A composite insulated radio frequency coaxial cable with improved heat resistance and a preparation method thereof

By adopting a composite insulating layer structure in RF coaxial cables, combining chemical foaming and physical foaming processes, the heat resistance and transmission performance of the cable are improved, the problem of insufficient heat resistance in the prior art is solved, and the cost is achieved Improved efficiency.

CN118762866BActive Publication Date: 2024-11-22JIANGSU TRIGIANT TECH
View PDF 4 Cites 0 Cited by

Patent Information

Application Number
CN202411220615.5
Authority / Receiving Office
CN · China
Patent Type
Patents(China)
Current Assignee / Owner
Filing Date
2024-09-02
Publication Date
2024-11-22
Estimated Expiration
2044-09-02

AI Technical Summary

Technical Problem

Existing RF coaxial cables are insufficient in heat resistance at high temperatures, resulting in deterioration in transmission performance, and conventional improvements such as increasing cable specifications or using materials with better heat resistance can increase costs.

Method used

Adopt a composite insulating layer structure from the inside to the outside, including the endothelial insulating layer using chemical foam extruded tetrafluoroethylene-perfluoroane vinyl ether copolymer, and the intermediate insulating layer using high melt strength polypropylene and high density polyethylene The blend is physically foamed and extruded, and the outer skin insulation layer is made of chemically foamed and extruded polyperfluoroethylene, combined with specific foaming agents and nucleating agents to improve heat resistance and reduce costs.

Benefits of technology

It significantly improves the insulation heat resistance of RF coaxial cables, reduces manufacturing costs and production costs, and is suitable for high-power mobile communication base station antenna feeder systems, achieving good cost-effectiveness.

✦ Generated by Eureka AI based on patent content.

Smart Images

  • Figure CN118762866B_ABST
    Figure CN118762866B_ABST
Patent Text Reader

Abstract

The present invention relates to the technical field of communication transmission cables, and in particular to a composite insulated radio frequency coaxial cable with improved heat resistance and a preparation method thereof, comprising an inner conductor, a composite insulating layer and an outer conductor, wherein the composite insulating layer comprises an inner skin insulating layer, an intermediate insulating layer and an outer skin insulating layer in sequence from the inside to the outside, wherein the inner skin insulating layer adopts a thin-walled insulating layer of tetrafluoroethylene-perfluoroalkyl vinyl ether copolymer extruded by chemical foaming, the intermediate insulating layer adopts a blend of high melt strength polypropylene and high density polyethylene through physical foaming extrusion, and the outer skin insulating layer adopts a thin-walled insulating layer of polyperfluoroethylene propylene extruded by chemical foaming. The present application adopts three different thermoplastic materials to make a composite insulating layer, improves the insulation and heat resistance of the radio frequency coaxial cable, takes into account the communication performance of the radio frequency coaxial cable, effectively reduces the manufacturing cost, improves the production efficiency, is suitable for the application of high-power mobile communication base station antenna feeder system, and has good application prospects and economic benefits.
Need to check novelty before this filing date? Find Prior Art

Description

Technical Field

[0001] The present invention relates to the technical field of communication transmission cables, and in particular to a composite insulated radio frequency coaxial cable with improved heat resistance and a preparation method thereof. Background Art

[0002] In the antenna feeder system of mobile communication base stations, RF coaxial cables are usually used to connect antennas and signal transceiver equipment. In order to increase the transmission radius of wireless signals, the transmission signal power is required to be large enough, which requires the RF coaxial cable to be able to withstand large power, and the temperature of the inner and outer conductors of the RF coaxial cable will increase significantly. When the conductor temperature is higher than the softening point of the cable's plastic insulation layer, the insulation layer of the RF coaxial cable deforms, resulting in deterioration of transmission performance, and in severe cases, communication interruption. In engineering practice, the peak power of the coaxial cable is usually tested to examine the heat resistance of the cable in a short time. On the other hand, in order to increase the receiving radius of wireless signals, in addition to the receiver having sufficient sensitivity, the attenuation of the coaxial cable should be low enough. When the dimensions of the inner and outer conductors of the coaxial cable have been determined, this requires that the dielectric loss of the coaxial cable insulation layer is low enough. In actual applications, users and manufacturers are also more concerned about the low manufacturing cost and high production efficiency of the insulation layer.

[0003] The product structure of conventional RF coaxial cable complies with the industry standard YD / T 1092 "50Ω Foam Polyolefin Insulated Corrugated Copper Tube Outer Conductor RF Coaxial Cable for Communication Cable and Wireless Communication". Its insulation layer is usually divided into three layers. The solid thin insulation layer near the inner and outer conductors of the cable is mainly made of low-density polyethylene (LDPE) or high-density polyethylene (HDPE), mixed with ethylene-vinyl acetate (EVA) plastic resin with bonding effect; the foam insulation layer in the middle is thicker, and its material composition is mainly LDPE and HDPE mixture mixed with nucleating agent, and is made by physical foaming continuous extrusion process. This kind of insulation structure can better take into account the requirements of attenuation, cost and production efficiency, but its heat resistance is insufficient. The root cause is that the LDPE in the cable insulation layer will soften at 70℃ or even lower. When the cable feed power is increased, resulting in a sharp rise in the temperature of the cable conductor, the air bubble structure in the insulation layer that is in close contact with the conductor and adjacent to the conductor collapses, and the cable transmission performance deteriorates sharply.

[0004] In order to solve the problem that conventional RF coaxial cables are unable to withstand high-power base station communication transmission, the following two solutions are usually adopted: one is to increase the cable specifications, that is, to use larger cables, but this will increase the cable outer diameter and cost, and is not suitable for occasions where the cable installation space is cramped; the other is to replace the entire cable insulation layer with fluoroplastics with better heat resistance such as polyperfluoroethylene propylene (FEP), but this will also significantly increase the cable cost. Summary of the invention

[0005] The technical problem to be solved by the present invention is: in order to solve the technical problems of high temperature resistance faced by existing RF coaxial cables, the present invention provides a composite insulated RF coaxial cable with improved heat resistance and a preparation method thereof. The insulating layer of the present application is made of three different thermoplastic materials to form a composite insulating layer, which greatly improves the insulation and heat resistance of the RF coaxial cable, thereby taking into account the communication performance of the RF coaxial cable, and effectively reduces the manufacturing cost and improves the production efficiency. It is suitable for the application of high-power mobile communication base station antenna feed line system, and has good application prospects and economic benefits.

[0006] The technical solution adopted by the present invention to solve its technical problems is: a composite insulation radio frequency coaxial cable with improved heat resistance, comprising an inner conductor, a composite insulation layer, an outer conductor and a sheath layer arranged in sequence from the inside to the outside, the composite insulation layer comprises in sequence from the inside to the outside: an inner skin insulation layer, an intermediate insulation layer and an outer skin insulation layer, the inner skin insulation layer adopts a chemically foamed extruded tetrafluoroethylene-perfluoroalkyl vinyl ether copolymer thin-wall insulation layer, the intermediate insulation layer adopts a high melt strength polypropylene and high density polyethylene blend through physical foaming extrusion, and the outer skin insulation layer adopts a chemically foamed extruded polyperfluoroethylene propylene thin-wall insulation layer.

[0007] The present invention discloses a composite insulated radio frequency coaxial cable with improved heat resistance. The inner insulating layer adopts fusible polytetrafluoroethylene with lower dielectric loss than polyethylene and much higher heat resistance than polyolefin materials. The fusible polytetrafluoroethylene retains the advantages of high temperature resistance and low dielectric loss of polytetrafluoroethylene, and has a melting point of up to 310°C. It also has the characteristics of melt processing that polytetrafluoroethylene does not have, and can be well attached to metal. The inner insulating layer is made by chemical foaming extrusion process, which can further reduce cable attenuation. The high melt strength polypropylene adopted in the middle insulating layer has better heat resistance and higher heat deformation temperature tolerance than traditional LDPF, and can significantly improve the heat resistance of the middle insulating layer. The outer insulating layer adopts polyperfluoroethylene propylene material with heat resistance significantly higher than HMW-PP / HDPE mixture but not as good as PFA, lower dielectric loss but not as good as PFA, and lower cost, and is made by chemical foaming extrusion process. It can reduce communication loss and cost while improving heat resistance, and achieve higher cost performance.

[0008] Furthermore, the thickness of the endothelial insulation layer is between 0.2 mm and 1.2 mm.

[0009] Furthermore, the endothelial insulation layer uses ammonium polyphosphate as a foaming agent, and the median particle size is maintained at 1.0μm to 4.5μm; the endothelial insulation layer uses a composite nucleating agent comprising boron nitride and calcium tetraborate, and the mixing weight ratio of boron nitride and calcium tetraborate in the composite nucleating agent is between 5:5 and 9:1.

[0010] Furthermore, the weight ratio of the high melt strength polypropylene to the high density polyethylene in the intermediate insulating layer is 15%wt-40%wt: 60%wt-85%wt.

[0011] Furthermore, the nucleating agent used for foaming the intermediate insulating layer is a nucleating agent masterbatch with HMS-PP as a carrier resin, wherein the weight ratio of PTFE to HMS-PP is 15%wt~50%wt:50%wt~85%wt.

[0012] Furthermore, the thickness of the outer insulation layer is maintained between 0.2 mm and 1.4 mm.

[0013] Furthermore, the outer skin insulating layer uses boron nitride powder as a nucleating agent, and uses hydrated magnesium silicate as a foaming agent, and the median particle size is 1.0 μm to 4.5 μm.

[0014] A method for preparing a coaxial cable, based on the above-mentioned composite insulated radio frequency coaxial cable with improved heat resistance, comprises the following steps:

[0015] S1. Preparation of inner skin insulation layer: put the inner conductor into the outlet of the inner skin insulation extruder, and coat the inner conductor surface with fusible polytetrafluoroethylene through chemical foaming extrusion process, and process to form the inner skin insulation layer. During extrusion foaming, put the three components of fusible polytetrafluoroethylene resin particles, foaming agent and composite nucleating agent into a mixer equipped with three independent feeding hoppers, and let the three components enter the extruder chamber according to the selected mixing ratio. During the preparation process, the melt flow rate of fusible polytetrafluoroethylene is limited to 3-16g / 10min, so as to obtain better extrusion foaming processability and make the inner skin insulation layer fully bonded to the surface of the inner conductor;

[0016] S2, cooling of the inner skin insulation layer: after the inner skin insulation layer is formed, the inner skin insulation layer is cooled by the first cooling air ring;

[0017] S3, preparation of the middle insulating layer: after the inner skin insulating layer is cooled and formed, the inner conductor covered with the inner skin insulating layer (2) is introduced into the outer layer insulating extruder, and a blend of high melt strength polypropylene and high density polyethylene is used to form a coating on the inner skin insulating layer by physical foaming extrusion, and the middle insulating layer is processed to form a middle insulating layer. During the extrusion foaming, the nucleating agent masterbatch, high melt strength polypropylene plastic particles, and high density polyethylene plastic particles are mixed uniformly in proportion and then added to the extruder hopper;

[0018] S4, cooling of the middle insulation layer: after the middle insulation layer is formed, it enters the water tank to complete cooling and is blown dry with high-pressure dry air, and then enters the outer insulation extruder for extrusion;

[0019] S5. Preparation of outer skin insulation layer: using polyperfluoroethylene propylene to form an outer skin insulation layer by chemical foaming and extrusion, and coating the outer skin insulation layer on the middle insulation layer. During extrusion and foaming, a chemical foaming agent and a nucleating agent are added to the polyperfluoroethylene propylene base material, and the mixture is uniformly mixed in proportion and then added to the extruder hopper;

[0020] S6. Process the outer conductor on the outer insulation layer.

[0021] Furthermore, in step S1, the foaming agent used in the inner insulating layer is ammonium polyphosphate, and the specific surface area of ​​the processed ammonium polyphosphate powder is not less than 5.5 m 2 / g, the foaming agent is added in an amount of 0.10%wt to 0.5%wt of the mass of the fusible polytetrafluoroethylene resin, a mixed powder composed of boron nitride and calcium tetraborate is used as a composite nucleating agent required for foaming, and the composite nucleating agent is added in an amount of 0.5%wt to 3.5%wt of the mass of the fusible polytetrafluoroethylene base resin, so that the foaming degree of the fusible polytetrafluoroethylene insulation layer is 10% to 35%;

[0022] In step S2, the high melt strength polypropylene selected for the middle insulation layer should have a melt strength greater than 2.0 cN at 200°C, the nucleating agent masterbatch accounts for 0.1%wt to 1.5%wt of the weight of the plastic particles of the middle insulation layer, the extrusion die of the middle insulation extruder adopts an extrusion process, and a gear pump for increasing the die pressure is installed between the extruder head and the machine chamber;

[0023] In step S3, when the high melt strength polypropylene and high density polyethylene blend are physically foamed, CO2 in a supercritical fluid state is injected into the chamber where the polypropylene and high density polyethylene insulation mixture in a molten state are located to fully mix and foam;

[0024] In step S5, the proportion of the foaming agent added to the outer skin insulation layer is 0.10%wt~1.0%wt of the mass of the polyperfluoroethylene propylene base resin, and the foaming degree of the outer skin insulation layer is controlled at 10%~40%. The foaming agent used is hydrated magnesium silicate, and the specific surface area of ​​the processed hydrated magnesium silicate is not less than 5.5m 2 / g.

[0025] Furthermore, the inner skin insulation layer, the middle insulation layer and the outer skin insulation layer are extruded in series, that is, they are continuously processed on the same production line; the distance between the head of the inner skin insulation extruder and the head of the middle insulation extruder is maintained at 1.0m to 5.0m.

[0026] The beneficial effects of the present invention are:

[0027] 1. In the electromagnetic field between the inner and outer conductors of the cable, the electromagnetic field intensity on the surface of the inner conductor of the cable is the largest, which has the greatest impact on the cable attenuation and the highest temperature. Therefore, the inner insulation layer uses fusible polytetrafluoroethylene, which has lower dielectric loss than polyethylene and much higher heat resistance than polyolefin materials. Fusible polytetrafluoroethylene retains the advantages of high temperature resistance and low dielectric loss of polytetrafluoroethylene, with a melting point of up to 310°C. At the same time, it has the characteristics of melt processing that polytetrafluoroethylene does not have, and can adhere to metal well. In order to reduce cable attenuation, the inner insulation layer is made of chemical foaming extrusion process;

[0028] 2. Although the middle insulation layer is not in direct contact with the conductor, it still affects the overall heat resistance of the cable. The heat deformation temperatures of LDPE and HDPE are 38-49°C and 60-82°C respectively. The heat resistance of the traditional RF cable insulation layer is mainly restricted by LDPE. Therefore, replacing the LDPE in the LDPE / HDPE mixture used in RF cables with a high melt strength polypropylene material with better heat resistance and a heat deformation temperature slightly higher than 110°C can significantly improve the heat resistance of the middle insulation layer.

[0029] 3. The outer insulation layer is close to the inner surface of the outer conductor and will be affected by the heat generated by the outer conductor during the use of the cable. However, since the electromagnetic field strength on the inner surface of the outer conductor is lower than that on the outer surface of the inner conductor of the cable, and the DC resistance of the outer conductor is usually smaller than that of the inner conductor, it is easier to dissipate heat. Therefore, the outer conductor has less influence on the cable attenuation and the temperature rise of the conductor than the inner conductor. The outer insulation layer is made of polytetrafluoroethylene propylene material with a heat resistance significantly higher than that of the HMW-PP / HDPE mixture but lower than that of PFA, lower dielectric loss but not as good as that of PFA, and lower cost through a chemical foaming extrusion process. It can improve heat resistance while reducing communication losses and costs, achieving a higher cost-effectiveness. BRIEF DESCRIPTION OF THE DRAWINGS

[0030] The present invention is further described below in conjunction with the accompanying drawings and embodiments.

[0031] Figure 1 It is a side structural schematic diagram of a composite insulated radio frequency coaxial cable with improved heat resistance in the present invention.

[0032] Figure 2 The diagram is a schematic diagram of the end face structure of a composite insulated radio frequency coaxial cable with improved heat resistance in the present invention.

[0033] Figure 3 It is a schematic diagram of the process of the coaxial cable preparation method in the present invention.

[0034] Figure 4 It is a three-dimensional structural schematic diagram of the production line in the present invention.

[0035] Figure 5It is a schematic diagram of the top view of the production line in the present invention.

[0036] Figure 6 It is a schematic structural diagram of the first cooling air ring, the water tank and the second cooling air ring in the present invention.

[0037] Figure 7 It is a schematic structural diagram of the first dust cover in the present invention.

[0038] In the figure: 1, inner conductor; 2, inner insulation layer; 3, intermediate insulation layer; 4, outer insulation layer; 5, outer conductor; 6, sheath layer; 71, inner insulation extruder; 72, intermediate insulation extruder; 721, gas injection system; 722, gas injection port; 73, outer insulation extruder; 74, first dust cover; 741, lower shell; 742, upper shell; 743, transparent observation window; 75, second dust cover; 76, first cooling air ring; 77, water tank; 771, water tank; 772, water box; 773, delivery pump; 774, refrigerator; 775, heat exchanger; 776, nozzle; 78, second cooling air ring; 8, air compressor; 81, three-way pipe. DETAILED DESCRIPTION

[0039] The present invention will now be described in further detail with reference to the accompanying drawings. These drawings are simplified schematic diagrams, which only illustrate the basic structure of the present invention in a schematic manner, and therefore only show the components related to the present invention.

[0040] In the description of the present invention, it should be understood that the terms "center", "longitudinal", "lateral", "length", "width", "thickness", "up", "down", "front", "back", "left", "right", "vertical", "horizontal", "top", "bottom", "inside", "outside", "clockwise", "counterclockwise", "axial", "radial", "circumferential" and the like indicate positions or positional relationships based on the positions or positional relationships shown in the drawings, and are only for the convenience of describing the present invention and simplifying the description, rather than indicating or implying that the device or element referred to must have a specific orientation, be constructed and operated in a specific orientation, and therefore cannot be understood as a limitation on the present invention. In addition, the features defined as "first" and "second" may explicitly or implicitly include one or more of the features. In the description of the present invention, unless otherwise specified, "multiple" means two or more. In the description of the present invention, it should be noted that, unless otherwise clearly specified and limited, the terms "installed", "connected" and "connected" should be understood in a broad sense, for example, it can be a fixed connection, a detachable connection, or an integral connection; it can be a mechanical connection or an electrical connection; it can be a direct connection, or it can be indirectly connected through an intermediate medium, or it can be a connection between the two elements. For those skilled in the art, the specific meanings of the above terms in the present invention can be understood according to specific circumstances.

[0041] The invention discloses a composite insulated radio frequency coaxial cable with improved heat resistance and a preparation method thereof.

[0042] Reference Figure 1 and Figure 2 A composite insulated radio frequency coaxial cable with improved heat resistance comprises an inner conductor 1, a composite insulating layer, an outer conductor 5 and a sheath layer 6 which are arranged in sequence from the inside to the outside. The composite insulating layer comprises an inner skin insulating layer 2, an intermediate insulating layer 3 and an outer skin insulating layer 4 which are arranged in sequence from the inside to the outside. The inner skin insulating layer 2 is a thin-walled insulating layer of tetrafluoroethylene-perfluoroalkyl vinyl ether copolymer extruded by chemical foaming, the intermediate insulating layer 3 is a blend of high melt strength polypropylene and high density polyethylene extruded by physical foaming, and the outer skin insulating layer 4 is a thin-walled insulating layer of polyperfluoroethylene propylene extruded by chemical foaming.

[0043] Specifically, the inner conductor 1 can be a smooth copper tube or a copper-clad aluminum wire. The sheath layer 6 can be made of a high-temperature resistant plastic material and is coated on the outer surface of the outer conductor 5 .

[0044] Specifically, the thickness of the endothelial insulation layer 2 is between 0.2 mm and 1.2 mm, preferably between 0.4 mm and 0.7 mm. The endothelial insulation layer 2 uses ammonium polyphosphate as a foaming agent, and the median particle size is maintained at 1.0 μm to 4.5 μm; the endothelial insulation layer 2 uses a composite nucleating agent containing boron nitride and calcium tetraborate, and the mixing weight ratio of boron nitride and calcium tetraborate in the composite nucleating agent is between 5:5 and 9:1, preferably 7:3.

[0045] Specifically, the weight ratio of high melt strength polypropylene to high density polyethylene in the middle skin insulation layer is 15%wt~40%wt:60%wt~85%wt, preferably 30%wt:70%wt; the nucleating agent used for foaming the middle insulation layer 3 is a nucleating agent masterbatch with HMS-PP as the carrier resin, wherein the weight ratio of PTFE and HMS-PP is 15%wt~50%wt:50%wt~85%wt, preferably 20%wt:80%wt.

[0046] Specifically, the thickness of the outer skin insulation layer 4 is maintained between 0.2 mm and 1.4 mm, preferably between 0.4 mm and 0.8 mm. A thinner outer skin insulation layer 4 can improve heat dissipation performance. The outer skin insulation layer 4 uses boron nitride powder as a nucleating agent and hydrated magnesium silicate as a foaming agent, with a median particle size of 1.0 μm to 4.5 μm.

[0047] The outer conductor 5 is made of copper strip, which is welded by an argon arc welding roller graining machine, coated on the outside of the composite insulation layer, and grained on the outer surface.

[0048] The application also discloses a method for preparing the coaxial cable.

[0049] A method for preparing a coaxial cable, based on the above-mentioned composite insulated radio frequency coaxial cable with improved heat resistance, referring to Figure 3 , including the following steps:

[0050] S1. Preparation of the inner skin insulation layer 2: The inner conductor 1 is placed in an inner skin insulation extruder 71, and the fusible polytetrafluoroethylene is made into the inner skin insulation layer 2 coated on the surface of the inner conductor 1 through a chemical foaming extrusion process. During the extrusion foaming, the three components of the fusible polytetrafluoroethylene resin particles, the foaming agent and the composite nucleating agent are placed in a mixer equipped with three independent feeding hoppers, and the three components are allowed to enter the extruder chamber according to the selected mixing ratio.

[0051] Among them, during the preparation process, the melt flow rate of the fusible polytetrafluoroethylene can be limited to 3 to 16 g / 10 min, preferably 5 to 9 g / 10 min, so as to obtain better extrusion foaming processability and make the inner skin insulation layer 2 fully bonded to the surface of the inner conductor 1. The selected foaming degree of the fusible polytetrafluoroethylene insulation layer is 10% to 35%, preferably 15% to 20%. A chemical foaming agent and a nucleating agent are added to the fusible polytetrafluoroethylene material, and the foaming agent used is ammonium polyphosphate. The specific surface area of ​​the processed ammonium polyphosphate powder is required to be not less than 5.5 m 2 / g, preferably not less than 8.0m 2 / g, the foaming agent is added in an amount of 0.10%wt to 0.5%wt of the mass of the fusible polytetrafluoroethylene resin, preferably 0.15%wt to 0.35%wt. A mixed powder composed of boron nitride and calcium tetraborate is used as a composite nucleating agent required for foaming, and the composite nucleating agent is added in an amount of 0.5%wt to 3.5%wt of the mass of the fusible polytetrafluoroethylene base resin, preferably 1.0%wt to 2.5%wt.

[0052] S2, cooling of the endothelial insulation layer (2): After the endothelial insulation layer (2) is formed, the endothelial insulation layer (2) is cooled by the first cooling air ring 76 to increase the cooling speed of the endothelial insulation layer 2. The distance between the head of the endothelial insulation extruder 71 and the head of the intermediate insulation extruder 72 is maintained at 1.0m to 5.0m.

[0053] S3, preparation of the intermediate insulating layer 3: after the inner skin insulating layer 2 is cooled and formed, the inner conductor 1 covered with the inner skin insulating layer 2 is introduced into the intermediate insulating extruder 72, and the high melt strength polypropylene and high density polyethylene blend are used for physical foaming and extrusion to form the intermediate insulating layer 3 coated on the inner skin insulating layer 2. During the extrusion foaming, the nucleating agent masterbatch, high melt strength polypropylene plastic particles, and high density polyethylene plastic particles are mixed evenly in proportion and added to the extruder hopper. When the high melt strength polypropylene and high density polyethylene blend are physically foamed, CO2 in a supercritical fluid state is injected into the machine chamber where the polypropylene and high density polyethylene insulation mixture in the molten state is located, that is, the machine chamber of the intermediate insulating extruder 72, and is fully mixed and foamed.

[0054] The melt strength of the selected high melt strength polypropylene at 200°C should be greater than 2.0 cN, preferably greater than 3.5 cN. The extrusion die of the intermediate insulating extruder 72 adopts an extrusion process, and a gear pump for increasing the head pressure is installed between the extruder head and the machine chamber. During extrusion foaming, the nucleating agent masterbatch, high melt strength polypropylene plastic particles, and high density polyethylene plastic particles are mixed uniformly in proportion and added to the extruder hopper, and the nucleating agent masterbatch accounts for 0.1%wt to 1.5%wt of the weight of the high melt strength polypropylene plastic particles / high density polyethylene plastic particles, preferably 0.4%wt to 0.8%wt.

[0055] S4, cooling of the intermediate insulating layer 3: After the intermediate insulating layer 3 is formed, the inner conductor 1 with the inner skin insulating layer 2 and the intermediate insulating layer 3 enters the water tank 77 to complete cooling and is blown dry with high-pressure dry air, and then enters the outer skin insulation extruder 73 for extrusion.

[0056] S5. Preparation of outer skin insulation layer 4: The outer skin insulation layer 4 covering the middle insulation layer 3 is formed by chemical foaming extrusion of polyperfluoroethylene propylene. During extrusion foaming, chemical foaming agent and nucleating agent are added to the polyperfluoroethylene propylene base material, which are mixed evenly in proportion and then added to the extruder hopper.

[0057] The proportion of the foaming agent added to the outer skin insulation layer 4 is 0.10%wt~1.0%wt of the mass of the polyperfluoroethylene propylene base resin, preferably 0.40%wt~0.7%wt. The foaming degree of the outer skin insulation layer 4 is controlled at 10%~40%, preferably 15%~25%; the foaming agent used is hydrated magnesium silicate, and the specific surface area of ​​the processed hydrated magnesium silicate is not less than 5.5m 2 / g, preferably not less than 8.5m 2 / g.

[0058] S6. Process the outer conductor 5 on the outer insulation layer 4 and process the sheath layer 6 on the outer conductor 5.

[0059] In addition, the inner insulating layer 2, the middle insulating layer 3 and the outer insulating layer 4 are formed by serial extrusion, that is, by continuous processing on the same production line.

[0060] Reference Figures 4 to 7 The production line includes an inner skin insulation extruder 71, an intermediate insulation extruder 72 and an outer skin insulation extruder 73 arranged in sequence. The intermediate insulation extruder 72 is provided with an air injection port 722, and the air injection port 722 is connected to an air injection system 721. The air injection system 721 is convenient for injecting CO2 in a supercritical fluid state into the machine chamber of the intermediate insulation extruder 72 when the high melt strength polypropylene and high density polyethylene blend are physically foamed, and fully mixed with the polypropylene and high density polyethylene insulation mixture in the molten state and foamed. A first dust cover 74 is provided between the inner skin insulation extruder 71 and the middle insulation extruder, and a first cooling air ring 76 is provided in the first dust cover 74. A second dust cover 75 is provided between the intermediate insulation extruder 72 and the outer skin insulation extruder 73, and a water tank 77 and a second cooling air ring 78 are provided in the second dust cover 75. The first cooling air ring 76, the water tank 77 and the second cooling air ring 78 can be moved by moving the first dust cover 74 and the second dust cover 75, which is simple and convenient.

[0061] Specifically, the first dust cover 74 and the second dust cover 75 each include a lower shell 741 and an upper shell 742, the lower shell 741 and the upper shell 742 are separately provided and can be connected by bolts. A transparent observation window 743 is installed on the upper shell 742 to observe the internal situation.

[0062] More specifically, the first cooling air ring 76 is connected to the lower shell 741 of the first dust cover 74, and a first cooling cavity is provided in the first cooling air ring 76 for passing cooling gas, and a plurality of injection ports are provided on the inner wall of the first cooling air ring 76 along its circumference, and the injection ports are connected to the first cooling cavity, so that the cooling gas in the first cooling cavity is sprayed toward the endothelial insulation layer 2 in the first cooling air ring 76, thereby quickly cooling the endothelial insulation layer 2. The structure of the second cooling air ring 78 is the same as that of the first cooling air ring 76, and will not be repeated here.

[0063] The water tank 77 includes a water box 772 and a water tank 771. The water tank 771 is connected to the lower shell 741 of the second dust cover 75, and the water box 772 is installed in the water tank 771. A through hole is provided in the horizontal direction on the water box 772 so that the inner conductor 1 with the inner skin insulation layer 2 and the middle insulation layer 3 can pass through. A leaking hole is provided at the bottom of the water box 772 so that the cooling water in the water box 772 can flow into the water tank 771. A delivery pump 773 is installed at the bottom of the water tank 771, and the input end of the delivery pump 773 is connected to the bottom of the water tank 771, and the output end of the delivery pump 773 is connected to the refrigerator 774. The output end of the refrigerator 774 is connected to a heat exchanger 775, and the heat exchanger 775 has a first heat exchange channel and a second heat exchange channel. The input end of the first heat exchange channel is connected to the output end of the refrigerator 774, and the output end of the first heat exchange channel is connected to a nozzle 776, which is installed on the water box 772 so as to input cooling water into the water box 772, thereby forming a circulating cooling. The nozzle 776 is arranged at one end of the water box 772 away from the middle insulation extruder 72, so that the temperature of the cooling water in the water box 772 gradually decreases along the direction from the middle insulation extruder 72 to the outer skin insulation extruder 73, thereby making the cooling speed of the middle insulation layer 3 relatively slow, reducing the possibility of excessive internal stress of the middle insulation layer 3 caused by too fast cooling speed.

[0064] An air compressor 8 is provided on one side of the heat exchanger 775, and an air filter and a dehumidifier are connected to the input end of the air compressor 8 so that the air compressor 8 outputs high-speed, high-pressure, pure and dry gas. The output end of the air compressor 8 is connected to the input end of the second heat exchange channel, and the output end of the second heat exchange channel is connected to a three-way pipe 81, and the other two ends of the three-way pipe 81 are respectively connected to the first cooling air ring 76 and the second cooling air ring 78 to input cooling gas to the first cooling air ring 76 and the second cooling air ring 78. The heat exchanger 775 can be a plate heat exchanger or a tube heat exchanger.

[0065] During operation, the inner conductor 1 with the inner skin insulation layer 2 passes through the first cooling air ring 76, enters the machine chamber of the intermediate insulation extruder 72 after being cooled by the first cooling air ring 76, and then the intermediate insulation extruder 72 outputs the inner conductor 1 with the inner skin insulation layer 2 and the intermediate insulation layer 3, and the inner conductor 1 with the inner skin insulation layer 2 and the intermediate insulation layer 3 passes through the water box 772, and then passes through the second cooling air ring 78, and enters the machine chamber of the outer skin insulation extruder 73. At this time, the delivery pump 773 extracts the cooling water in the water tank 771 and inputs it into the refrigerator 774. The cooling water cooled by the refrigerator 774 passes through the first heat exchange channel and flows out from the nozzle 776 into the water box 772. At the same time, the air compressor 8 outputs gas, and the gas passes through the second heat exchange channel, exchanges heat with the cooling water in the first heat exchange channel, and then enters the first cooling air ring 76 and the second cooling air ring 78 respectively.

[0066] The following examples further illustrate the scheme of the present invention in conjunction with the optimized process.

[0067] Embodiment 1:

[0068] Applicable to the HCAAY-50-12 cable (cable specification is -12) in the YD / T 1092 standard, the inner conductor 1 is a copper-clad aluminum wire with a diameter of 4.80 mm.

[0069] The thickness of the endothelial insulation layer 2 is 0.4 mm, and the foaming degree is 20%. The endothelial insulation layer 2 uses DuPont TEFLON 340. The nucleating agent boron nitride (BN) uses BN-B from Liaobin Chemical Company, and the median particle size is 1-2μm; the nucleating agent calcium tetraborate (CTB) uses CTB from Shanghai Jinjinle Chemical Testing Company, and is mechanically refined. The extrusion die of the endothelial insulation extruder adopts an extrusion process, and the extrusion melt temperature is controlled at 320-365℃. A mixed powder composed of boron nitride (BN) and calcium tetraborate (CTB) is used as the composite nucleating agent required for foaming. The mixing ratio (mass ratio) of BN and CTB in the composite nucleating agent is 7:3, and the addition ratio of the composite nucleating agent is 1.5%wt of the weight of the PFA base resin.

[0070] The thickness of the intermediate insulating layer 3 is 3.1 mm, and the foaming degree is 72%. The intermediate insulating layer 3 can be made of high melt strength polypropylene such as HMS20Z of Sinopec, PP-UMS of SABIC, GCH0002 of Zibo Gechen Plastic Technology Co., Ltd. There are many domestic and foreign companies on the market that provide high-density polyethylene materials for RF cable insulation foaming, which are not listed here.

[0071] The thickness of the outer insulation layer 4 is 0.3 mm, the foaming degree is 20%, and the outer diameter of the cable insulation is 12.4 mm. The polyperfluoroethylene propylene base materials used are DuPont TEFLON 9475 and Zhejiang Juhua cable insulation grade FEP. Talc powder is purchased from the market and then mechanically refined. The extrusion melt temperature is controlled at 305-350℃, and the extrusion tube extrusion is adopted, and the extrusion draw ratio (DDR) is controlled at 10.

[0072] Compared with conventional foamed polyethylene insulated RF cables of the same specification (cable specification is -12), the peak power of conventional foamed polyethylene insulated RF cables is 40 kW, and the peak power of the structural cable of the present application is increased to 48 kW, an increase of 20%. Therefore, the insulation layer of the structural cable of the present application can significantly improve the heat resistance of the coaxial cable.

[0073] Embodiment 2:

[0074] Used for cables with model HCTAY-50-22 in YD / T 1092 standard, cable specification is -22.

[0075] The difference from Example 1 is that the inner conductor 1 is a copper tube with an outer diameter of 9.00 mm, the inner insulation layer 2 is 0.6 mm thick and has a foaming degree of 3%; the middle insulation layer 3 is 5.4 mm thick and has a foaming degree of 74%; the outer insulation layer 4 is 0.7 mm thick and has a foaming degree of 25%, and the cable insulation outer diameter is 2.4 mm.

[0076] The sources of materials used and the main process conditions are basically the same as those in Example 1.

[0077] Compared with conventional foamed polyethylene insulated RF cables of the same specification (cable specification is -22), the peak power of conventional foamed polyethylene insulated RF cables is 80 kW, and the peak power of the structural cable of the present application is increased to 95 kW, an increase of about 19%. Therefore, the insulation layer of the structural cable of the present application can significantly improve the heat resistance of the coaxial cable.

[0078] Based on the above ideal embodiments of the present invention, the relevant staff can make various changes and modifications without departing from the technical concept of the present invention through the above description. The technical scope of the present invention is not limited to the contents of the specification, and its technical scope must be determined according to the scope of the claims.

Claims

1. A composite insulated radio frequency coaxial cable with improved heat resistance, characterized in that: The invention comprises an inner conductor (1), a composite insulating layer, an outer conductor (5) and a sheath layer (6) which are arranged in sequence from the inside to the outside. The composite insulating layer comprises, in sequence from the inside to the outside: an inner skin insulating layer (2), an intermediate insulating layer (3) and an outer skin insulating layer (4). The inner skin insulating layer (2) is a thin-walled insulating layer of tetrafluoroethylene-perfluoroalkyl vinyl ether copolymer extruded by chemical foaming, the intermediate insulating layer (3) is a blend of high melt strength polypropylene and high density polyethylene extruded by physical foaming, and the outer skin insulating layer (4) is a thin-walled insulating layer of polyperfluoroethylene propylene extruded by chemical foaming.

2. The composite insulated radio frequency coaxial cable with improved heat resistance according to claim 1, characterized in that: The thickness of the endothelial insulation layer (2) is between 0.2 mm and 1.2 mm.

3. The composite insulated radio frequency coaxial cable with improved heat resistance according to claim 1, characterized in that: The inner skin insulation layer (2) uses ammonium polyphosphate as a foaming agent, and the median particle size is maintained at 1.0 μm to 4.5 μm; The endothelial insulating layer (2) uses a composite nucleating agent comprising boron nitride and calcium tetraborate, wherein the mixing weight ratio of the boron nitride and calcium tetraborate in the composite nucleating agent is between 5:5 and 9:

1.

4. The composite insulated radio frequency coaxial cable with improved heat resistance according to claim 1, characterized in that: The weight ratio of high melt strength polypropylene to high density polyethylene in the intermediate insulating layer (3) is 15%wt-40%wt: 60%wt-85%wt.

5. A composite insulated radio frequency coaxial cable with improved heat resistance as claimed in claim 1, characterized in that: The nucleating agent used for foaming the intermediate insulating layer (3) is a nucleating agent masterbatch with HMS-PP as a carrier resin, wherein the weight ratio of PTFE to HMS-PP is 15%wt-50%wt:50%wt-85%wt.

6. The composite insulated radio frequency coaxial cable with improved heat resistance according to claim 1, characterized in that: The thickness of the outer insulation layer (4) is maintained between 0.2 mm and 1.4 mm.

7. A composite insulated radio frequency coaxial cable with improved heat resistance as claimed in claim 1, characterized in that: The outer skin insulating layer (4) uses boron nitride powder as a nucleating agent and hydrated magnesium silicate as a foaming agent, and the median particle size is 1.0 μm to 4.5 μm.

8. A method for preparing a coaxial cable, based on the composite insulated radio frequency coaxial cable with improved heat resistance according to any one of claims 1 to 7, characterized in that: The steps include: S1. Preparation of the inner skin insulation layer (2): the inner conductor (1) is placed at the outlet of the head of the inner skin insulation extruder (71), and fusible polytetrafluoroethylene is coated on the surface of the inner conductor (1) through a chemical foaming extrusion process, and the inner skin insulation layer (2) is formed. During the extrusion foaming, the three components of fusible polytetrafluoroethylene resin particles, foaming agent and composite nucleating agent are placed in a mixer equipped with three independent feeding hoppers, and the three components are allowed to enter the extruder chamber according to a selected mixing ratio. During the preparation process, the melt flow rate of the fusible polytetrafluoroethylene is limited to 3 to 16 g / 10 min to obtain better extrusion foaming processability and to ensure that the inner skin insulation layer (2) is fully bonded to the surface of the inner conductor (1); S2, cooling the endothelial insulation layer (2): after the endothelial insulation layer (2) is formed, the endothelial insulation layer (2) is cooled by a first cooling air ring (76); S3, preparation of the intermediate insulating layer (3): after the inner skin insulating layer (2) is cooled and formed, the inner conductor (1) covered with the inner skin insulating layer (2) is introduced into the intermediate insulating extruder (72), and a blend of high melt strength polypropylene and high density polyethylene is formed by physical foaming and extrusion to cover the inner skin insulating layer (2), and the intermediate insulating layer (3) is formed. During the extrusion foaming, the nucleating agent masterbatch, high melt strength polypropylene plastic particles, and high density polyethylene plastic particles are mixed uniformly in proportion and then added to the extruder hopper; S4, cooling of the middle insulating layer (3): after the middle insulating layer (3) is formed, it enters a water tank to complete cooling and is blown dry with high-pressure dry air, and then enters an outer skin insulation extruder (73) for extrusion; S5, preparation of the outer skin insulation layer (4): using polyperfluoroethylene propylene to form a coating on the middle insulation layer (3) through chemical foaming extrusion, processing to form the outer skin insulation layer (4), during extrusion foaming, adding a chemical foaming agent and a nucleating agent to the polyperfluoroethylene propylene base material, mixing them evenly in proportion, and then adding them to the extruder hopper; S6. Processing the outer conductor (5) on the outer insulation layer (4).

9. A method for preparing a coaxial cable according to claim 8, characterized in that: In step S1, the foaming agent used in the inner insulating layer is ammonium polyphosphate, and the specific surface area of ​​the processed ammonium polyphosphate powder is not less than 5.5m 2 / g, the foaming agent is added in an amount of 0.10%wt to 0.5%wt of the mass of the fusible polytetrafluoroethylene resin, a mixed powder composed of boron nitride and calcium tetraborate is used as a composite nucleating agent required for foaming, and the composite nucleating agent is added in an amount of 0.5%wt to 3.5%wt of the mass of the fusible polytetrafluoroethylene base resin, so that the foaming degree of the fusible polytetrafluoroethylene insulation layer is 10% to 35%; In step S2, the high melt strength polypropylene selected for the middle insulating layer (3) should have a melt strength greater than 2.0 cN at 200°C, the nucleating agent masterbatch accounts for 0.1%wt to 1.5%wt of the weight of the plastic particles of the middle insulating layer (3), the extrusion die of the middle layer insulation extruder adopts an extrusion process, and a gear pump for increasing the die head pressure is installed between the extruder head and the machine chamber; In step S3, when the high melt strength polypropylene and high density polyethylene blend are physically foamed, CO2 in a supercritical fluid state is injected into the chamber where the polypropylene and high density polyethylene insulation mixture in a molten state are located to fully mix and foam; In step S5, the proportion of the foaming agent added to the outer skin insulation layer (4) is 0.10%wt to 1.0%wt of the mass of the polyperfluoroethylene propylene base resin, and the foaming degree of the outer skin insulation layer (4) is controlled at 10% to 40%. The foaming agent used is hydrated magnesium silicate, and the specific surface area of ​​the processed hydrated magnesium silicate is not less than 5.5m 2 / g.

10. The method for preparing a coaxial cable according to claim 8, characterized in that: The inner insulating layer (2), the middle insulating layer (3) and the outer insulating layer (4) are formed by serial extrusion, that is, by continuous processing on the same production line; The distance between the head of the inner skin insulation extruder and the head of the middle insulation extruder is maintained at 1.0m to 5.0m.

Citation Information

Patent Citations

  • Flame-retardant high-speed data cable for 5G data center system and manufacturing system of flame-retardant high-speed data cable

    CN110211733A

  • Coaxial cable for movable part

    CN111724929A

  • Three-layer co-extrusion production method of medium-voltage polypropylene insulated wire core

    CN115312271A

  • Masterbatch for foaming resin composition, foamed coaxial cable and method for producing the same