Preparation process of biodegradable antibacterial deodorizing spun-bonded non-woven fabric

By using biodegradable materials such as polylactic acid and natural plant ingredients, combined with ultrasonic and ultraviolet treatment, highly efficient biodegradable antibacterial and deodorizing spunbond non-woven fabrics are prepared, which solves the problem of the weakening of the function of spunbond non-woven fabrics during the degradation process. , achieving efficient environmental friendliness and antibacterial and deodorizing properties.

CN118756433AInactive Publication Date: 2024-10-11PINGXIANG XIAORI TECH CO LTD
View PDF 0 Cites 0 Cited by

Patent Information

Application Number
CN202411092883.3
Authority / Receiving Office
CN · China
Patent Type
Applications(China)
Current Assignee / Owner
Filing Date
2024-08-09
Publication Date
2024-10-11
Estimated Expiration
Not applicable · inactive patent

AI Technical Summary

Technical Problem

The functions of existing spunbond non-woven fabrics are weakened during the degradation process or it is difficult to achieve biodegradability, leading to environmental pollution, and it is difficult to have antibacterial and deodorizing functions and good physical properties at the same time.

Method used

Using materials such as polylactic acid, natural plant resin, eucalyptus oil and epoxy soybean oil, through a specific spinning process and hot rolling bonding process, combined with ultrasonic treatment and ultraviolet deodorization, a biodegradable antibacterial and deodorizing spunbond is prepared Non-woven fabric.

Benefits of technology

It achieves high biodegradability of spunbond non-woven fabrics, with a decomposition rate of 96.5-98.3%, antibacterial and bacteriostatic rates as high as 96.2-99.4%, and improves the physical properties of non-woven fabrics, such as peel strength and tensile strength, The service life is extended and production energy consumption and emissions are reduced.

✦ Generated by Eureka AI based on patent content.

Smart Images

  • Figure BDA0004987070180000091
    Figure BDA0004987070180000091
  • Figure BDA0004987070180000101
    Figure BDA0004987070180000101
Patent Text Reader

Abstract

The invention provides a preparation process of a biodegradable antibacterial deodorizing spun-bonded non-woven fabric, which comprises the following steps: S1, spinning, S2, bonding, S3, finishing and the like, comprising the following raw materials in parts by weight: 40-80 parts of a polymer, 12-52 parts of natural plant resin, 8-12 parts of chlorogenic acid, 5-8 parts of eucalyptus oil, 2-4 parts of glycerol and 3-7 parts of epoxidized soybean oil, the non-woven fabric prepared by a specific combination and spunbond process of the degradable polymer and the natural plant resin has better biodegradability and excellent physical properties, the decomposition rate is 96.5-98.3%, and the degradation rate is 96.5-98.3%. According to the present invention, the peeling strength is 40.5-48.1 N / m, the tensile strength is 39.3-42.4 MPa, the natural plant resin has characteristics of good antibacterial property, and the eucalyptus oil and the epoxidized soybean oil are added so as to provide the antibacterial effect, such that the staphylococcus aureus inhibition rate is 96.2-98.3%, the escherichia coli inhibition rate is 96.5-98.6%, and the candida albicans inhibition rate is 97.1-99.4%; the non-woven fabric has wide application prospects in the fields of medical treatment, sanitation, home furnishing, packaging and the like.
Need to check novelty before this filing date? Find Prior Art

Description

Technical Field

[0001] The invention relates to the technical field of nonwoven fabric processing, and in particular to a preparation process of a biodegradable antibacterial and deodorizing spunbonded nonwoven fabric. Background Art

[0002] Spunbond nonwoven fabric is an important textile material. It is made by extruding and stretching polymers to form continuous filaments, and then laying the filaments into a net. The fiber net is then bonded, thermally bonded, chemically bonded or mechanically reinforced to make the fiber net into a nonwoven fabric. It is widely used in the fields of medical, health, packaging, etc. It has the characteristics of high production efficiency, low cost, and excellent performance. However, there are some difficulties and challenges in the process of spunbond nonwoven fabric. Degradable antibacterial and deodorizing spunbond nonwoven fabrics are difficult to degrade because the molecular structure of polypropylene is a saturated carbon-carbon single bond, and the relative molecular structure is relatively stable. Such simple polypropylene spunbond nonwoven fabrics bring convenience to people's production and life, but also cause great environmental pollution. The degradation rate of biodegradable materials in the natural environment is affected by many factors, such as temperature, humidity, and microbial species. In the process of preparing spunbond nonwoven fabrics, it is necessary to accurately control the degradation degree of the material to ensure that the product can be effectively degraded at the end of its service life, while avoiding premature degradation. The degradation of product performance; therefore, the preparation and research of environmentally friendly and degradable polypropylene composite spunbond nonwoven fabrics is particularly important. Polylactic acid is a biodegradable polymer with excellent biocompatibility and mechanical properties. However, it is difficult to achieve and maintain antibacterial and deodorizing functions while degrading. Adding antibacterial and deodorizing ingredients to spunbond nonwovens can give the product these functions. However, these ingredients may be lost over time or damaged during the production process, resulting in weakened or lost functions. Summary of the invention

[0003] In view of this, the present invention proposes a preparation process of a biodegradable antibacterial and deodorizing spunbonded nonwoven fabric to solve the above problems.

[0004] The technical solution of the present invention is achieved as follows: A preparation process of a biodegradable antibacterial and deodorizing spunbonded nonwoven fabric comprises the following steps:

[0005] S1, spinning: put the polymerized degradable material into a reaction container, heat it to 50-80°C, stir and mix evenly, react for 30-50 minutes, extrude it through a fine-pore plate to form polymer spinning, and airflow draws the spinning into a web;

[0006] S2, bonding: spinning the polymer formed above and bonding it through heat treatment to obtain a spunbond nonwoven fabric;

[0007] S3, finishing: testing, drying, calendering, deodorizing and waterproofing the above spunbond nonwoven fabric to obtain a biodegradable antibacterial and deodorizing spunbond nonwoven fabric.

[0008] Furthermore, the polymerized degradable material in S1 comprises the following raw materials in parts by weight: 40-80 parts of polymer, 12-52 parts of natural plant resin, 8-12 parts of chlorogenic acid, 5-8 parts of eucalyptus oil, 2-4 parts of glycerol, and 3-7 parts of epoxidized soybean oil.

[0009] Furthermore, the polymers in S1 are polylactic acid, poly 3-hydroxyalkanoate and polyvinyl butyral in a mass ratio of (10-15):(5-8):(2-4).

[0010] Furthermore, the natural plant resin in S1 is at least one or a combination of cashew nut shell oil resin, tung oil resin, rosin resin, shellac resin, copal resin, frankincense resin, and carnauba resin.

[0011] Furthermore, the spinning in S1 comprises the following specific steps:

[0012] i) The polymer is vacuum dried at 40-60°C and sliced ​​using a slicer with a thickness of 10-30 mm.

[0013] ii), adding the pretreated polymer and natural plant resin into a reactor, heating to 50-80°C, stirring and mixing at a rate of 200-500rpm, reacting for 30-50min, adding the above-mentioned weight portions of chlorogenic acid, eucalyptus oil, glycerin, and epoxidized soybean oil, and continuing to heat to 70-90°C and stirring for 15-25min to obtain a mixed solution I;

[0014] iii), adding a protective agent to the mixed solution I while stirring, and placing the mixed solution in an ultrasonic container after continuous stirring for 5-15 minutes, turning on the ultrasonic device, and applying ultrasonic waves to the spinning solution, so that bubbles rise rapidly and escape to the surface through ultrasonic vibration and cavitation effect, thereby obtaining a mixed solution II;

[0015] iv), adding the mixed liquid II into a twin-screw extruder, and melt-kneading at a temperature of 120-160° C. to obtain a mixed liquid III;

[0016] Furthermore, the protective agent in iii) is a silicate, polyethylene glycol and polysiloxane with a mass volume ratio of g / mL of (2.5-5.5):(6-8):10, and the added amount of the protective agent is 2-4% of the volume of the mixed solution I.

[0017] Furthermore, in the above iii), the ultrasonic frequency is 20-40kHz, the power is 10-100W, and the ultrasonic time is 2-15min.

[0018] Furthermore, the bonding of S2 uses a hot rolling forming process, and the multi-layer polymer spinning is conveyed to a hot rolling mill, the line pressure of the hot rolling mill is controlled to be 80-100N / mm, the upper roller temperature is 80-120°C, the lower roller temperature is 100-140°C, the mill heat melt ratio is >14%, and hot rolling bonding is performed to obtain a spunbonded non-woven fabric.

[0019] Furthermore, the deodorization is performed by irradiating the spunbonded nonwoven fabric with ultraviolet rays for 30-60 minutes.

[0020] Furthermore, the ultraviolet wavelength range is 250-260nm, and the ultraviolet intensity is 300-400μW·s / cm 2 , temperature is 20-40℃, relative humidity is 50-70%.

[0021] Compared with the prior art, the present invention has the following beneficial effects:

[0022] The spun nonwoven fabric of the present invention has high biodegradability. By adopting specific biodegradable polymers and natural plant resins, the nonwoven fabric can be decomposed into harmless substances such as water and carbon dioxide by microorganisms after use, thereby reducing pollution to the environment. The decomposition rate is 96.5-98.3%. The nonwoven fabric has antibacterial and deodorizing functions. The nonwoven fabric is added with antibacterial natural plant resins, eucalyptus oil and epoxidized soybean oil components. These components can destroy the biofilm and cell wall of bacteria, thereby playing an antibacterial and bacteriostatic role. The antibacterial rate of Staphylococcus aureus is 96.2-98.3%, the antibacterial rate of Escherichia coli is 96.5-98.6%, and the antibacterial rate of Bacillus aureus is 96.2-98.3%. The antibacterial rate of Candida albicans is 97.1-99.4%; the non-woven fabric prepared by the spunbond process has excellent physical properties, and ultrasonic defoaming is used to promote uniform density of the non-woven fabric, good air permeability, and improve the peel strength and tensile strength of the non-woven fabric. Adding the protective agent of the present invention can prevent the spun non-woven fabric from being mechanically damaged during the ultrasonic defoaming process, thereby improving the mechanical properties of the non-woven fabric, the peel strength is 40.5-48.1N / m, and the tensile strength is 39.3-42.4MPa, so that the non-woven fabric can maintain a stable shape and performance during use, thereby improving its service life and practicality.

[0023] The nonwoven fabric of the present invention is biodegradable and will not cause long-term pollution to the environment. At the same time, the materials and processes used in the preparation process also meet environmental protection requirements, reducing energy consumption and emissions in the production process; since the nonwoven fabric has antibacterial and deodorizing properties and is biodegradable, it has broad application prospects in the fields of medical care, hygiene, household, packaging, etc. This multifunctional nonwoven fabric product can meet the needs of different fields and improve its market competitiveness. DETAILED DESCRIPTION

[0024] In order to better understand the technical content of the present invention, specific embodiments are provided below to further illustrate the present invention.

[0025] Unless otherwise specified, the experimental methods used in the embodiments of the present invention are all conventional methods.

[0026] Unless otherwise specified, the materials, reagents, etc. used in the embodiments of the present invention can be obtained from commercial sources.

[0027] Example 1

[0028] A preparation process of a biodegradable antibacterial and deodorizing spunbonded nonwoven fabric comprises the following steps:

[0029] S1. Put the polymerized degradable material into a reaction vessel, heat it to 50°C, stir and mix evenly, react for 30 minutes, extrude it through a fine-pore plate to form polymer spinning, and draw the airflow to form a net.

[0030] The polymeric degradable material comprises the following raw materials in parts by weight: 40 parts of polymer, 12 parts of cashew nut shell oil resin, 8 parts of chlorogenic acid, 5 parts of eucalyptus oil, 2 parts of glycerol, and 3 parts of epoxidized soybean oil;

[0031] The polymer is polylactic acid, poly 3-hydroxyalkanoate and polyvinyl butyral in a mass ratio of 10:5:2;

[0032] Specific steps:

[0033] i) The polymer was vacuum dried at 40°C and sliced ​​using a slicer with a thickness of 10 mm.

[0034] ii), the pretreated polymer and cashew nut shell oil resin were put into a reactor, heated to 50°C, stirred and mixed at a rate of 200 rpm, reacted for 30 minutes, and then the above-mentioned weight parts of chlorogenic acid, eucalyptus oil, glycerin, and epoxidized soybean oil were added, and the temperature was continued to be raised to 70°C and stirred for 15 minutes to obtain a mixed solution I;

[0035] iii), adding a protective agent to the mixed solution I while stirring, wherein the protective agent is a silicate, polyethylene glycol and polysiloxane with a mass volume ratio of g / mL of 2.5:6:10, and the amount of the protective agent added is 2% of the volume of the mixed solution I. After continuous stirring for 5 minutes, the mixed solution is placed in an ultrasonic container, and the ultrasonic equipment is turned on to apply ultrasonic waves to the spinning solution. The ultrasonic frequency is 20kHz, the power is 10W, and the ultrasonic wave is performed for 2 minutes to obtain a mixed solution II;

[0036] iv), adding the mixed liquid II into a twin-screw extruder, and melt-kneading at a temperature of 120° C. to obtain a mixed liquid III;

[0037] S2, bonding: bonding the polymer spun yarn formed above by hot rolling forming process, conveying the multi-layer polymer spun yarn to a hot rolling mill, controlling the line pressure of the hot rolling mill to be 80N / mm, the upper roller temperature to be 80°C, the lower roller temperature to be 100°C, the mill heat melt ratio to be greater than 14%, hot rolling bonding to obtain a spunbonded nonwoven fabric;

[0038] S3, finishing: testing, drying, calendering, deodorizing, and waterproofing the spunbond nonwoven fabric, and irradiating the spunbond nonwoven fabric with ultraviolet light for 30 minutes for deodorizing, with the ultraviolet light wavelength range of 250nm and the ultraviolet light intensity of 300μW·s / cm 2 , temperature is 20°C, relative humidity is 50%, and biodegradable antibacterial and deodorizing spunbonded nonwoven fabric is obtained.

[0039] Example 2

[0040] A preparation process of a biodegradable antibacterial and deodorizing spunbonded nonwoven fabric comprises the following steps:

[0041] S1. Put the polymerized degradable material into a reaction vessel, heat it to 80°C, stir and mix evenly, react for 50 minutes, extrude it through a fine-mesh plate to form polymer spinning, and draw the spinning into a web with airflow.

[0042] The polymeric degradable material comprises the following raw materials in parts by weight: 80 parts of polymer, 52 parts of tung oil resin, 12 parts of chlorogenic acid, 8 parts of eucalyptus oil, 4 parts of glycerol, and 7 parts of epoxidized soybean oil;

[0043] The polymer is polylactic acid, poly 3-hydroxyalkanoate and polyvinyl butyral in a mass ratio of 15:8:4;

[0044] Specific steps:

[0045] i) The polymer was vacuum dried at 60°C and sliced ​​using a slicer with a thickness of 30 mm.

[0046] ii), adding the pretreated polymer and tung oil resin into a reactor, heating to 80°C, stirring and mixing at a rate of 500 rpm, reacting for 50 minutes, adding the above-mentioned weight parts of chlorogenic acid, eucalyptus oil, glycerin, and epoxidized soybean oil, and continuing to heat to 90°C and stirring for 25 minutes to obtain a mixed solution I;

[0047] iii), adding a protective agent to the mixed solution I while stirring, wherein the protective agent is a silicate, polyethylene glycol and polysiloxane with a mass volume ratio of 5.5:8:10 g / mL, and the amount of the protective agent added is 4% of the volume of the mixed solution I, and the mixed solution is placed in an ultrasonic container after continuous stirring for 15 minutes, and the ultrasonic equipment is turned on to apply ultrasonic waves to the spinning solution, the ultrasonic frequency is 40kHz, the power is 100W, and the ultrasonic wave is applied for 15 minutes to obtain a mixed solution II;

[0048] iv), adding the mixed liquid II into a twin-screw extruder, and melt-kneading at a temperature of 160° C. to obtain a mixed liquid III;

[0049] S2, bonding: bonding the polymer spun yarn formed above by hot rolling forming process, conveying the multi-layer polymer spun yarn to a hot rolling mill, controlling the line pressure of the hot rolling mill to be 100N / mm, the upper roller temperature to be 120°C, the lower roller temperature to be 140°C, the mill heat melt ratio to be greater than 14%, hot rolling bonding to obtain a spunbonded nonwoven fabric;

[0050] S3, finishing: testing, drying, calendering, deodorizing, and waterproofing the spunbond nonwoven fabric, and irradiating the spunbond nonwoven fabric with ultraviolet light for 60 minutes for deodorizing, with the ultraviolet light wavelength range of 260nm and the ultraviolet light intensity of 400μW·s / cm 2 , temperature is 40°C, relative humidity is 70%, and biodegradable antibacterial and deodorizing spunbonded nonwoven fabric is obtained.

[0051] Example 3

[0052] A preparation process of a biodegradable antibacterial and deodorizing spunbonded nonwoven fabric comprises the following steps:

[0053] S1. Put the polymerized degradable material into a reaction vessel, heat it to 70°C, stir and mix evenly, react for 40 minutes, extrude it through a fine-pore plate to form polymer spinning, and airflow draws the spinning into a net.

[0054] The polymeric degradable material comprises the following raw materials in parts by weight: 60 parts of polymer, 30 parts of rosin resin, 10 parts of chlorogenic acid, 7 parts of eucalyptus oil, 3 parts of glycerol, and 5 parts of epoxidized soybean oil;

[0055] The polymer is polylactic acid, poly 3-hydroxyalkanoate and polyvinyl butyral in a mass ratio of 12:7:3;

[0056] Specific steps:

[0057] i) The polymer was vacuum dried at 50°C and sliced ​​using a slicer with a thickness of 20 mm.

[0058] ii), adding the pretreated polymer and rosin resin into a reactor, heating to 70°C, stirring and mixing at a rate of 300 rpm, reacting for 40 minutes, adding the above-mentioned weight parts of chlorogenic acid, eucalyptus oil, glycerin, and epoxidized soybean oil, and continuing to heat to 80°C and stirring for 20 minutes to obtain a mixed solution I;

[0059] iii), adding a protective agent to the mixed solution I while stirring, wherein the protective agent is a silicate, polyethylene glycol and polysiloxane in a mass volume ratio of 4:7:10 g / mL, and the amount of the protective agent added is 3% of the volume of the mixed solution I, and the mixed solution is placed in an ultrasonic container after continuous stirring for 10 minutes, and the ultrasonic equipment is turned on to apply ultrasonic waves to the spinning solution, the ultrasonic frequency is 30kHz, the power is 50W, and the ultrasonic wave is performed for 8 minutes to obtain a mixed solution II;

[0060] iv), adding the mixed liquid II into a twin-screw extruder, and melt-kneading at a temperature of 140° C. to obtain a mixed liquid III;

[0061] S2, bonding: bonding the polymer spun yarn formed above by hot rolling forming process, conveying the multi-layer polymer spun yarn to a hot rolling mill, controlling the line pressure of the hot rolling mill to be 90N / mm, the upper roller temperature to be 100°C, the lower roller temperature to be 130°C, the mill heat melt ratio to be greater than 14%, hot rolling bonding to obtain a spunbonded nonwoven fabric;

[0062] S3. Finishing: The spunbond nonwoven fabric is tested, dried, calendered, deodorized, and waterproofed. The spunbond nonwoven fabric is deodorized by irradiating it with ultraviolet light for 45 minutes. The ultraviolet light has a wavelength of 255 nm and an intensity of 350 μW·s / cm 2 , temperature is 30°C, relative humidity is 60%, and biodegradable antibacterial and deodorizing spunbonded nonwoven fabric is obtained.

[0063] Example 4

[0064] A preparation process of a biodegradable antibacterial and deodorizing spunbonded nonwoven fabric comprises the following steps:

[0065] S1. Put the polymerized degradable material into a reaction vessel, heat it to 70°C, stir and mix evenly, react for 40 minutes, extrude it through a fine-pore plate to form polymer spinning, and airflow draws the spinning into a net.

[0066] The polymeric degradable material comprises the following raw materials in parts by weight: 40 parts of polymer, 12 parts of rosin resin, 8 parts of chlorogenic acid, 5 parts of eucalyptus oil, 2 parts of glycerol, and 3 parts of epoxidized soybean oil;

[0067] The polymer is polylactic acid, poly 3-hydroxyalkanoate and polyvinyl butyral in a mass ratio of 12:7:3;

[0068] Specific steps:

[0069] i) The polymer was vacuum dried at 50°C and sliced ​​using a slicer with a thickness of 20 mm.

[0070] ii), adding the pretreated polymer and rosin resin into a reactor, heating to 70°C, stirring and mixing at a rate of 300 rpm, reacting for 40 minutes, adding the above-mentioned weight parts of chlorogenic acid, eucalyptus oil, glycerin, and epoxidized soybean oil, and continuing to heat to 80°C and stirring for 20 minutes to obtain a mixed solution I;

[0071] iii), adding a protective agent to the mixed solution I while stirring, wherein the protective agent is a silicate, polyethylene glycol and polysiloxane in a mass volume ratio of 4:7:10 g / mL, and the amount of the protective agent added is 3% of the volume of the mixed solution I, and the mixed solution is placed in an ultrasonic container after continuous stirring for 10 minutes, and the ultrasonic equipment is turned on to apply ultrasonic waves to the spinning solution, the ultrasonic frequency is 30kHz, the power is 50W, and the ultrasonic wave is performed for 8 minutes to obtain a mixed solution II;

[0072] iv), adding the mixed liquid II into a twin-screw extruder, and melt-kneading at a temperature of 140° C. to obtain a mixed liquid III;

[0073] S2, bonding: bonding the polymer spun yarn formed above by hot rolling forming process, conveying the multi-layer polymer spun yarn to a hot rolling mill, controlling the line pressure of the hot rolling mill to be 90N / mm, the upper roller temperature to be 100°C, the lower roller temperature to be 130°C, the mill heat melt ratio to be greater than 14%, hot rolling bonding to obtain a spunbonded nonwoven fabric;

[0074] S3. Finishing: The spunbond nonwoven fabric is tested, dried, calendered, deodorized, and waterproofed. The spunbond nonwoven fabric is deodorized by irradiating it with ultraviolet light for 45 minutes. The ultraviolet light has a wavelength of 255 nm and an intensity of 350 μW·s / cm 2 , temperature is 30°C, relative humidity is 60%, and biodegradable antibacterial and deodorizing spunbonded nonwoven fabric is obtained.

[0075] Example 5

[0076] A preparation process of a biodegradable antibacterial and deodorizing spunbonded nonwoven fabric comprises the following steps:

[0077] S1. Put the polymerized degradable material into a reaction vessel, heat it to 70°C, stir and mix evenly, react for 40 minutes, extrude it through a fine-pore plate to form polymer spinning, and airflow draws the spinning into a net.

[0078] The polymeric degradable material comprises the following raw materials in parts by weight: 80 parts of polymer, 52 parts of rosin resin, 12 parts of chlorogenic acid, 8 parts of eucalyptus oil, 4 parts of glycerol, and 7 parts of epoxidized soybean oil;

[0079] The polymer is polylactic acid, poly 3-hydroxyalkanoate and polyvinyl butyral in a mass ratio of 12:7:3;

[0080] Specific steps:

[0081] i) The polymer was vacuum dried at 50°C and sliced ​​using a slicer with a thickness of 20 mm.

[0082] ii), adding the pretreated polymer and rosin resin into a reactor, heating to 70°C, stirring and mixing at a rate of 300 rpm, reacting for 40 minutes, adding the above-mentioned weight parts of chlorogenic acid, eucalyptus oil, glycerin, and epoxidized soybean oil, and continuing to heat to 80°C and stirring for 20 minutes to obtain a mixed solution I;

[0083] iii), adding a protective agent to the mixed solution I while stirring, wherein the protective agent is a silicate, polyethylene glycol and polysiloxane in a mass volume ratio of 4:7:10 g / mL, and the amount of the protective agent added is 3% of the volume of the mixed solution I, and the mixed solution is placed in an ultrasonic container after continuous stirring for 10 minutes, and the ultrasonic equipment is turned on to apply ultrasonic waves to the spinning solution, the ultrasonic frequency is 30kHz, the power is 50W, and the ultrasonic wave is performed for 8 minutes to obtain a mixed solution II;

[0084] iv), adding the mixed liquid II into a twin-screw extruder, and melt-kneading at a temperature of 140° C. to obtain a mixed liquid III;

[0085] S2, bonding: bonding the polymer spun yarn formed above by hot rolling forming process, conveying the multi-layer polymer spun yarn to a hot rolling mill, controlling the line pressure of the hot rolling mill to be 90N / mm, the upper roller temperature to be 100°C, the lower roller temperature to be 130°C, the mill heat melt ratio to be greater than 14%, hot rolling bonding to obtain a spunbonded nonwoven fabric;

[0086] S3. Finishing: The spunbond nonwoven fabric is tested, dried, calendered, deodorized, and waterproofed. The spunbond nonwoven fabric is deodorized by irradiating it with ultraviolet light for 45 minutes. The ultraviolet light has a wavelength of 255 nm and an intensity of 350 μW·s / cm 2 , temperature is 30°C, relative humidity is 60%, and biodegradable antibacterial and deodorizing spunbonded nonwoven fabric is obtained.

[0087] Comparative Example 1

[0088] The difference between this comparative example and Example 3 is that the polymerized degradable material does not contain natural plant resin.

[0089] Comparative Example 2

[0090] The difference between this comparative example and Example 3 is that the polymeric degradable material does not contain eucalyptus oil.

[0091] Comparative Example 3

[0092] The difference between this comparative example and Example 3 is that the polymerized degradable material does not contain epoxidized soybean oil.

[0093] Antibacterial performance test

[0094] The antibacterial properties of the spunbonded nonwoven fabrics obtained in Examples 1-5 and Comparative Examples 1-3 were tested with reference to GB / T 20944.2 "Evaluation of antibacterial properties of textiles Part 2: Absorption method";

[0095] 1. Prepare samples: Prepare 8 groups of non-woven fabric samples according to the specified size and weight;

[0096] 2. Preparation of bacterial solution: According to the test requirements, the cultured Staphylococcus aureus, Escherichia coli and Candida albicans were diluted to a concentration of 2×10 6 CFU / mL;

[0097] 3. Inoculation: Immerse the non-woven fabric sample in the bacterial solution to ensure that the bacterial solution is in full contact with the non-woven fabric;

[0098] 4. Cultivation: Place the inoculated non-woven fabric in a constant temperature incubator, culture Staphylococcus aureus and Escherichia coli at 37°C for 24 hours, and Candida albicans at 25°C for 72 hours;

[0099] 5. Elution: Perform immediate elution and elution after culture respectively, determine the number of bacteria in the elution solution and calculate the inhibition value or inhibition rate to evaluate the antibacterial effect of the sample.

[0100] 6. Result expression: When the calculated value of the antibacterial rate is >99%, it is expressed as ">99%". When the antibacterial rate is ≥99%, the sample has a good antibacterial effect. The test results are as follows:

[0101]

[0102] The above results show that the use of natural plant resin, eucalyptus oil and epoxidized soybean oil has better antibacterial properties and can effectively inhibit the growth and reproduction of Staphylococcus aureus, Escherichia coli and Candida albicans.

[0103] Comparative Example 4

[0104] The difference between this comparative example and Example 3 is that in the step iii), no protective agent is added to the mixed solution I. Specifically, the mixed solution I is placed in an ultrasonic container, and the ultrasonic equipment is turned on to apply ultrasonic waves to the spinning solution. The ultrasonic frequency is 30 kHz, the power is 50 W, and the ultrasonic wave is applied for 8 minutes to obtain a mixed solution II.

[0105] Comparative Example 5

[0106] The difference between this comparative example and Example 3 is that the mixed solution I in step iii) is not subjected to ultrasonic defoaming.

[0107] Degradability and strength performance tests:

[0108] (1) Peel strength: According to the standard GB / T2792-2014, a standard non-woven fabric (25 mm*200 mm) was attached to a stainless steel plate wiped clean with alcohol, and pressed back and forth with a 2 kg roller. After being left at room temperature for 20 min, it was tested by a peel strength tester. The test was performed more than three times, and the average value was calculated.

[0109] (2) Tensile strength: The tensile strength of the nonwoven fabrics of Examples 1-5 and Comparative Examples 1-5 was tested according to the method specified in GB / T1040.

[0110] (3) Degradability: The tapes of Examples 1-5 and Comparative Examples 1-5 were cut into 5 samples of 20 m in length and 5 cm in width. The mass m0 before degradation was weighed. The samples were buried in soil with a pH of 6 for 1 month, and the mass m1 after degradation was weighed.

[0111] Decomposition rate = (m0-m1) / m0*100%.

[0112] The decomposition results are shown in the following table:

[0113]

[0114]

[0115] The above results show that the spun nonwoven fabric of the present invention has a high decomposition efficiency, which is 96.5-98.3% in the embodiment group, and has high peel strength and tensile strength, which are 40.5-48.1N / m and 39.3-42.4MPa, respectively. It can be seen from the comparison between the embodiment group and comparative example 1 that the addition of the natural plant resin of the present invention has better degradation ability, and is easily decomposed by microorganisms in the natural environment, and becomes organic matter and returns to nature; compared with comparative examples 2 and 3, eucalyptus oil and epoxidized soybean oil are added in proportion, which can attract microorganisms and stimulate their growth on nonwoven fabrics. Microorganisms decompose the polymer chains in nonwoven fabrics by secreting enzymes, thereby promoting the biodegradation process of nonwoven fabrics. Epoxidized soybean oil itself also has good biodegradability and can be decomposed into smaller molecules by microorganisms, thereby accelerating the degradation of nonwoven fabrics. Compared with Comparative Example 4, the addition of the protective agent of the present invention can prevent the spun non-woven fabric from being mechanically damaged during the ultrasonic defoaming process, thereby improving the mechanical properties of the non-woven fabric; Comparative Example 5 shows that the use of ultrasonic defoaming has a better effect, promotes the uniform density of the non-woven fabric, good air permeability, and improves the peel strength and tensile strength of the non-woven fabric.

[0116] The above description is only a preferred embodiment of the present invention and is not intended to limit the present invention. Any modifications, equivalent substitutions, improvements, etc. made within the spirit and principle of the present invention should be included in the protection scope of the present invention.

Claims

1. A preparation process of a biodegradable antibacterial and deodorizing spunbonded nonwoven fabric. Features: The following steps are involved: S1, spinning: put the polymerized degradable material into a reaction container, heat it to 50-80°C, stir and mix evenly, react for 30-50 minutes, extrude it through a fine-pore plate to form polymer spinning, and airflow draws the spinning into a web; S2, bonding: spinning the polymer formed above and bonding it through heat treatment to obtain a spunbond nonwoven fabric; S3, finishing: testing, drying, calendering, deodorizing and waterproofing the above spunbond nonwoven fabric to obtain a biodegradable antibacterial and deodorizing spunbond nonwoven fabric.

2. A process for preparing a biodegradable antibacterial and deodorizing spunbonded nonwoven fabric as claimed in claim 1, Features: The polymerized degradable material in S1 comprises the following raw materials in parts by weight: 40-80 parts of polymer, 12-52 parts of natural plant resin, 8-12 parts of chlorogenic acid, 5-8 parts of eucalyptus oil, 2-4 parts of glycerol, and 3-7 parts of epoxidized soybean oil.

3. A process for preparing a biodegradable antibacterial and deodorizing spunbonded nonwoven fabric as claimed in claim 2, Features: The polymers in S1 are polylactic acid, poly 3-hydroxyalkanoate and polyvinyl butyral in a mass ratio of (10-15):(5-8):(2-4).

4. A process for preparing a biodegradable antibacterial and deodorizing spunbonded nonwoven fabric as claimed in claim 2, Features: The natural plant resin in S1 is at least one of cashew nut shell oil resin, tung oil resin, rosin resin, shellac resin, copal resin, frankincense resin, and carnauba resin, or a combination of several of them.

5. A process for preparing a biodegradable antibacterial and deodorizing spunbonded nonwoven fabric as claimed in claim 1, Features: The spinning in S1 comprises the following specific steps: i) The polymer is vacuum dried at 40-60°C and sliced ​​using a slicer with a thickness of 10-30 mm. ii), adding the pretreated polymer and natural plant resin into a reactor, heating to 50-80°C, stirring and mixing at a rate of 200-500rpm, reacting for 30-50min, adding the above-mentioned weight portions of chlorogenic acid, eucalyptus oil, glycerin, and epoxidized soybean oil, and continuing to heat to 70-90°C and stirring for 15-25min to obtain a mixed solution I; iii), adding a protective agent to the mixed solution I while stirring, and placing the mixed solution in an ultrasonic container after continuous stirring for 5-15 minutes, turning on the ultrasonic equipment, and applying ultrasonic waves to the spinning solution to obtain a mixed solution II; iv), adding the mixed liquid II into a twin-screw extruder, and melt-kneading at a temperature of 120-160° C. to obtain a mixed liquid III; v) The mixed liquid III is stretched and sucked for spinning at a rotation speed of 20-40 rpm and a temperature of 160-180° C. to obtain polymer spinning, which is air-drawn into a web, and the fiber fineness is less than 0.01 Den.

6. A process for preparing a biodegradable antibacterial and deodorizing spunbonded nonwoven fabric as claimed in claim 5, Features: The protective agent in said iii) is silicate, polyethylene glycol and polysiloxane with a mass volume ratio of g / mL of (2.5-5.5):(6-8):10, and the added amount of the protective agent is 2-4% of the volume of the mixed solution I.

7. A process for preparing a biodegradable antibacterial and deodorizing spunbonded nonwoven fabric as claimed in claim 5, Features: In the above iii), the ultrasonic frequency is 20-40kHz, the power is 10-100W, and the ultrasonic treatment lasts for 2-15min.

8. A process for preparing a biodegradable antibacterial and deodorizing spunbonded nonwoven fabric as claimed in claim 1, Features: The bonding of S2 uses a hot rolling forming process, and the multi-layer polymer spinning is conveyed to a hot rolling mill, and the line pressure of the hot rolling mill is controlled to be 80-100N / mm, the upper roller temperature is 80-120°C, the lower roller temperature is 100-140°C, the mill heat melt ratio is greater than 14%, and hot rolling bonding is performed to obtain a spunbonded nonwoven fabric.

9. A process for preparing a biodegradable antibacterial and deodorizing spunbonded nonwoven fabric as claimed in claim 1, Features: The deodorization is performed by irradiating the spunbonded nonwoven fabric with ultraviolet rays for 30-60 minutes.

10. A process for preparing a biodegradable antibacterial and deodorizing spunbonded nonwoven fabric as claimed in claim 9, Features: The ultraviolet wavelength range is 250-260nm, and the ultraviolet intensity is 300-400μW·s / cm 2 , temperature is 20-40℃, relative humidity is 50-70%.