Method and device for evaluating dielectric properties of modified silicone rubber, and electronic equipment

By simulating the electrical branch damage coefficient and dielectric factor of modified silicone rubber under high voltage environment and calculating the evaluation score, the problem of dielectric performance evaluation of modified silicone rubber is solved, and the selection accuracy and insulation performance of transformer materials are improved.

CN118759327BActive Publication Date: 2024-11-29FOSHAN POWER SUPPLY BUREAU GUANGDONG POWER GRID
View PDF 2 Cites 0 Cited by

Patent Information

Application Number
CN202411228179.6
Authority / Receiving Office
CN · China
Patent Type
Patents(China)
Current Assignee / Owner
Filing Date
2024-09-03
Publication Date
2024-11-29
Estimated Expiration
2044-09-03

AI Technical Summary

Technical Problem

The prior art lacks effective methods to accurately and effectively evaluate the dielectric properties of modified silicone rubber, making it difficult to select materials with higher dielectric properties for transformers.

Method used

By obtaining the target experimental platform and control experimental samples, simulate the high-voltage operating environment, measure the electrical branch damage coefficient and dielectric factor of the modified silicone rubber samples, and calculate the evaluation score to generate dielectric performance evaluation results.

Benefits of technology

Accurate evaluation of the dielectric properties of modified silicone rubber, determine whether it has improved dielectric properties after modification, solves the problem of degradation of dielectric properties in transformers, improves the accuracy of selection of insulating materials and the reliability of transformers sex.

✦ Generated by Eureka AI based on patent content.

Smart Images

  • Figure CN118759327B_ABST
    Figure CN118759327B_ABST
Patent Text Reader

Abstract

The present invention discloses a method and device for evaluating the dielectric properties of modified silicone rubber, and electronic equipment, and relates to the technical field of online monitoring and fault diagnosis of electrical insulation, wherein the method comprises: obtaining a target experimental platform and a control experimental sample; controlling the target experimental platform to simulate a high-voltage operating environment for the control experimental sample, and obtaining simulation experimental results based on a specified simulation cycle, wherein the simulation experimental results comprise: an electrical tree damage coefficient and a dielectric factor of the modified silicone rubber sample; calculating an evaluation score of the modified silicone rubber sample based on the electrical tree damage coefficient and the dielectric factor indicated by the simulation experimental results; and generating a dielectric property evaluation result of the modified silicone rubber sample based on the evaluation score. The present invention solves the technical problem in the related art that the dielectric properties of modified silicone rubber cannot be accurately and effectively evaluated.
Need to check novelty before this filing date? Find Prior Art

Description

Technical Field

[0001] The present invention relates to the technical field of online monitoring and fault diagnosis of electrical insulation, and in particular to a method and device for evaluating the dielectric properties of modified silicone rubber, and electronic equipment. Background Art

[0002] Silicone rubber has good weather resistance due to its high bond energy silicon-oxygen bond. In actual use, it can withstand corona, ozone, tracking and electrical corrosion, and has excellent waterproof properties. Therefore, silicone rubber has gradually replaced many insulating materials and is widely used in many fields, including electronics, automobiles, medical equipment, aerospace, etc. Modified silicone rubber is chemically modified or other inorganic materials are added to traditional silicone rubber to improve its performance. Through modification, the thermal properties, electrical properties and mechanical properties of silicone rubber can be adjusted. They provide higher levels of performance and functions to meet the ever-changing application needs.

[0003] In traditional dry-type transformers, epoxy resin as the main insulating material is very prone to irreversible damage such as cracks and degradation of dielectric properties, which ultimately lead to insulation failure and the end of transformer life. As an excellent insulating material, the dielectric properties of modified silicone rubber can not only meet the basic needs of transformers, but also achieve green recycling and reduce material loss. In order to select modified silicone rubber materials with better dielectric properties for transformers, a series of experiments are required on silicone rubber materials before and after modification to determine the dielectric properties of the modified insulating materials. However, there is currently a lack of effective evaluation methods for the dielectric properties of modified silicone rubber.

[0004] To address the above-mentioned problems, no effective solution has been proposed yet. Summary of the invention

[0005] The embodiments of the present invention provide a method and device for evaluating the dielectric properties of modified silicone rubber, and an electronic device, so as to at least solve the technical problem in the related art that the dielectric properties of modified silicone rubber cannot be accurately and effectively evaluated.

[0006] According to one aspect of an embodiment of the present invention, a method for evaluating the dielectric properties of modified silicone rubber is provided, comprising: obtaining a target experimental platform and a control experimental sample, wherein the target experimental platform is used to detect dielectric property parameters of an insulating material, and the types of the control experimental samples include at least: ordinary silicone rubber samples and modified silicone rubber samples; controlling the target experimental platform to simulate a high-voltage operating environment for the control experimental sample, and obtaining a simulation experimental result based on a specified simulation period, wherein the simulation experimental result includes: an electrical tree damage coefficient and a dielectric factor of the modified silicone rubber sample; calculating an evaluation score of the modified silicone rubber sample based on the electrical tree damage coefficient and the dielectric factor indicated by the simulation experimental result; and generating a dielectric property evaluation result of the modified silicone rubber sample based on the evaluation score.

[0007] Furthermore, the target experimental platform includes: an experimental box, a temperature controller, a temperature sensor, a high-voltage power supply, a dielectric analyzer, an electromagnetic controller, a magnetic flux density meter, an electromagnetic pole plate, a voltmeter, a needle electrode, a ground electrode, a microscopic imaging system and a computer terminal, wherein the experimental box is used to carry the simulated high-voltage operating environment; the temperature controller, the electromagnetic controller, the temperature sensor and the magnetic flux density meter are all arranged on the inner wall of the experimental box, and pre-establish data connections with the computer terminal respectively; the electromagnetic pole plate is arranged in the internal space of the experimental box and is connected to the electromagnetic controller, and the electromagnetic pole plate includes: an N pole plate and an S pole plate; the needle electrode and the ground electrode are arranged in the The ground electrode is used to place the control experimental sample between the N-pole plate and the S-pole plate of the electromagnetic plate, and the needle electrode is aligned with the geometric center of the control experimental sample; the voltmeter is connected in parallel to both ends of the needle electrode and the ground electrode, and a data connection is pre-established with the computer terminal; the positive pole of the high-voltage power supply is connected to the needle electrode, and the negative pole of the high-voltage power supply is connected to the ground electrode; the dielectric analyzer is connected to the control experimental sample, and a data connection is pre-established with the computer terminal to measure the dielectric parameters of the control experimental sample; the microscopic imaging system is configured on the inner wall of the experimental box, and a data connection is pre-established with the computer terminal to monitor the electrical tree parameters of the control experimental sample.

[0008] Furthermore, before controlling the target experimental platform to simulate the high-voltage operating environment for the control experimental sample, it also includes: obtaining winding-related parameters of the target traction transformer after running for a specified period of time in the actual high-voltage operating environment, wherein the target traction transformer refers to a transformer using the ordinary silicone rubber sample and / or the modified silicone rubber sample as the insulating material; determining simulated operating parameters based on the winding-related parameters, and transmitting the simulated operating parameters to the computer terminal of the target experimental platform, wherein the computer terminal controls the target experimental platform to simulate the high-voltage operating environment based on the simulated operating parameters.

[0009] Furthermore, the step of determining the simulated operation parameters based on the winding-related parameters includes: determining the sample quantity R of each type of the control experimental samples, and determining R simulated operation temperatures based on the sample quantity and the winding-side temperature in the winding-related parameters, wherein R is a positive integer; determining R simulated operation magnetic flux densities and R simulated operation voltages based on the sample quantity and the magnetic flux density and the winding-side voltage in the winding-related parameters, respectively; and determining the simulated operation parameters based on the simulated operation temperature, the simulated operation magnetic flux density and the simulated operation voltage.

[0010] Furthermore, the step of controlling the target experimental platform to simulate a high-voltage operating environment for the control experimental sample and obtaining a simulation experimental result based on a specified simulation cycle includes: controlling the target experimental platform to generate the high-voltage operating environment based on the simulation operating parameters, and applying the high-voltage operating environment to the control experimental sample placed in the experimental box; obtaining the electrical tree damage coefficient and dielectric factor of the modified silicone rubber sample in the experimental box after the specified simulation cycle to obtain the simulation experimental result.

[0011] Furthermore, the step of obtaining the electrical tree damage coefficient of the modified silicone rubber sample in the experimental box after the specified simulation cycle includes: after simulating a high-voltage operating environment for the control experimental sample, using the microscopic imaging system of the target experimental platform to respectively obtain the electrical tree length, electrical tree width, electrical tree damage area and fractal dimension of the ordinary silicone rubber sample and the modified silicone rubber sample; substituting the electrical tree length, the electrical tree width, the electrical tree damage area and the fractal dimension into the damage calculation formula to calculate the electrical tree damage coefficient of the modified silicone rubber sample.

[0012] Furthermore, the step of obtaining the dielectric factor of the modified silicone rubber sample in the experimental box after the specified simulation cycle includes: after simulating a high-voltage operating environment for the control experimental sample, using a dielectric analyzer in the target experimental platform to respectively obtain the relative dielectric constant and dielectric loss of the ordinary silicone rubber sample and the modified silicone rubber sample; substituting the relative dielectric constant and the dielectric loss into a dielectric calculation formula to calculate the dielectric factor of the modified silicone rubber sample.

[0013] According to another aspect of an embodiment of the present invention, there is also provided a device for evaluating the dielectric properties of modified silicone rubber, comprising: an acquisition unit, for acquiring a target experimental platform and a control experimental sample, wherein the target experimental platform is used to detect the dielectric performance parameters of the insulating material, and the types of the control experimental samples include at least: ordinary silicone rubber samples and modified silicone rubber samples; a control unit, for controlling the target experimental platform to simulate a high-voltage operating environment for the control experimental sample, and to obtain a simulation experiment result based on a specified simulation period, wherein the simulation experiment result includes: an electrical tree damage coefficient and a dielectric factor of the modified silicone rubber sample; a calculation unit, for calculating an evaluation score of the modified silicone rubber sample based on the electrical tree damage coefficient and the dielectric factor indicated by the simulation experiment result; and a generation unit, for generating a dielectric property evaluation result of the modified silicone rubber sample based on the evaluation score.

[0014] Furthermore, the target experimental platform includes: an experimental box, a temperature controller, a temperature sensor, a high-voltage power supply, a dielectric analyzer, an electromagnetic controller, a magnetic flux density meter, an electromagnetic pole plate, a voltmeter, a needle electrode, a ground electrode, a microscopic imaging system and a computer terminal, wherein the experimental box is used to carry the simulated high-voltage operating environment; the temperature controller, the electromagnetic controller, the temperature sensor and the magnetic flux density meter are all arranged on the inner wall of the experimental box, and pre-establish data connections with the computer terminal respectively; the electromagnetic pole plate is arranged in the internal space of the experimental box and is connected to the electromagnetic controller, and the electromagnetic pole plate includes: an N pole plate and an S pole plate; the needle electrode and the ground electrode are arranged in the The ground electrode is used to place the control experimental sample between the N-pole plate and the S-pole plate of the electromagnetic plate, and the needle electrode is aligned with the geometric center of the control experimental sample; the voltmeter is connected in parallel to both ends of the needle electrode and the ground electrode, and a data connection is pre-established with the computer terminal; the positive pole of the high-voltage power supply is connected to the needle electrode, and the negative pole of the high-voltage power supply is connected to the ground electrode; the dielectric analyzer is connected to the control experimental sample, and a data connection is pre-established with the computer terminal to measure the dielectric parameters of the control experimental sample; the microscopic imaging system is configured on the inner wall of the experimental box, and a data connection is pre-established with the computer terminal to monitor the electrical tree parameters of the control experimental sample.

[0015] Furthermore, the device for evaluating the dielectric properties of modified silicone rubber also includes: a first acquisition module, used to obtain winding-related parameters of a target traction transformer after the target traction transformer has been operating for a specified period of time in an actual high-voltage operating environment, wherein the target traction transformer refers to a transformer using the ordinary silicone rubber sample and / or the modified silicone rubber sample as the insulating material; a transmission module, used to determine simulated operating parameters based on the winding-related parameters, and transmit the simulated operating parameters to a computer terminal of the target experimental platform, wherein the computer terminal controls the target experimental platform to simulate a high-voltage operating environment based on the simulated operating parameters.

[0016] Furthermore, the transmission module includes: a first determination submodule, used to determine the sample quantity R of each type of the control experimental samples, and determine R simulated operating temperatures based on the sample quantity and the winding side temperature in the winding-related parameters, wherein R is a positive integer; a second determination submodule, used to determine R simulated operating magnetic flux densities and R simulated operating voltages based on the sample quantity and the magnetic flux density and winding side voltage in the winding-related parameters; and a third determination submodule, used to determine the simulated operating parameters based on the simulated operating temperature, the simulated operating magnetic flux density and the simulated operating voltage.

[0017] Furthermore, the control unit includes: a control module, used to control the target experimental platform to generate the high-voltage operating environment based on the simulated operating parameters, and apply the high-voltage operating environment to the control experimental sample placed in the experimental box; a second acquisition module, used to obtain the electrical tree damage coefficient and dielectric factor of the modified silicone rubber sample in the experimental box after the specified simulation cycle to obtain the simulation experiment results.

[0018] Furthermore, the second acquisition module includes: a first acquisition submodule, which is used to use the microscopic imaging system of the target experimental platform to respectively obtain the electrical tree length, electrical tree width, electrical tree damage area and fractal dimension of the ordinary silicone rubber sample and the modified silicone rubber sample after simulating a high-voltage operating environment for the control experimental sample; and a second calculation submodule, which is used to substitute the electrical tree length, the electrical tree width, the electrical tree damage area and the fractal dimension into the damage calculation formula to calculate the electrical tree damage coefficient of the modified silicone rubber sample.

[0019] Furthermore, the second acquisition module also includes: a second acquisition submodule, which is used to obtain the relative dielectric constant and dielectric loss of the ordinary silicone rubber sample and the modified silicone rubber sample respectively using the dielectric analyzer in the target experimental platform after simulating a high-voltage operating environment for the control experimental sample; and a second calculation submodule, which is used to substitute the relative dielectric constant and the dielectric loss into the dielectric calculation formula to calculate the dielectric factor of the modified silicone rubber sample.

[0020] According to another aspect of an embodiment of the present invention, a computer-readable storage medium is also provided, wherein the computer-readable storage medium includes a stored computer program, wherein when the computer program is running, the device where the computer-readable storage medium is located is controlled to execute any one of the above-mentioned methods for evaluating the dielectric properties of modified silicone rubber.

[0021] According to another aspect of an embodiment of the present invention, there is also provided an electronic device, comprising one or more processors and a memory, wherein the memory is used to store one or more programs, wherein when the one or more programs are executed by the one or more processors, the one or more processors implement any one of the above-mentioned methods for evaluating the dielectric properties of modified silicone rubber.

[0022] In the present invention, a method for evaluating the dielectric properties of modified silicone rubber is proposed. First, a target experimental platform and a control experimental sample are obtained, wherein the target experimental platform is used to detect the dielectric performance parameters of the insulating material, and the types of the control experimental samples include at least: ordinary silicone rubber samples and modified silicone rubber samples. Then, the target experimental platform is controlled to simulate a high-voltage operating environment for the control experimental sample, and a simulation experiment result is obtained based on a specified simulation cycle, wherein the simulation experiment result includes: an electrical tree damage coefficient and a dielectric factor of the modified silicone rubber sample. Then, an evaluation score of the modified silicone rubber sample is calculated based on the electrical tree damage coefficient and the dielectric factor indicated by the simulation experiment result, and finally, a dielectric property evaluation result of the modified silicone rubber sample is generated based on the evaluation score.

[0023] In the present invention, a control simulation experiment is carried out on ordinary silicone rubber insulating materials and modified silicone rubber insulating materials through a multi-field coupling experimental platform, and the electrical tree damage coefficient and dielectric factor of the two insulating material samples after the high-voltage operation simulation test under the same experimental conditions are obtained, and the evaluation score of the modified silicone rubber insulating material is calculated. The evaluation score is used to judge the dielectric properties of the modified silicone rubber insulating material, and then it is judged whether the dielectric properties of the silicone rubber insulating material used for transformers after different surface modifications are improved, which solves the technical problem that the dielectric properties of the modified silicone rubber cannot be accurately and effectively evaluated in the related art. BRIEF DESCRIPTION OF THE DRAWINGS

[0024] The drawings described herein are used to provide a further understanding of the present invention and constitute a part of this application. The exemplary embodiments of the present invention and their descriptions are used to explain the present invention and do not constitute an improper limitation of the present invention. In the drawings:

[0025] Figure 1 is a flow chart of an optional method for evaluating the dielectric properties of modified silicone rubber according to an embodiment of the present invention;

[0026] Figure 2 is a schematic diagram of an optional test platform for dielectric properties of modified silicone rubber according to an embodiment of the present invention;

[0027] Figure 3 is a flow chart of an optional method for evaluating the dielectric properties of modified silicone rubber based on electrical tree distribution for transformers according to an embodiment of the present invention;

[0028] Figure 4 is a schematic diagram of an optional device for evaluating the dielectric properties of modified silicone rubber according to an embodiment of the present invention;

[0029] Figure 5 is a schematic diagram of an optional electronic device according to an embodiment of the present invention. DETAILED DESCRIPTION

[0030] In order to enable those skilled in the art to better understand the scheme of the present invention, the technical scheme in the embodiments of the present invention will be clearly and completely described below in conjunction with the drawings in the embodiments of the present invention. Obviously, the described embodiments are only part of the embodiments of the present invention, not all of the embodiments. Based on the embodiments of the present invention, all other embodiments obtained by ordinary technicians in this field without creative work should fall within the scope of protection of the present invention.

[0031] It should be noted that the terms "first", "second", etc. in the specification and claims of the present invention and the above-mentioned drawings are used to distinguish similar objects, and are not necessarily used to describe a specific order or sequence. It should be understood that the data used in this way can be interchanged where appropriate, so that the embodiments of the present invention described herein can be implemented in an order other than those illustrated or described herein. In addition, the terms "including" and "having" and any variations thereof are intended to cover non-exclusive inclusions, for example, a process, method, system, product or device that includes a series of steps or units is not necessarily limited to those steps or units that are clearly listed, but may include other steps or units that are not clearly listed or inherent to these processes, methods, products or devices.

[0032] The following embodiments of the present invention can be applied to various systems / applications / equipment that require dielectric property testing and insulation performance detection of insulating materials, and can provide a basis for the selection of insulating materials based on dielectric property testing. The present invention conducts a comparative simulation experiment on ordinary silicone rubber samples and modified silicone rubber samples through a multi-field coupling experimental platform to obtain the electrical tree damage coefficient and dielectric factor, and then calculates the evaluation score of the modified silicone rubber insulating material, which can better judge the dielectric properties of the modified silicone rubber insulating material.

[0033] The present invention is described in detail below in conjunction with various embodiments.

[0034] Embodiment 1

[0035] According to an embodiment of the present invention, an embodiment of a method for evaluating the dielectric properties of modified silicone rubber is provided. It should be noted that the steps shown in the flowchart of the accompanying drawings can be executed in a computer system such as a set of computer executable instructions, and although a logical order is shown in the flowchart, in some cases, the steps shown or described can be executed in an order different from that shown here.

[0036] Figure 1 is a flow chart of an optional method for evaluating the dielectric properties of modified silicone rubber according to an embodiment of the present invention, such as Figure 1 As shown, the method comprises the following steps:

[0037] Step S101, obtaining a target experimental platform and control experimental samples, wherein the target experimental platform is used to detect dielectric performance parameters of insulating materials, and the types of control experimental samples include at least: ordinary silicone rubber samples and modified silicone rubber samples.

[0038] Step S102, controlling the target experimental platform to simulate a high voltage operating environment for the control experimental sample, and obtaining simulation experimental results based on a specified simulation cycle, wherein the simulation experimental results include: an electrical tree damage coefficient and a dielectric factor of the modified silicone rubber sample.

[0039] Step S103, calculating the evaluation score of the modified silicone rubber sample based on the electrical tree damage coefficient and the dielectric factor indicated by the simulation experiment results.

[0040] Step S104: generating a dielectric property evaluation result of the modified silicone rubber sample based on the evaluation score.

[0041] Through the above steps, the target experimental platform and the control experimental samples can be first obtained, wherein the target experimental platform is used to detect the dielectric performance parameters of the insulating material, and the types of the control experimental samples include at least: ordinary silicone rubber samples and modified silicone rubber samples, and then the target experimental platform is controlled to simulate the high-voltage operating environment for the control experimental samples, and the simulation experimental results are obtained based on the specified simulation cycle, wherein the simulation experimental results include: the electrical tree damage coefficient and dielectric factor of the modified silicone rubber sample, and then the evaluation score of the modified silicone rubber sample is calculated based on the electrical tree damage coefficient and dielectric factor indicated by the simulation experimental results, and finally the dielectric performance evaluation result of the modified silicone rubber sample is generated based on the evaluation score.

[0042] In the embodiment of the present invention, a control simulation experiment is carried out on ordinary silicone rubber insulating materials and modified silicone rubber insulating materials through a multi-field coupling experimental platform, and the electrical tree damage coefficient and dielectric factor of the two insulating material samples after the high-voltage operation simulation test under the same experimental conditions are obtained, and the evaluation score of the modified silicone rubber insulating material is calculated. The evaluation score is used to judge the dielectric properties of the modified silicone rubber insulating material, and then it is judged whether the dielectric properties of the silicone rubber insulating material used for the transformer after different surface modifications are improved, which solves the technical problem that the dielectric properties of the modified silicone rubber cannot be accurately and effectively evaluated in the related art.

[0043] The embodiment of the present invention is described in detail below in combination with the above steps.

[0044] The implementation subject of the embodiment of the present invention can be an automated testing system or an automated testing robot for a high-voltage system. The implementation subject is configured to perform complex experimental processes and data acquisition tasks, and comprehensively evaluate the dielectric properties of modified silicone rubber by combining various technical means such as experimental testing, high-voltage simulation, mathematical modeling and data analysis.

[0045] In the embodiments of the present invention, through simulation experiments and computational analysis, the performance differences between ordinary silicone rubber and modified silicone rubber under high pressure environments can be accurately compared, providing a scientific basis and guidance for engineering applications.

[0046] Step S101, obtaining a target experimental platform and control experimental samples, wherein the target experimental platform is used to detect dielectric performance parameters of insulating materials, and the types of control experimental samples include at least: ordinary silicone rubber samples and modified silicone rubber samples.

[0047] In order to execute the dielectric properties testing process, it is necessary to build a target experimental platform in advance, which is used to experiment and test the dielectric properties of ordinary / modified silicone rubber used for transformers in the embodiments of the present invention. Optionally, the target experimental platform includes: an experimental box, a temperature controller, a temperature sensor, a high-voltage power supply, a dielectric analyzer, an electromagnetic controller, a magnetic flux density meter, an electromagnetic pole plate, a voltmeter, a needle electrode, a ground electrode, a microscopic imaging system and a computer terminal.

[0048] Specifically, the test box is used to carry a simulated high-voltage operating environment. The temperature controller and the electromagnetic controller are arranged on the inner wall of the test box, and a data connection is pre-established with the computer terminal for adjusting the simulated environment inside the test box, specifically adjusting various simulated operating parameters; the temperature sensor is arranged on the inner wall of the test box, and a data connection is pre-established with the computer terminal for real-time monitoring of the internal ambient temperature of the test box, and transmitting the real-time monitoring data back to the computer terminal.

[0049] Another thing that needs to be explained is that the electromagnetic pole plate is arranged in the internal space of the experimental box, which is divided into an N pole and an S pole. The experimental sample, the needle electrode and the ground electrode are arranged between the N pole and the S pole, wherein the ground electrode platform is used to place the experimental sample, and the needle electrode is aligned with the geometric center of the experimental sample; the magnetic flux density meter is installed on the inner wall of the experimental box close to the S pole of the electrode magnetic plate, and a data connection is pre-established with the computer terminal, which is used to measure the magnetic flux density between the pole plates and transmit the magnetic flux density data to the computer terminal.

[0050] In addition, the positive port of the high-voltage power supply is connected to the needle electrode, the ground port is connected to the ground electrode, and the voltmeter is connected in parallel at both ends of the needle plate electrode and connected to the computer terminal to measure the real-time voltage at both ends of the electrode and transmit the voltage data to the computer terminal.

[0051] The dielectric analyzer in the embodiment of the present invention needs to be directly connected to the experimental sample and pre-establish a data connection with the computer terminal to measure the dielectric parameters of the experimental sample, including dielectric constant and dielectric loss, and transmit the measurement data to the computer terminal.

[0052] The microscopic imaging system in the embodiment of the present invention can be installed on the inner wall of the experimental box where the experimental samples can be directly observed, and a data connection can be pre-established with a computer terminal to monitor the electrical tree distribution and electrical tree parameters of the experimental samples, and return the monitoring data to the computer terminal.

[0053] After the target experimental platform is built, the main process of the program can be executed. In step S101 of the embodiment of the present invention, the target experimental platform and control experimental samples for the experiment are selected and obtained, ensuring a unified environment for the experiment and a clear source of basic data.

[0054] Step S102, control the target experimental platform to simulate the high-voltage operating environment for the control experimental sample, and obtain the simulation experimental results based on the specified simulation cycle, wherein the simulation experimental results include: the electrical tree damage coefficient and dielectric factor of the modified silicone rubber sample. By simulating the high-voltage conditions in the real working environment, the performance of the insulating material in actual use can be evaluated and predicted.

[0055] In order to better simulate the high-voltage environment, optionally, before executing step S102, it also includes: obtaining winding-related parameters of the target traction transformer after running for a specified period of time in the actual high-voltage operating environment, wherein the target traction transformer refers to a transformer using ordinary silicone rubber samples and / or modified silicone rubber samples as insulating materials; determining simulation operating parameters based on the winding-related parameters, and transmitting the simulation operating parameters to the computer terminal of the target experimental platform, wherein the computer terminal controls the target experimental platform to simulate the high-voltage operating environment based on the simulation operating parameters.

[0056] In an optional embodiment, when obtaining winding-related parameters, the highest temperature T of the high-voltage winding side of the traction transformer during the actual operation of the traction transformer in one year can be obtained according to the operation record of the traction transformer. max , minimum temperature T min , unit is K; maximum magnetic flux density on the high voltage winding side B max , minimum magnetic flux density B min , unit is T; the maximum voltage U that the high voltage winding side can withstand max , minimum voltage U min , unit is kV.

[0057] Optionally, the step of determining the simulated operation parameters based on the winding-related parameters includes: determining the sample quantity R of each type of control experimental sample, and determining R simulated operation temperatures based on the sample quantity and the winding-side temperature in the winding-related parameters, wherein R is a positive integer; determining R simulated operation magnetic flux densities and R simulated operation voltages based on the sample quantity and the magnetic flux density and the winding-side voltage in the winding-related parameters, respectively; determining the simulated operation parameters based on the simulated operation temperature, the simulated operation magnetic flux density and the simulated operation voltage.

[0058] Continuing with the above example, when the number of samples R = 10, 10 uniformly increasing simulation operating temperatures can be determined as T i , i=1, 2...10, unit is K, where T1=T min , T 10 =T max Similarly, determine 10 uniformly increasing simulation running magnetic flux densities as B i , unit is T, where B1=B min , B 10 =B max ; Determine 10 uniformly increasing simulated operating voltages as U i , the unit is kV, the pulse frequency is 100HZ, where U1=U min , U 10 =U max And each simulation operation parameter is integrated into a group accordingly, and 10 groups of simulation operation parameters are obtained to generate 10 high-voltage operation environments.

[0059] In order to make the experimental effect more obvious, a specified simulation cycle can also be set. Optionally, the target experimental platform is controlled to simulate a high-voltage operating environment for the control experimental sample, and the steps of obtaining the simulation experimental results based on the specified simulation cycle include: controlling the target experimental platform to generate a high-voltage operating environment based on the simulation operating parameters, and applying the high-voltage operating environment to the control experimental sample placed in the experimental box; after the specified simulation cycle, the electrical tree damage coefficient and dielectric factor of the modified silicone rubber sample in the experimental box are obtained to obtain the simulation experimental results.

[0060] For example, the experimental time of each experimental sample may be set to 50 cycles, and the experimental cycle may be set to 20 times to simulate the operation of 1 year in an actual high-voltage operating environment.

[0061] Optionally, the step of obtaining the electrical tree damage coefficient of the modified silicone rubber sample in the experimental box after a specified simulation cycle includes: after simulating a high-voltage operating environment for a control experimental sample, using a microscopic imaging system of a target experimental platform to respectively obtain the electrical tree length, electrical tree width, electrical tree damage area and fractal dimension of the ordinary silicone rubber sample and the modified silicone rubber sample; substituting the electrical tree length, electrical tree width, electrical tree damage area and fractal dimension into a damage calculation formula to calculate the electrical tree damage coefficient of the modified silicone rubber sample.

[0062] In the embodiment of the present invention, the common silicone rubber samples and the modified silicone rubber samples are experimented separately. For example, when 10 common silicone rubber samples and 10 modified silicone rubber samples are obtained, the 10 common silicone rubber samples are experimented in the target experimental platform respectively. After the experiment, the length and width of the electrical tree of the common silicone rubber samples are measured by using a microscopic imaging system, and are recorded as Li and D i , the damage area of ​​the electrical tree is S i , the fractal dimension is P i , where i=1, 2...10; then 10 modified silicone rubber samples were tested in the target experimental platform. After the experiment, the length and width of the electrical tree of the modified silicone rubber samples were measured using a microscopic imaging system and recorded as L j and D j , the damage area of ​​the electrical tree is S j , the fractal dimension is P j , where j=1, 2...10.

[0063] The embodiment of the present invention also provides an exemplary damage calculation formula based on the above embodiment:

[0064]

[0065] in, is the electrical tree damage coefficient of the modified silicone rubber sample, R is the radius of curvature at the tip of the needle electrode, d is the distance between the positive and negative electrodes, T0 is the average temperature of the high-voltage winding side of the transformer within one year, and B0 is the average magnetic flux density of the high-voltage winding side of the transformer within one year.

[0066] Optionally, the step of obtaining the dielectric factor of the modified silicone rubber sample in the experimental box after a specified simulation cycle includes: after simulating a high-voltage operating environment for a control experimental sample, using a dielectric analyzer in a target experimental platform to respectively obtain the relative dielectric constant and dielectric loss of the ordinary silicone rubber sample and the modified silicone rubber sample; substituting the relative dielectric constant and dielectric loss into a dielectric calculation formula to calculate the dielectric factor of the modified silicone rubber sample.

[0067] After obtaining the electrical tree damage coefficient, the environmental parameters of the target experimental platform are kept unchanged, and the relative dielectric constant of the ordinary silicone rubber sample is measured using a dielectric analyzer. , the dielectric loss is recorded as , the relative dielectric constant of the modified silicone rubber sample is measured to be , the dielectric loss is recorded as , where i=1, 2...10, j=1, 2...10.

[0068] The embodiment of the present invention further provides an exemplary dielectric calculation formula based on the above embodiment:

[0069]

[0070] in, is the dielectric factor of the modified silicone rubber sample, R is the radius of curvature at the tip of the needle electrode, d is the distance between the positive and negative electrodes, T0 is the average temperature of the high-voltage winding side of the transformer within one year, and B0 is the average magnetic flux density of the high-voltage winding side of the transformer within one year.

[0071] Step S103, calculating the evaluation score of the modified silicone rubber sample based on the electrical tree damage coefficient and the dielectric factor indicated by the simulation experiment results.

[0072] The embodiment of the present invention also provides an exemplary evaluation calculation formula: Evaluation score .

[0073] Step S104: generating a dielectric property evaluation result of the modified silicone rubber sample based on the evaluation score.

[0074] In an optional embodiment, an evaluation threshold or an evaluation threshold interval may be preset, and a dielectric performance evaluation result may be generated by comparing the evaluation score with the evaluation threshold (interval). It means that the dielectric properties of the modified silicone rubber are good. It means that the dielectric properties of modified silicone rubber are average. This means that the dielectric properties of the modified silicone rubber are poor.

[0075] The embodiment of the present invention provides a complete dielectric performance evaluation process, starting from the selection of experimental samples, simulating the experimental environment and obtaining experimental data, to calculating and generating evaluation scores, and finally obtaining evaluation results. Each step provides necessary data and analysis for evaluating the dielectric properties of insulating materials. The entire process can not only provide quantitative and objective evaluation indicators, but also help optimize the selection of insulating materials and the design process of transformer products, thereby improving the operating reliability and insulation performance of transformer products in high-voltage systems.

[0076] The present invention is described below in conjunction with another specific implementation manner.

[0077] Figure 2 is a schematic diagram of an optional test platform for dielectric properties of modified silicone rubber according to an embodiment of the present invention, such as Figure 2 As shown, the test platform (i.e., the target experimental platform in Example 1) includes: an experimental box 1, a temperature controller 2, a temperature sensor 3, a high-voltage power supply 4, a dielectric analyzer 5, an electromagnetic controller 6, a magnetic flux density meter 7, an electromagnetic pole plate N pole 8, an electromagnetic pole plate S pole 9, a voltmeter 10, a needle electrode 11, a ground electrode 12, a circular silicone rubber sample 13, a microscopic imaging system 14, and a computer terminal 15.

[0078] Among them, the temperature controller 2 and the electromagnetic controller 6 are controlled by the computer terminal 15 to adjust the internal environmental parameters of the experimental box 1; the temperature sensor 3 is installed on the inner wall of the experimental box 1 to monitor the internal environmental temperature of the experimental box in real time, and return the temperature data to the computer terminal 15; the magnetic flux density meter 7 is installed near the S pole 9 of the electromagnetic pole plate to measure the magnetic flux density between the two pole plates, and return the magnetic flux density data to the computer terminal 15; the positive terminal of the high-voltage power supply 4 is connected to the needle electrode 11, and the grounding port is connected to the ground electrode 12, and the center of the circular silicone rubber sample 13 is aligned with the needle electrode 11; the voltmeter 10 is connected in parallel to both ends of the needle plate electrode to measure the real-time voltage at both ends of the electrode, and the dielectric analyzer 5 is connected to the circular silicone rubber sample 13. After the discharge stage, the dielectric constant and dielectric loss of the sample are measured, and the data are returned to the computer terminal 15; the microscopic imaging system 14 is installed on the right inner wall of the experimental box 1 to monitor the distribution of electrical dendrites in the sample, and record related parameters and return them to the computer terminal 15.

[0079] Figure 3 is a flow chart of an optional method for evaluating the dielectric properties of modified silicone rubber based on electrical tree distribution for transformers according to an embodiment of the present invention, such as Figure 3 As shown, the method comprises the following steps:

[0080] The first step is to build a modified silicone rubber dielectric performance test platform for transformers (i.e., the target experimental platform in Example 1);

[0081] Step 2: Calculate the electrical tree damage coefficient;

[0082] First, the relevant parameters of the traction transformer winding are obtained; according to the operation record, the maximum temperature T of the high-voltage winding side within one year of actual operation of the traction transformer (that is, the specified time in the first embodiment is set to one year) is obtained. max , minimum temperature T min , unit is K; maximum magnetic flux density on the high voltage winding side B max , minimum magnetic flux density B min , unit is T; the maximum voltage U that the high voltage winding side can withstand max , minimum voltage U min , unit is kV;

[0083] Ten samples of common silicone rubber insulation material (i.e., the common silicone rubber samples in the control experiment samples in Example 1) were prepared, and the ten samples were respectively subjected to experiments on the experimental platform, and ten groups of evenly increasing experimental temperatures were taken, namely, T i , the unit is K, where T1=T min , T 10 =T max ; Take 10 groups of uniformly increasing magnetic flux density as B i , unit is T, where B1=Bmin , B 10 =B max ; Take 10 groups of uniformly increasing pulse voltage amplitudes and record them as U i , the unit is kV, the pulse frequency is 100HZ, where U1=U min , U 10 =U max In order to make the experimental effect more obvious, the experimental time of each sample was 50 cycles, and the experimental cycle was 20 times. After the experiment, the length and width of the electrical tree of the silicone rubber sample were measured using a microscopic imaging system and recorded as L i and D i , the damage area of ​​the electrical tree is S i , the fractal dimension is P i , where i=1, 2...10;

[0084] Ten samples of silicone rubber insulation material with modified filler surface (i.e., the modified silicone rubber samples in the control experimental samples in Example 1) were prepared, and the ten samples were respectively subjected to experiments in an experimental platform, and ten groups of uniformly increasing experimental temperatures were taken, namely, T j , the unit is K, where T1=T min , T 10 =T max ; Take 10 groups of uniformly increasing magnetic flux density as B j , unit is T, where B1=B min , B 10 =B max ; Take 10 groups of uniformly increasing pulse voltage amplitudes and record them as U j , the unit is kV, the pulse frequency is 100HZ, where U1=U min , U 10 =U max In order to make the experimental effect more obvious, the experimental time of each sample was 50 cycles, and the experimental cycle was 20 times. After the experiment, the length and width of the electrical tree of the silicone rubber sample were measured using a microscopic imaging system and recorded as L j and D j , the damage area of ​​the electrical tree is S j , the fractal dimension is P j , where j=1, 2...10;

[0085] The electrical tree damage coefficient is obtained by formula (1):

[0086] (1)

[0087] Where R is the radius of curvature at the tip of the needle electrode, d is the distance between the positive and negative electrodes, T0 is the average temperature of the high-voltage winding side of the transformer within one year, and B0 is the average magnetic flux density of the high-voltage winding side of the transformer within one year;

[0088] Step 3: Calculate the dielectric factor;

[0089] The environmental parameters of the experimental platform remain unchanged, and the relative dielectric constant of the ordinary silicone rubber sample is measured by a dielectric analyzer. , the dielectric loss is recorded as ; The relative dielectric constant of the modified silicone rubber sample was measured by a dielectric analyzer. , the dielectric loss is recorded as , where i=1, 2...10, j=1, 2...10;

[0090] The dielectric factor is obtained by formula (2):

[0091] (2)

[0092] Where R is the radius of curvature at the tip of the needle electrode, d is the distance between the positive and negative electrodes, T0 is the average temperature of the high-voltage winding side of the transformer within one year, and B0 is the average magnetic flux density of the high-voltage winding side of the transformer within one year;

[0093] Step 4: Calculate the dielectric performance evaluation factor;

[0094] The dielectric property evaluation factor of the modified silicone rubber for transformer based on the electrical tree distribution (i.e., the evaluation score of the modified silicone rubber sample in Example 1) is calculated using formula (3):

[0095] (3)

[0096] Step 5: Further verify the dielectric properties of modified silicone rubber used for transformers based on the evaluation factors;

[0097] According to formula (3), the dielectric properties of modified silicone rubber used in transformers are evaluated. It means that the dielectric properties of the modified silicone rubber are good. It means that the dielectric properties of modified silicone rubber are average. This means that the dielectric properties of the modified silicone rubber are poor.

[0098] The beneficial effect of the present invention lies in that, by building a multi-field coupling experimental platform, the influence of electromagnetic thermal coupling on the dielectric properties of modified silicone rubber is simulated, the two parameters of electrical tree damage coefficient and dielectric factor are integrated, and a modified silicone rubber dielectric property evaluation method for transformers based on electrical tree distribution is provided. The dielectric property evaluation factor of modified silicone rubber can be effectively calculated, which provides a way to evaluate the dielectric properties of modified silicone rubber used for transformers.

[0099] The present invention is described below in conjunction with another optional embodiment.

[0100] Embodiment 2

[0101] The device for evaluating the dielectric properties of modified silicone rubber provided in this embodiment includes a plurality of implementation units, each of which corresponds to each implementation step in the above-mentioned embodiment 1.

[0102] Figure 4 is a schematic diagram of an optional device for evaluating the dielectric properties of modified silicone rubber according to an embodiment of the present invention, such as Figure 4 As shown, the device may include: an acquisition unit 41, a control unit 42, a calculation unit 43, and a generation unit 44.

[0103] The acquisition unit 41 is used to acquire a target experimental platform and control experimental samples, wherein the target experimental platform is used to detect dielectric performance parameters of insulating materials, and the types of control experimental samples include at least: ordinary silicone rubber samples and modified silicone rubber samples.

[0104] The control unit 42 is used to control the target experimental platform to simulate the high voltage operating environment for the control experimental sample, and obtain the simulation experimental results based on the specified simulation cycle, wherein the simulation experimental results include: the electrical tree damage coefficient and dielectric factor of the modified silicone rubber sample.

[0105] The calculation unit 43 is used to calculate the evaluation score of the modified silicone rubber sample based on the electrical tree damage coefficient and the dielectric factor indicated by the simulation experiment result.

[0106] The generating unit 44 is used to generate a dielectric property evaluation result of the modified silicone rubber sample based on the evaluation score.

[0107] The above-mentioned modified silicone rubber dielectric property evaluation device can first acquire a target experimental platform and a control experimental sample through an acquisition unit 41, wherein the target experimental platform is used to detect the dielectric property parameters of the insulating material, and the types of the control experimental samples include at least: ordinary silicone rubber samples and modified silicone rubber samples, and then control the target experimental platform through a control unit 42 to simulate a high-voltage operating environment for the control experimental sample, and obtain a simulation experiment result based on a specified simulation cycle, wherein the simulation experiment result includes: an electrical tree damage coefficient and a dielectric factor of the modified silicone rubber sample, and then calculate the evaluation score of the modified silicone rubber sample based on the electrical tree damage coefficient and the dielectric factor indicated by the simulation experiment result through a calculation unit 43, and finally generate a dielectric property evaluation result of the modified silicone rubber sample based on the evaluation score through a generation unit 44.

[0108] In the embodiment of the present invention, a control simulation experiment is carried out on ordinary silicone rubber insulating materials and modified silicone rubber insulating materials through a multi-field coupling experimental platform, and the electrical tree damage coefficient and dielectric factor of the two insulating material samples after the high-voltage operation simulation test under the same experimental conditions are obtained, and the evaluation score of the modified silicone rubber insulating material is calculated. The evaluation score is used to judge the dielectric properties of the modified silicone rubber insulating material, and then it is judged whether the dielectric properties of the silicone rubber insulating material used for the transformer after different surface modifications are improved, which solves the technical problem that the dielectric properties of the modified silicone rubber cannot be accurately and effectively evaluated in the related art.

[0109] Optionally, the target experimental platform includes: an experimental box, a temperature controller, a temperature sensor, a high-voltage power supply, a dielectric analyzer, an electromagnetic controller, a magnetic flux density meter, an electromagnetic pole plate, a voltmeter, a needle electrode, a ground electrode, a microscopic imaging system and a computer terminal, wherein the experimental box is used to carry a simulated high-voltage operating environment; the temperature controller, the electromagnetic controller, the temperature sensor and the magnetic flux density meter are all arranged on the inner wall of the experimental box, and data connections are pre-established with the computer terminal respectively; the electromagnetic pole plate is arranged in the internal space of the experimental box and is connected to the electromagnetic controller, and the electromagnetic pole plate includes: an N pole plate and an S pole plate; the needle electrode and the ground The electrode is arranged between the N-pole plate and the S-pole plate of the electromagnetic plate, the ground electrode is used to place the control experimental sample, and the needle electrode is aligned with the geometric center of the control experimental sample; the voltmeter is connected in parallel to both ends of the needle electrode and the ground electrode, and a data connection is pre-established with a computer terminal; the positive pole of the high-voltage power supply is connected to the needle electrode, and the negative pole of the high-voltage power supply is connected to the ground electrode; the dielectric analyzer is connected to the control experimental sample, and a data connection is pre-established with the computer terminal to measure the dielectric parameters of the control experimental sample; the microscopic imaging system is arranged on the inner wall of the experimental box, and a data connection is pre-established with the computer terminal to monitor the electrical tree parameters of the control experimental sample.

[0110] Optionally, the device for evaluating the dielectric properties of modified silicone rubber also includes: a first acquisition module, used to obtain winding-related parameters of a target traction transformer after the target traction transformer has been running for a specified period of time in an actual high-voltage operating environment, wherein the target traction transformer refers to a transformer using ordinary silicone rubber samples and / or modified silicone rubber samples as insulating materials; a transmission module, used to determine simulated operating parameters based on the winding-related parameters, and transmit the simulated operating parameters to a computer terminal of a target experimental platform, wherein the computer terminal controls the target experimental platform to simulate a high-voltage operating environment based on the simulated operating parameters.

[0111] Optionally, the transmission module includes: a first determination submodule, used to determine the sample quantity R of each type of control experimental sample, and determine R simulated operating temperatures based on the sample quantity and the winding side temperature in the winding-related parameters, where R is a positive integer; a second determination submodule, used to determine R simulated operating magnetic flux densities and R simulated operating voltages based on the sample quantity and the magnetic flux density and winding side voltage in the winding-related parameters; a third determination submodule, used to determine the simulated operating parameters based on the simulated operating temperature, the simulated operating magnetic flux density and the simulated operating voltage.

[0112] Optionally, the control unit includes: a control module, used to control the target experimental platform to generate a high-voltage operating environment based on simulated operating parameters, and apply the high-voltage operating environment to a control experimental sample placed in the experimental box; a second acquisition module, used to obtain the electrical tree damage coefficient and dielectric factor of the modified silicone rubber sample in the experimental box after a specified simulation cycle to obtain the simulation experimental results.

[0113] Optionally, the second acquisition module includes: a first acquisition submodule, which is used to use the microscopic imaging system of the target experimental platform to respectively obtain the electrical tree length, electrical tree width, electrical tree damage area and fractal dimension of ordinary silicone rubber samples and modified silicone rubber samples after simulating a high-voltage operating environment for the control experimental sample; and a second calculation submodule, which is used to substitute the electrical tree length, electrical tree width, electrical tree damage area and fractal dimension into the damage calculation formula to calculate the electrical tree damage coefficient of the modified silicone rubber sample.

[0114] Optionally, the second acquisition module also includes: a second acquisition sub-module, which is used to obtain the relative dielectric constant and dielectric loss of ordinary silicone rubber samples and modified silicone rubber samples respectively using a dielectric analyzer in the target experimental platform after simulating a high-voltage operating environment for the control experimental sample; a second calculation sub-module, which is used to substitute the relative dielectric constant and dielectric loss into the dielectric calculation formula to calculate the dielectric factor of the modified silicone rubber sample.

[0115] The above-mentioned evaluation device for the dielectric properties of modified silicone rubber may also include a processor and a memory. The above-mentioned acquisition unit 41, control unit 42, calculation unit 43, generation unit 44, etc. are all stored in the memory as program units, and the processor executes the above-mentioned program units stored in the memory to realize corresponding functions.

[0116] The processor includes a kernel, which retrieves the corresponding program unit from the memory. One or more kernels can be set, and the evaluation score is calculated based on the electrical tree damage coefficient and dielectric factor indicated by the simulation experiment results by adjusting the kernel parameters, and the dielectric performance evaluation result of the modified silicone rubber sample is generated based on the evaluation score.

[0117] The above-mentioned memory may include non-permanent memory in a computer-readable medium, random access memory (RAM) and / or non-volatile memory, such as read-only memory (ROM) or flash RAM, and the memory includes at least one memory chip.

[0118] The present application also provides a computer program product, which, when executed on a data processing device, is suitable for executing an initialization program having the following method steps: obtaining a target experimental platform and a control experimental sample, wherein the target experimental platform is used to detect the dielectric performance parameters of the insulating material, and the types of the control experimental samples include at least: ordinary silicone rubber samples and modified silicone rubber samples; controlling the target experimental platform to simulate a high-voltage operating environment for the control experimental sample, and obtaining simulation experimental results based on a specified simulation cycle, wherein the simulation experimental results include: an electrical tree damage coefficient and a dielectric factor of the modified silicone rubber sample; calculating an evaluation score based on the electrical tree damage coefficient and the dielectric factor indicated by the simulation experimental results; and generating a dielectric performance evaluation result of the modified silicone rubber sample based on the evaluation score.

[0119] According to another aspect of an embodiment of the present invention, a computer-readable storage medium is further provided, the computer-readable storage medium including a stored computer program, wherein when the computer program is running, the device where the computer-readable storage medium is located is controlled to execute the method for evaluating the dielectric properties of modified silicone rubber of any one of the above-mentioned embodiments.

[0120] According to another aspect of an embodiment of the present invention, there is also provided an electronic device, comprising one or more processors and a memory, wherein the memory is used to store one or more programs, wherein when the one or more programs are executed by one or more processors, the one or more processors implement the method for evaluating the dielectric properties of modified silicone rubber of any one of the above-mentioned embodiments one.

[0121] Figure 5 is a schematic diagram of an optional electronic device according to an embodiment of the present invention, such as Figure 5 As shown, an embodiment of the present invention provides an electronic device, the electronic device includes a processor, a memory, and a program stored in the memory and executable on the processor, the processor is used to execute computer-readable instructions, wherein the computer-readable instructions execute a method for evaluating the dielectric properties of modified silicone rubber when they are executed. The device in the present invention can be a server, a PC, a PAD, a mobile phone, etc.

[0122] The serial numbers of the above embodiments of the present invention are only for description and do not represent the advantages or disadvantages of the embodiments.

[0123] In the above embodiments of the present invention, the description of each embodiment has its own emphasis. For parts that are not described in detail in a certain embodiment, reference can be made to the relevant descriptions of other embodiments.

[0124] In the several embodiments provided in this application, it should be understood that the disclosed technical content can be implemented in other ways. Among them, the device embodiments described above are only schematic. For example, the division of units can be a logical function division. There may be other division methods in actual implementation. For example, multiple units or components can be combined or integrated into another system, or some features can be ignored or not executed. Another point is that the mutual coupling or direct coupling or communication connection shown or discussed can be through some interfaces, indirect coupling or communication connection of units or modules, which can be electrical or other forms.

[0125] The units described as separate components may or may not be physically separated, and the components shown as units may or may not be physical units, that is, they may be located in one place or distributed over multiple units. Some or all of the units may be selected according to actual needs to achieve the purpose of the present embodiment.

[0126] In addition, each functional unit in each embodiment of the present invention may be integrated into one processing unit, or each unit may exist physically separately, or two or more units may be integrated into one unit. The above-mentioned integrated unit may be implemented in the form of hardware or in the form of software functional units.

[0127] If the integrated unit is implemented in the form of a software functional unit and sold or used as an independent product, it can be stored in a computer-readable storage medium. Based on this understanding, the technical solution of the present invention, in essence, or the part that contributes to the prior art, or all or part of the technical solution can be embodied in the form of a software product. The computer software product is stored in a storage medium, including several instructions for a computer device (which can be a personal computer, server or network device, etc.) to perform all or part of the steps of the methods of each embodiment of the present invention. The aforementioned storage medium includes: U disk, read-only memory (ROM, Read-Only Memory), random access memory (RAM, Random Access Memory), mobile hard disk, disk or optical disk, etc. Various media that can store program codes.

[0128] The above are only preferred embodiments of the present invention. It should be pointed out that, for ordinary technicians in this technical field, several improvements and modifications can be made without departing from the principles of the present invention. These improvements and modifications should also be regarded as the scope of protection of the present invention.

Claims

1. A method for evaluating the dielectric properties of modified silicone rubber, characterized in that: include: Acquire a target experimental platform and control experimental samples, wherein the target experimental platform is used to detect dielectric performance parameters of insulating materials, and the types of the control experimental samples include at least: ordinary silicone rubber samples and modified silicone rubber samples; Obtaining winding-related parameters of a target traction transformer after it has been running for a specified period of time in an actual high-voltage operating environment, wherein the target traction transformer refers to a transformer using the ordinary silicone rubber sample or the modified silicone rubber sample as the insulating material; Determine simulation operation parameters based on the winding related parameters, and transmit the simulation operation parameters to the computer terminal of the target experimental platform, wherein the computer terminal controls the target experimental platform to simulate a high-voltage operating environment based on the simulation operation parameters, The step of determining the simulated operation parameters based on the winding related parameters comprises: Determine the number of samples of each type of the control experimental samples as 10, and determine 10 simulated operating temperatures based on the number of samples and the winding side temperature in the winding-related parameters , i =1, 2...10, Based on the number of samples and the magnetic flux density and winding side voltage in the winding related parameters, 10 simulated running magnetic flux densities are determined respectively. and 10 analog operating voltages , Based on the simulated operating temperature The simulation runs magnetic density And the simulated operating voltage Determining the simulation operation parameters; Controlling the target experimental platform to simulate a high-voltage operating environment for the control experimental sample, and obtaining simulation experimental results based on a specified simulation cycle, wherein the simulation experimental results include: the electrical tree damage coefficient and dielectric factor of the modified silicone rubber sample, The electrical tree damage coefficient is obtained based on a damage calculation formula, which is: , in, is the electrical tree damage coefficient, It refers to i The ordinary silicone rubber samples, It refers to j The modified silicone rubber samples, j =1, 2...10, It refers to i The simulated operating temperature increases uniformly. It refers to i The simulated running magnetic density increases uniformly. It refers to i The simulated operating voltage is uniformly increased, R is the radius of curvature at the tip of the needle electrode, d is the distance between the positive and negative electrodes, is the average temperature of the high-voltage winding side of the target traction transformer in one year, is the average magnetic flux density on the high-voltage winding side of the target traction transformer in one year, is the average voltage of the high-voltage winding side of the target traction transformer in one year. After simulating the high-voltage operating environment of the ordinary silicone rubber sample, the length of the electrical tree is recorded as , the width of the electrical tree is recorded as The area of ​​electrical tree damage is recorded as , the fractal dimension is recorded as After simulating a high-voltage operating environment for the modified silicone rubber sample, the length of the electrical tree is recorded as , the width of the electrical tree is recorded as The area of ​​electrical tree damage is recorded as , the fractal dimension is recorded as , The dielectric factor is obtained based on the dielectric calculation formula, which is: , in, is the dielectric factor, and after simulating a high-voltage operating environment for the ordinary silicone rubber sample, the relative dielectric constant is recorded as , the dielectric loss is recorded as After simulating a high-voltage operating environment for the modified silicone rubber sample, the relative dielectric constant is recorded as , the dielectric loss is recorded as ; calculating an evaluation score of the modified silicone rubber sample based on the electrical tree damage coefficient and the dielectric factor indicated by the simulation experiment result; A dielectric property evaluation result of the modified silicone rubber sample is generated based on the evaluation score.

2. The evaluation method according to claim 1, characterized in that: The target experimental platform includes: an experimental box, a temperature controller, a temperature sensor, a high voltage power supply, a dielectric analyzer, an electromagnetic controller, a magnetic flux density meter, an electromagnetic plate, a voltmeter, a needle electrode, a ground electrode, a microscopic imaging system and a computer terminal, wherein: The experimental box is used to carry the simulated high-voltage operating environment; The temperature controller, the electromagnetic controller, the temperature sensor and the magnetic flux density measuring instrument are all arranged on the inner wall of the experimental box, and are respectively pre-connected with the computer terminal; The electromagnetic pole plate is arranged in the internal space of the experimental box and is connected to the electromagnetic controller. The electromagnetic pole plate comprises: an N pole plate and an S pole plate; The needle electrode and the ground electrode are arranged between the N-pole plate and the S-pole plate of the electromagnetic plate, the ground electrode is used to place the control experiment sample, and the needle electrode is aligned with the geometric center of the control experiment sample; The voltmeter is connected in parallel to both ends of the needle electrode and the ground electrode, and a data connection is pre-established with the computer terminal; The positive electrode of the high voltage power supply is connected to the needle electrode, and the negative electrode of the high voltage power supply is connected to the ground electrode; The dielectric analyzer is connected to the control experimental sample and pre-establishes a data connection with the computer terminal for measuring the dielectric parameters of the control experimental sample; The microscopic image system is arranged on the inner wall of the experimental box and pre-establishes a data connection with the computer terminal for monitoring the electrical tree parameters of the control experimental sample.

3. The evaluation method according to claim 1, characterized in that: The step of controlling the target experimental platform to simulate a high-voltage operating environment for the control experimental sample and obtaining a simulation experimental result based on a specified simulation cycle includes: Controlling the target experimental platform to generate the high-pressure operating environment based on the simulated operating parameters, and applying the high-pressure operating environment to the control experimental sample placed in the experimental box; The electrical tree damage coefficient and dielectric factor of the modified silicone rubber sample in the test box are obtained after the specified simulation cycle to obtain the simulation experiment result.

4. The evaluation method according to claim 3, characterized in that: The step of obtaining the electrical tree damage coefficient of the modified silicone rubber sample in the test box after the specified simulation cycle comprises: After simulating a high-voltage operating environment for the control experimental sample, using the microscopic imaging system of the target experimental platform to obtain the electrical tree length, electrical tree width, electrical tree damage area and fractal dimension of the ordinary silicone rubber sample and the modified silicone rubber sample respectively; The electrical tree length, the electrical tree width, the electrical tree damage area, and the fractal dimension are substituted into a damage calculation formula to calculate the electrical tree damage coefficient of the modified silicone rubber sample.

5. The evaluation method according to claim 3, characterized in that: The step of obtaining the dielectric factor of the modified silicone rubber sample in the test box after the specified simulation cycle comprises: After simulating a high-voltage operating environment for the control experimental sample, using a dielectric analyzer in the target experimental platform to obtain the relative dielectric constant and dielectric loss of the ordinary silicone rubber sample and the modified silicone rubber sample respectively; The relative dielectric constant and the dielectric loss are substituted into a dielectric calculation formula to calculate the dielectric factor of the modified silicone rubber sample.

6. A device for evaluating the dielectric properties of modified silicone rubber, characterized in that: include: An acquisition unit, used for acquiring a target experimental platform and a control experimental sample, wherein the target experimental platform is used for detecting dielectric performance parameters of insulating materials, and the types of the control experimental samples include at least: ordinary silicone rubber samples and modified silicone rubber samples; A first acquisition module is used to obtain winding-related parameters of a target traction transformer after the target traction transformer has been running for a specified period of time in an actual high-voltage operating environment, wherein the target traction transformer refers to a transformer using the ordinary silicone rubber sample and / or the modified silicone rubber sample as the insulating material; A transmission module is used to determine simulation operation parameters based on the winding related parameters, and transmit the simulation operation parameters to the computer terminal of the target experimental platform, wherein the computer terminal controls the target experimental platform to simulate a high-voltage operating environment based on the simulation operation parameters, The transmission module comprises: The first determination submodule is used to determine the number of samples of each type of the control experimental samples 10, and determine 10 simulated operating temperatures based on the number of samples and the winding side temperature in the winding related parameters , i =1, 2...10; the second determination submodule is used to determine 10 simulated operation magnetic flux density values ​​based on the number of samples and the magnetic flux density and winding side voltage in the winding related parameters. and 10 analog operating voltages ; A third determination submodule is used based on the simulated operating temperature The simulation runs magnetic density And the simulated operating voltage Determining the simulation operation parameters; A control unit, used to control the target experimental platform to simulate a high-voltage operating environment for the control experimental sample, and obtain simulation experimental results based on a specified simulation cycle, wherein the simulation experimental results include: the electrical tree damage coefficient and dielectric factor of the modified silicone rubber sample, The electrical tree damage coefficient is obtained based on a damage calculation formula, which is: , in, is the electrical tree damage coefficient, It refers to i The ordinary silicone rubber samples, It refers to j The modified silicone rubber samples, j =1, 2...10, It refers to i The simulated operating temperature increases uniformly. It refers to i The simulated running magnetic density increases uniformly. It refers to i The simulated operating voltage is uniformly increased, R is the radius of curvature at the tip of the needle electrode, d is the distance between the positive and negative electrodes, is the average temperature of the high-voltage winding side of the target traction transformer in one year, is the average magnetic flux density on the high-voltage winding side of the target traction transformer in one year, is the average voltage of the high-voltage winding side of the target traction transformer in one year. After simulating the high-voltage operating environment of the ordinary silicone rubber sample, the length of the electrical tree is recorded as , the width of the electrical tree is recorded as The area of ​​electrical tree damage is recorded as , the fractal dimension is recorded as After simulating a high-voltage operating environment for the modified silicone rubber sample, the length of the electrical tree is recorded as , the width of the electrical tree is recorded as The area of ​​electrical tree damage is recorded as , the fractal dimension is recorded as , The dielectric factor is obtained based on the dielectric calculation formula, which is: , in, is the dielectric factor, and after simulating a high-voltage operating environment for the ordinary silicone rubber sample, the relative dielectric constant is recorded as , the dielectric loss is recorded as After simulating a high-voltage operating environment for the modified silicone rubber sample, the relative dielectric constant is recorded as , the dielectric loss is recorded as ; a calculation unit, configured to calculate an evaluation score of the modified silicone rubber sample based on the electrical tree damage coefficient and the dielectric factor indicated by the simulation experiment result; A generating unit is used to generate a dielectric property evaluation result of the modified silicone rubber sample based on the evaluation score.

7. A computer-readable storage medium, characterized in that: The computer-readable storage medium includes a stored computer program, wherein when the computer program is executed, the device where the computer-readable storage medium is located is controlled to execute the method for evaluating the dielectric properties of modified silicone rubber according to any one of claims 1 to 5.

8. An electronic device, characterized in that: The invention comprises one or more processors and a memory, wherein the memory is used to store one or more programs, wherein when the one or more programs are executed by the one or more processors, the one or more processors implement the method for evaluating the dielectric properties of the modified silicone rubber according to any one of claims 1 to 5.

Citation Information

Patent Citations

  • 10kV XLPE cable aging state assessment method based on electrical tree state assessment factors

    CN114184903A

  • Method for evaluating insulating material of dry-type transformer in high-temperature and high-humidity environment

    CN116125147A