] (2) 500 mg of red phosphorus (RP), 50 mg of tin (Sn) powder and 25 mg of iodine (I2) particles were fully mixed and the mixture was encapsulated in a quartz tube under vacuum conditions. Subsequently, the temperature was raised from room temperature to 620°C at a rate of 2°C / min and kept at this temperature for 5 h. Afterwards, the temperature was lowered to 485°C at a rate of 0.5°C / min and kept at this temperature for 4 h. Finally, the temperature was slowly lowered to 120°C at a rate of 1°C / min and then cooled to room temperature in the furnace to obtain black BP crystals with a metallic luster.

[0063] (3) Two Ti sheets (5×40 mm) with TiO2 nanofiber films grown thereon and 3 mg of BP were placed in a quartz tube, and 2 mg of I2 was added. The quartz tube was evacuated and sealed, and then placed in a muffle furnace and heated to 650°C for calcination for 4 h. After cooling to room temperature, it was washed and dried to obtain a P-TiO2 / P heterojunction composite thin film photoelectrode.

[0064] Comparative Example 2

[0065] In order to compare the effects of different phosphorus sources on the photoelectrocatalytic performance of the composite thin film photoelectrode, the black phosphorus (BP) placed in the quartz tube in Example 3 was replaced by red phosphorus (RP), and the other experimental methods remained unchanged. The product obtained was marked as P-TiO2 / P(RP) heterojunction composite thin film photoelectrode.

[0066] The photoelectrolysis cell with three electrodes was used to characterize the performance of photoelectrohydrogen production. TiO2 nanofiber film and P-TiO2 / P heterojunction composite film were used as photoanodes, Pt sheet was used as photocathode, and Ag / AgCl electrode was used as reference electrode. Photoelectrohydrogen was produced under a bias voltage of 0.8V (vs.RHE). The electrolyte was a 0.5M Na2SO4 solution, and the light source was a 300W xenon lamp with an AM1.5 G filter to simulate sunlight. Parallel light was irradiated vertically onto the photoanode surface through a quartz window. The reactor was sealed and evacuated several times before the reaction started. Online sampling was performed every 30 minutes after the reaction started, and the hydrogen production was detected by gas chromatography.

[0067] Figure 7The graph of hydrogen production performance of the P-TiO2 / P heterojunction composite film of Example 3 is shown. The experiment was carried out at a constant room temperature, and the applied bias voltage was stabilized at 1 V. The experimental results showed that after 43200 seconds, the volume ratio of oxygen to hydrogen was close to 1:2, proving that the separation of photogenerated carriers was significant and was effectively utilized by the water decomposition reaction. Figure 8 The transient photocurrent-time curve of the P-TiO2 / P heterojunction composite film in Example 3 under simulated sunlight and visible light conditions is shown. Under simulated sunlight (AM 1.5G), the photocurrent density of the P-TiO2 / P photoelectrode increases to 101.3 μA / cm 2 , which is 4.6 times the photocurrent density of pure TiO2 nanofiber film; while the photocurrent density of the P-TiO2 / P(RP) photoelectrode in comparative example 2 is 82.6μA / cm 2 Under the conditions of 300W xenon lamp, plus visible light filter to filter out ultraviolet light below 420nm, and 0.8V (vs. RHE) bias, the photocurrent density of the P-TiO2 / P photoelectrode of Example 3 reached 28.7μA·cm -2 , which is 5.2 times the photocurrent density of pure TiO2 nanofiber film, while the photocurrent density of the P-TiO2 / P(RP) photoelectrode in comparative example 2 is 17.9μA / cm 2 The reason for this phenomenon may be that black phosphorus and red phosphorus have different crystal structures, different sublimation and decomposition temperatures under high temperature and high pressure conditions, different phosphorus source activities, different amounts of doped TiO2 and different thicknesses of the coating layer, which ultimately affect the photoelectrode's photoelectrocatalytic performance.

[0068] It can be seen from the above examples that the P-TiO2 / P heterojunction composite thin film photoelectrode prepared by the present invention using black phosphorus as the phosphorus source has excellent light absorption capacity due to the doping of phosphorus element and phosphorus single substance coating, and at the same time improves the electron-hole separation efficiency by constructing a heterojunction, and the photocurrent response is significantly enhanced under visible light irradiation. The photoelectrode prepared by this method has low cost and simple process, and is suitable for large-scale industrial production. Therefore, it can be applied to the field of industrial catalysis, especially for the research and development of photoelectric catalytic hydrogen production materials, as well as the fields of nitrogen fixation and CO2 conversion, and has broad application prospects.

Claims

1. A method for preparing a phosphorus-doped TiO2 / phosphorus single substance heterojunction composite thin film photoelectrode, characterized in that: include: (1) immersing a titanium metal sheet in a NaOH solution for a hydrothermal reaction, washing and drying the titanium metal sheet after the reaction, and then placing the titanium metal sheet in a hydrochloric acid solution for acidification. The acidified titanium metal sheet is calcined to in-situ grow a TiO2 nanofiber film on the titanium metal sheet; (2) A titanium metal sheet with an in-situ grown TiO2 nanofiber film, excess black phosphorus and iodine are placed in a quartz tube, the quartz tube is evacuated and sealed, and calcined. After cooling to room temperature, the titanium metal sheet is washed and dried to obtain a phosphorus-doped TiO2 / phosphorus single-element heterojunction composite thin film photoelectrode.

2. The method for preparing the phosphorus-doped TiO2 / phosphorus heterojunction composite thin film photoelectrode according to claim 1, characterized in that: Prior to step (1), the method further comprises the following steps: immersing the titanium metal sheet in a mixed acid for surface polishing, wherein the mixed acid is a mixed aqueous solution of HF and HNO3.

3. The method for preparing the phosphorus-doped TiO2 / phosphorus heterojunction composite thin film photoelectrode according to claim 1, characterized in that: The concentration of NaOH in the NaOH solution is 1 to 4.5 mol / L.

4. The method for preparing the phosphorus-doped TiO2 / phosphorus heterojunction composite thin film photoelectrode according to claim 1, characterized in that: In step (1), the temperature of the hydrothermal reaction is 180-210° C. and the time is 24-48 hours.

5. The method for preparing the phosphorus-doped TiO2 / phosphorus single substance heterojunction composite thin film photoelectrode according to claim 1, characterized in that: In step (1), the calcination temperature is 450-700°C.

6. The method for preparing the phosphorus-doped TiO2 / phosphorus single substance heterojunction composite thin film photoelectrode according to claim 1, characterized in that: In step (2), the preparation method of black phosphorus is: fully mixing red phosphorus, tin powder and iodine particles, and encapsulating the mixture into a quartz tube under vacuum conditions; calcining the quartz tube to obtain black phosphorus crystals.

7. The method for preparing the phosphorus-doped TiO2 / phosphorus heterojunction composite thin film photoelectrode according to claim 6, characterized in that: The mass ratio of red phosphorus, tin powder and iodine is 20:2:

1.

8. The method for preparing the phosphorus-doped TiO2 / phosphorus heterojunction composite thin film photoelectrode according to claim 1, characterized in that: In step (2), the calcination temperature is 550-650° C. and the calcination time is 3-6 hours.

9. A phosphorus-doped TiO2 / phosphorus heterojunction composite thin film photoelectrode obtained by the preparation method according to any one of claims 1 to 8, characterized in that: It is a one-dimensional core-shell structure, with the inner core layer being phosphorus-doped TiO2 and the outer shell being phosphorus alone.

10. Use of the phosphorus-doped TiO2 / phosphorus heterojunction composite thin film photoelectrode according to claim 8 in photoelectrocatalytic hydrogen production, nitrogen fixation or CO2 conversion.