Method for preparing electro-optical modulator by adopting lithium niobate material with skyrmion
By applying high temperature and magnetic field to the lithium niobate material to excite skyrmions and perform annealing treatment, the problem of improving the electro-optical coefficient of ferroelectric materials in the existing technology is solved, the electro-optical coefficient is increased by more than three times, and the waveguide loss in photonic integrated circuits is solved. The problem of high and low yield rate expands the application fields and reduces costs.
Patent Information
- Application Number
- CN202410846554.7
- Authority / Receiving Office
- CN · China
- Patent Type
- Applications(China)
- Current Assignee / Owner
- Filing Date
- 2024-06-27
- Publication Date
- 2024-10-11
AI Technical Summary
It is difficult to improve the electro-optical coefficient of ferroelectric materials without changing the physical properties of the material itself with existing technology, resulting in high waveguide loss and low yield, which hinders the industrialization process of photonic integrated circuits.
By applying high temperature and magnetic field to the lithium niobate material, skyrmions are excited, and annealing is performed to increase its electro-optic coefficient, forming a lithium niobate material with skyrmions for the preparation of electro-optic modulators.
The electro-optical coefficient of lithium niobate material has been significantly improved from 32pm/V to more than 100pm/V, reducing the device area, reducing process costs, and expanding optical signal modulation methods to achieve performance improvement and cost savings.
Smart Images

Figure CN118759743A_ABST
Abstract
Description
Technical Field
[0001] The present invention relates to the fields of condensed matter physics and photonic integrated circuits (PIC), and in particular to a method for significantly improving the electro-optic coefficient of ferroelectric materials. Background Art
[0002] The refractive index of electro-optical materials will change under the action of an external electric field. Therefore, they can be widely used in optical signal modulation and the mutual conversion of photoelectric signals. They are widely used in optical communications, optical computing, quantum computing, and lidar.
[0003] The electro-optic coefficient is the core parameter of electro-optic materials and directly determines the modulation efficiency of the device. A high electro-optic coefficient not only helps improve device performance, but also greatly improves system integration, helps reduce costs, and thus improves the industrialization capacity of photonic integrated circuits.
[0004] At present, the most widely used electro-optical material in the PIC field is lithium niobate (LiNbO 3 ), which has extremely low waveguide loss (<0.3dB / cm) and high electro-optic coefficient (32pm / V). At the same time, lithium niobate has an extremely high Curie temperature (1473K) and strong corrosion resistance. Therefore, lithium niobate is also called "optical silicon" and is considered to be one of the ideal platforms for the next generation of silicon optical devices.
[0005] In order to further realize the industrialization of PIC, obtaining materials with higher electro-optic coefficients is a key direction. Since the world has not yet achieved the improvement of the electro-optic coefficient of materials without changing the physical properties of the materials themselves (element ratio, crystal structure), the mainstream solution is still to find new materials with higher electro-optic coefficients, including lead zirconate titanate (PZT) and its dopants and barium titanate (BTO). These materials all have higher electro-optic coefficients than lithium niobate, but these platforms have higher waveguide losses (higher than 1dB / cm), and the related material growth and etching processes are not yet mature, and the yield rate is extremely low, so it is currently difficult to enter the industrialization track. Summary of the invention
[0006] In view of the above technical problems existing in the prior art, the present invention provides a method for preparing an electro-optic modulator using lithium niobate material with skyrmions. This scheme excites skyrmions in ferroelectric materials through high-temperature magnetic fluctuations, thereby affecting the electro-optic coefficient of the material.
[0007] A method for preparing an electro-optic modulator using a lithium niobate material with skyrmions comprises the following steps:
[0008] 1.1): Apply high temperature and magnetic field to lithium niobate material, then remove the field and cool it down to obtain lithium niobate intermediate;
[0009] 1.2): Annealing the lithium niobate intermediate obtained in step 1.1) to obtain a lithium niobate material with skyrmions;
[0010] 1.3): The lithium niobate material with skyrmions obtained in step 1.2) is used as a material platform to prepare an electro-optic modulator through a semiconductor process;
[0011] or;
[0012] 2.1): Using lithium niobate as a material platform to prepare electro-optic modulators through semiconductor technology;
[0013] 2.2): applying high temperature and magnetic field to the electro-optic modulator obtained in step 2.1), and then removing the field and cooling it to obtain an electro-optic modulator intermediate;
[0014] 2.3): Annealing the electro-optic modulator intermediate obtained in step 2.1) to obtain a lithium niobate electro-optic modulator with skyrmions.
[0015] In step 1.1), the high temperature ranges from 300°C to 700°C.
[0016] In step 1.1), the magnetic field ranges from 0.5T to 10T.
[0017] In step 1.2), the temperature range of the annealing treatment is: 400°C to 600°C.
[0018] In step 2.2), the high temperature ranges from 300°C to 700°C.
[0019] In step 2.2), the magnetic field ranges from 0.5T to 10T.
[0020] In step 2.3), the temperature range of the annealing treatment is: 400°C to 600°C.
[0021] The material used in the present invention is ferroelectric lithium niobate (LiNbO 3 ) materials, including lithium niobate materials of single crystal thin films and single crystal blocks.
[0022] In the present invention, the lithium niobate material carrying skyrmions has a higher electro-optic coefficient than the original one, which can greatly reduce the area required for the device, help improve the device integration, and significantly reduce the process cost. In addition, after carrying skyrmions, magnetism can be introduced and act on the modulator, thereby expanding the optical signal modulation means of the device and expanding its application field.
[0023] The present invention can increase the electro-optic coefficient of lithium niobate material from 32 pm / V to above 100 pm / V, with an increase of more than 200%.
[0024] The generation method comprises the following steps:
[0025] 1) High temperature magnetization:
[0026] A predetermined magnetic field is applied to the ferroelectric single crystal and the temperature is increased. After a period of time, the ferroelectric single crystal in the high temperature environment is removed from the field and cooled. The skyrmion is excited by the demagnetization field, and the formation energy required for the excitation is reduced by the high temperature.
[0027] 2) Annealing: The cooled ferroelectric single crystal is heated again, kept for a period of time, and then cooled down. This process can make skyrmions acquire ferroelectricity in a ferroelectric environment and improve the electro-optic coefficient.
[0028] Preferably: the magnetic field is above 0.3T
[0029] Preferably, the ferroelectric single crystal is lithium niobate (LiNbO 3 )Material
[0030] Preferably, the high temperature used is greater than 433K. The greater the applied magnetic field, the lower the critical temperature required.
[0031] Compared with the prior art, the present invention has the following advantages:
[0032] 1. Easy operation and low cost: The invention does not require changing the element ratio of the material, nor does it require changing the crystal structure of the material. It can be achieved with simple post-processing, so the cost is extremely low and allows large-scale processing.
[0033] 2. Excellent performance: The invention can increase the electro-optic coefficient to more than three times the original value, which is much higher than the initial value of the material.
[0034] 3. Compatibility: This invention can be directly applied to lithium niobate materials and is directly compatible with all currently supported process solutions. There is no need to find new materials or develop new platforms, which has huge advantages in R&D costs and time costs. Since this invention improves the basic physical properties of lithium niobate, all active devices based on the electro-optic coefficient of lithium niobate can achieve more than 3 times the performance of the previous ones, which is extremely cost-effective.
[0035] 4. Pioneering in the field: For the first time, the electro-optical coefficient of the material can be improved without changing the lattice, crystal orientation, and element ratio of the material itself. BRIEF DESCRIPTION OF THE DRAWINGS
[0036] Figure 1 The electro-optic modulator based on the Mach-Zehnder architecture using a thin-film lithium niobate platform in the embodiment is used to evaluate the electro-optic coefficient of lithium niobate, and its typical structure is the microscope image of the device used this time.
[0037] Figure 2The modulation efficiency measurement results of the lithium niobate electro-optic modulator without treatment;
[0038] Figure 3 This is the scheme used in step 1) in Example 1;
[0039] Figure 4 The modulation efficiency measurement result of the lithium niobate electro-optic modulator after step 1) in Example 1;
[0040] Figure 5 This is the scheme used in step 2) in Example 1;
[0041] Figure 6 The modulation efficiency measurement result of the lithium niobate electro-optic modulator after step 1) and step 2) in Example 1;
[0042] Figure 7 The modulation efficiency measurement result of the lithium niobate electro-optic modulator after step 1) and two steps 2) in Example 1;
[0043] Figure 8 The modulation efficiency and the corresponding electro-optic coefficient summary diagram obtained after each step of the embodiment 1 are shown in FIG. 1 , and the dotted line in the figure is the modulation efficiency simulation value of the device;
[0044] Fig. 9 This is the LTEM image of the untreated lithium niobate material;
[0045] Fig.10 The LTEM image of the lithium niobate material after step 1) and step 2);
[0046] Fig.11 This is the morphology of a single skyrmion magnetic vortex obtained after processing with the intensity transfer algorithm. DETAILED DESCRIPTION
[0047] In order to make the purpose and technical solution of the present invention more clear, the following will be combined with pictures to clearly describe the technical solution in the implementation of the present invention. In the embodiment, a thin-film lithium niobate platform based on Mach-Zehnder architecture electro-optic modulator is used to evaluate the size of the lithium niobate electro-optic coefficient. Its typical structure is similar to the device microscope image used in this study. Figure 1 Please note that this does not limit the types of devices to which the invention can be applied.
[0048] The following is the attached Figures 2 to 11 To further illustrate the embodiments of the present invention, the following pictures include images of lithium niobate single crystals observed by Lorentz transmission electron microscopy (LTEM). The magnetic structure of skyrmions can be described by LTEM images at three focal lengths, which are characterized by: the magnetic signal does not show any contrast in the positive focus state, the magnetic signal shows opposite contrast in underfocus and overfocus, and the contrast signal is in a ring shape.
[0049] Embodiment 1:
[0050] The electro-optic modulator prepared based on CMOS technology has a modulation area length of 4 mm. The measurement results without any processing are as follows Figure 2 As shown, it can be confirmed that the half-wave voltage is 4.95 V and the modulation efficiency is 1.98 V·cm.
[0051] Step 1) Apply a magnetic field of 1T to the modulator at room temperature. The purpose is to provide a magnetic environment in lithium niobate. Then heat the modulator to 733K. After 30 minutes, stop heating, let it cool naturally to 653K, and then remove the magnetic field. Finally, let it cool naturally to below 473K and then take it out. The whole process is as follows Figure 3 shown.
[0052] After this step, the half-wave voltage test result of the modulator is as follows: Figure 4 As shown in the figure, it can be seen that the half-wave voltage of the device has dropped to 4.25V, and the modulation efficiency is 1.7V·cm.
[0053] Step 2) The high temperature magnetized lithium niobate is heated up to 823K again, and then cooled back to room temperature after 20 minutes. Figure 5 shown.
[0054] After this step, the half-wave voltage test result of the modulator is as follows: Figure 6 As shown in the figure, the half-wave voltage of the device has dropped to 1.74V, and the modulation efficiency is 0.68V·cm. This value is much lower than the results of lithium niobate modulators with similar architectures reported so far.
[0055] Further, after repeating step 2), the half-wave voltage test result of the modulator is as follows: Figure 7 As shown in the figure, it can be seen that the half-wave voltage of the device has dropped to 1.57V, and the modulation efficiency has further decreased to 0.63V·cm.
[0056] The modulation efficiency of the device after each step is summarized in Figure 8 In the figure, the change of the electro-optic coefficient of lithium niobate after each step of treatment is calculated. In the figure, S0 represents the initial value of the device, S1 represents the device performance after step 1), S2 represents the device performance after step 1) and step 2), and S3 represents the device performance after step 1) and two steps 2). It can be seen that the electro-optic coefficient of lithium niobate is increased from 32pm / V to 101pm / V after each step of treatment, which is more than 3 times the original value.
[0057] Fig. 9The LTEM results of untreated lithium niobate films were shown, confirming the obvious magnetic structure in the untreated lithium niobate material, which is consistent with the current academic consensus that lithium niobate is a ferroelectric material without significant magnetism.
[0058] Fig.10 The LTEM results of the lithium niobate film after step 1) and step 2) of the embodiment are shown. It can be clearly seen that dense skyrmion magnetic vortices appear in the lithium niobate crystal. Furthermore, the magnetic vortex morphology of a single skyrmion depicted by the intensity transfer algorithm is as follows: Fig.11 As shown in the figure, the scale of the rectangle in the figure is 10nm, and the arrow represents the direction of the magnetic moment. It can be confirmed that the diameter of the skyrmion is on the order of 30nm and the topological charge is 1.
[0059] Although the present invention has been described through preferred embodiments, the present invention is not limited to the embodiments described herein but includes various changes and modifications that may be made without departing from the scope of the present invention.
Claims
1. A method for preparing an electro-optic modulator using lithium niobate material with skyrmions, It is characterized in that The following steps are involved: 1.1): Apply high temperature and magnetic field to lithium niobate material, then remove the field and cool it down to obtain lithium niobate intermediate; 1.2): Annealing the lithium niobate intermediate obtained in step 1.1) to obtain a lithium niobate material with skyrmions; 1.3): The lithium niobate material with skyrmions obtained in step 1.2) is used as a material platform to prepare an electro-optic modulator through a semiconductor process; or; 2.1): Using lithium niobate as a material platform to prepare electro-optic modulators through semiconductor technology; 2.2): applying high temperature and magnetic field to the electro-optic modulator obtained in step 2.1), and then removing the field and cooling it to obtain an electro-optic modulator intermediate; 2.3): Annealing the electro-optic modulator intermediate obtained in step 2.1) to obtain a lithium niobate electro-optic modulator with skyrmions.
2. The method for preparing an electro-optic modulator using lithium niobate material with skyrmions according to claim 1, It is characterized in that In step 1.1), the high temperature ranges from 300°C to 700°C.
3. The method for preparing an electro-optic modulator using lithium niobate material with skyrmions according to claim 1, It is characterized in that In step 1.1), the magnetic field ranges from 0.5T to 10T.
4. The method for preparing an electro-optic modulator using lithium niobate material with skyrmions according to claim 1, It is characterized in that In step 1.2), the temperature range of the annealing treatment is: 400°C to 600°C.
5. The method for preparing an electro-optic modulator using lithium niobate material with skyrmions according to claim 1, It is characterized in that In step 2.2), the high temperature ranges from 300°C to 700°C.
6. The method for preparing an electro-optic modulator using lithium niobate material with skyrmions according to claim 1, It is characterized in that In step 2.2), the magnetic field ranges from 0.5T to 10T.
7. The method for preparing an electro-optic modulator using lithium niobate material with skyrmions according to claim 1, It is characterized in that In step 2.3), the temperature range of the annealing treatment is: 400°C to 600°C.
Citation Information
Cited By
Method for preparing low-drift lithium niobate material by means of magnetoelectric-field coupling process
WO2026199948A1