Positive electrode material, preparation method thereof and electrochemical device

By doping Nb and B elements in the cathode material to form strong chemical bonds and coating layers, the problem of poor cycle performance of lithium-rich manganese-based cathode materials is solved, its rate performance and cycle stability are significantly improved, and efficient batteries are achieved. chemical properties.

CN118763203APending Publication Date: 2024-10-11NANTONG RESHINE NEW MATERIAL CO LTD
View PDF 0 Cites 1 Cited by

Patent Information

Application Number
CN202411009533.6
Authority / Receiving Office
CN · China
Patent Type
Applications(China)
Current Assignee / Owner
Filing Date
2024-07-25
Publication Date
2024-10-11

AI Technical Summary

Technical Problem

Lithium-rich manganese-based cathode materials have "oxygen release" phenomena and electrolyte oxidation reactions during the cycle, resulting in low first Coulombic efficiency and poor cycle performance, which limits their commercial promotion.

Method used

Nb element and B element are doped in the crystal lattice of the cathode material. Nb element forms a strong chemical bond with oxygen, inhibiting the release of oxygen. B element adjusts the electronic structure, forms a B2O3 coating layer to prevent electrolyte corrosion, and generates Li2O-B2O3 Lithium-ion conductor structure improves cycle performance.

Benefits of technology

Through the synergistic effect of Nb and B, the rate performance and cycle performance of the cathode material are significantly improved, the phase transition is delayed, the structural stability is enhanced, the transition metal dissolution and capacity loss are reduced, and the discharge capacity and cycle stability of the battery are improved. .

✦ Generated by Eureka AI based on patent content.

Smart Images

  • Figure CN118763203A_ABST
    Figure CN118763203A_ABST
Patent Text Reader

Abstract

The invention discloses a positive electrode material, a preparation method thereof and an electrochemical device, crystal lattices of the positive electrode material contain an Nb element and a B element, and the molar ratio of the doping amount of the Nb element to the doping amount of the B element is 1: (1-2). According to the positive electrode material, the Nb element and the B element are doped, the proportion of the doping amount of the Nb element and the doping amount of the B element is precisely regulated and controlled, and the synergistic effect of the Nb element and the B element is fully exerted, so that the first coulombic efficiency and the cycle performance of the positive electrode material are improved.
Need to check novelty before this filing date? Find Prior Art

Description

Technical Field

[0001] This application relates to the technical field of new energy materials, and particularly relates to a cathode material, a preparation method thereof, and an electrochemical device. Background Art

[0002] The lithium-rich manganese-based cathode material can be regarded as composed of two components, Li2MnO3 and LiMO2. The general composition can be expressed as xLi2MnO3·(1 - x)LiMO2 (0 < x < 1, M is at least one of transition metals such as Ni, Co, Mn, etc.). The lithium-rich manganese-based cathode material exhibits a high discharge specific capacity of 300 mAh / g at a low rate of 0.1C, far exceeding the 210 mAh / g of the high-nickel NCM811 ternary cathode material at the same rate, and has great potential to achieve an energy density of 400 Wh / kg for the battery cell. It is the most promising candidate for the next-generation lithium-ion cathode material.

[0003] However, the lithium-rich manganese-based cathode material has an "oxygen release" phenomenon and an electrolyte oxidation reaction during the cycling process, resulting in a low initial Coulombic efficiency and poor cycling performance of the lithium-rich manganese-based cathode material, which limits the commercial promotion of the lithium-rich manganese-based cathode material. Summary of the Invention

[0004] In view of this, in order to solve at least one of the above technical problems, an embodiment of this application provides a cathode material.

[0005] In addition, an embodiment of this application also provides a preparation method of the foregoing cathode material, and an electrochemical device using the cathode material.

[0006] An embodiment of this application provides a cathode material, wherein the lattice of the cathode material contains Nb element and B element, and the molar ratio of the doping amount of Nb element to the doping amount of B element is 1:(1 - 2).

[0007] In some possible embodiments, in terms of mole percentage, the doping amount of Nb element is 10% - 15%, and the doping amount of B element is 10% - 18%.

[0008] In some possible embodiments, a B2O3 coating layer is formed on the surface of the cathode material.

[0009] In some possible embodiments, the B2O3 coating layer contains a Li2O - B2O3 lithium ion conductor structure.

[0010] In some possible embodiments, the particle size D50 of the cathode material is 6.0 μm - 8.5 μm.

[0011] An embodiment of this application also provides a preparation method of a cathode material, including:

[0012] Mixing a transition metal oxide precursor, a lithium source, a B source and a Nb source to obtain a mixed material, wherein the molar ratio of the Nb source to the B source is 1:(1-2);

[0013] sintering the mixed material once to obtain a primary sintered material;

[0014] Dispersing the primary sintered material to obtain a dispersed material; and

[0015] The dispersed material is subjected to secondary sintering to obtain the positive electrode material, wherein during the secondary sintering process, the Nb element and the B element enter into the crystal lattice of the positive electrode material.

[0016] In some possible embodiments, the molar ratio of the transition metal oxide precursor, the lithium source, the Nb source and the B source is 1: (1.30-1.35): (0.1-0.15): (0.1-0.18).

[0017] In some possible embodiments, the primary sintering temperature is 400° C. to 600° C., and the primary sintering time is 5 h to 12 h.

[0018] In some possible embodiments, the secondary sintering temperature is 700° C. to 950° C., and the secondary sintering time is 5 h to 10 h.

[0019] In some possible embodiments, in the step of mixing the transition metal oxide precursor, lithium source, B source and Nb source, a step-by-step mixing method is adopted, and the step-by-step mixing includes a first step mixing and a second step mixing. The rotation speed of the first step mixing is 300r / min~500r / min, and the mixing time of the first step is 5min~10min. The rotation speed of the second step mixing is 500r / min~750r / min, and the mixing time of the second step is 5min~15min.

[0020] In some possible embodiments, in the step of dispersing the primary sintered material, the dispersing rotation speed is 500 r / min to 700 r / min, and the dispersing time is 6 min to 10 min.

[0021] In some possible embodiments, the molecular formula of the transition metal oxide precursor is Ni c Mn 1-c (OH)2,0.3 <c<0.4。

[0022] In addition, an embodiment of the present application further provides an electrochemical device, which includes a positive electrode plate, a negative electrode plate, a separator and an electrolyte, wherein the positive electrode plate includes a positive electrode active substance, and the positive electrode active substance is the aforementioned positive electrode material.

[0023] Compared with the prior art, the positive electrode material provided in the embodiment of the present application is a positive electrode material doped with Nb element and B element, wherein Nb element and B element are doped in the lattice of the positive electrode material. The strong binding between Nb element and oxygen inhibits the release of lattice oxygen, delays the phase transition, and at the same time, the corresponding proportion of B element doped acts on the additional electrons brought by Nb doping, adjusts the electronic structure inside the positive electrode material, and reduces the drawbacks of transition metal dissolution and capacity loss caused by Nb doping. By regulating the ratio of the doping amount of Nb element and B element, Nb element and B element effectively play a synergistic role, which effectively improves the rate performance and cycle performance of the positive electrode material. BRIEF DESCRIPTION OF THE DRAWINGS

[0024] Figure 1 A process flow chart of the method for preparing the positive electrode material provided in an embodiment of the present application.

[0025] Figure 2 This is a schematic diagram of the structure of the electrochemical device provided in an embodiment of the present application.

[0026] Figure 3 This is a scanning electron microscope image of the positive electrode material of Example 1 of the present application.

[0027] Figure 4 This is the X-ray diffraction pattern of the positive electrode material of Example 1 of the present application.

[0028] Figure 5 This is a comparison chart of the first charge and discharge curves of the battery prepared with the positive electrode materials in Example 1 of the present application and Comparative Example 1 at 0.1C.

[0029] Figure 6 It is a comparison chart of the cycle capacity retention rate curves at 45°C of the batteries prepared with the positive electrode materials in Example 1 of the present application and Comparative Example 1. DETAILED DESCRIPTION

[0030] The following will be combined with the drawings in the embodiments of the present application to clearly and completely describe the technical solutions in the embodiments of the present application. Obviously, the described embodiments are only part of the embodiments of the present application, not all of the embodiments. Based on the embodiments of the present application, all other embodiments obtained by those skilled in the art without creative work are within the scope of protection of the present application.

[0031] In order to solve the problem of poor first coulombic efficiency and cycle performance of positive electrode materials (especially lithium-rich manganese-based positive electrode materials), researchers have tried to use doping modification methods, most of which choose to add transition metal elements to enhance the bond energy between transition metal elements and oxygen elements in the positive electrode materials, thereby improving the cycle stability of the positive electrode materials. However, these methods either use expensive additives or require additional sintering steps, which cannot meet the needs of large-scale industrial production.

[0032] The inventors of the present application have found that when a certain proportion of Nb and B elements are co-doped into the positive electrode material, the synergistic effect of Nb and B will have a significant impact on the first coulombic efficiency and cycle performance of the positive electrode material. For this reason, an embodiment of the present application provides a positive electrode material, wherein the lattice of the positive electrode material contains Nb and B elements, and the molar ratio of the doping amount of the Nb element to the doping amount of the B element is 1:(1~2).

[0033] When the positive electrode material is under high working voltage, oxygen atoms will be precipitated in the lattice, affecting the cycle performance and stability of the positive electrode material. Especially for lithium-rich manganese-based positive electrode materials, when the voltage exceeds 4.4V during charging, a voltage platform will appear around 4.5V. At this time, Li in the Li2MnO3 phase + and O are released to generate electrochemically active MnO2. During the charging process at this voltage platform, the release of O is accompanied by the precipitation of O2, resulting in the loss of free oxygen, which in turn causes Li + It cannot be normally embedded back into the positive electrode material to generate Li2O, and the lack of oxygen vacancies will also cause Mn 4+ The migration of oxygen into the spinel phase is the "oxygen release" mechanism of lithium-rich manganese-based cathode materials. In addition, the released free oxygen will also oxidize the electrolyte, causing serious gas production in the battery, accompanied by the release of a large amount of heat, leading to thermal runaway of the battery.

[0034] By doping Nb and B elements in the positive electrode material and controlling the molar ratio of the doping amount of Nb and B elements to be 1:(1-2), the synergistic effect of Nb and B elements can be fully exerted, and the rate performance and cycle performance of the positive electrode material can be effectively improved. The strong binding between Nb and oxygen can inhibit the release of lattice oxygen, delay phase transformation, and improve the cycle performance of the positive electrode material. However, the doping of Nb also introduces excess electrons. The doping of B elements in a certain proportion with Nb elements can neutralize the above-mentioned excess electrons, adjust the electronic structure inside the positive electrode material, and reduce the disadvantages of transition metal dissolution and capacity loss caused by Nb doping.

[0035] In some embodiments, the doping amount of Nb element can be 10% to 15% in molar percentage. By doping a certain amount of Nb element, Nb element can not only form a strong chemical bond with oxygen, inhibit the oxidation of lattice oxygen, reduce the release of O2, delay phase transition, and improve the stability and cycle life of the positive electrode material, but also adjust the crystal structure and lattice parameters of the positive electrode material, thereby enhancing the structural stability of the material and inhibiting structural changes and mechanical damage during the charge and discharge cycle. Doping Nb element in the lattice is also beneficial to improving the electronic structure and electronic state density of the positive electrode material, optimizing the conductivity and electronic transmission performance of the material, thereby improving the discharge capacity, cycle stability and high rate performance of the battery. The doping amount of the Nb element can further be 10% to 13%, and can be 10%, 11%, 12%, 13%, 14% or 15% for example. If the doping amount of the Nb element is too little (less than 10%), the release of lattice oxygen cannot be fully suppressed, which will lead to a reduction in the doping modification effect; if the doping amount of the Nb element is too much (greater than 15%), too many electrons will be introduced, changing the electronic structure and crystal structure of the positive electrode material, resulting in a decrease in electrochemical performance, such as a decrease in specific capacity and cycle stability, and also causing the crystal structure of the positive electrode material to be unstable, thereby affecting the long-term stability and cycle life of the positive electrode material. Therefore, controlling the doping of the Nb element within the above range is conducive to improving the electrochemical performance and structural stability of the positive electrode material.

[0036] In some embodiments, the doping amount of the B element can be 10% to 18% by mole percentage, and further can be 13% to 18%, and can be 10%, 11%, 12%, 13%, 14%, 15%, 16%, 17% or 18% by mole percentage. Too little doping of the B element (less than 10%) will result in the inability to completely offset the excess electrons introduced by Nb, resulting in capacity loss, etc.; too high doping of the B element (greater than 18%) will result in a too thick B2O3 coating layer, which will affect ion transmission and reduce the conductivity of the positive electrode material. Therefore, by controlling the doping amount of the B element within the above range, it is possible to optimize and adjust the electronic structure of the positive electrode material, improve the cycle stability of the positive electrode material, and ensure the transmission efficiency of the ions.

[0037] In addition, the appropriate amount of B doping can generate B2O3 as a coating layer on the surface of the positive electrode material during the sintering process without an additional coating process. The B2O3 coating layer has good chemical stability and electrochemical stability, which can effectively prevent the corrosion of the electrolyte to the positive electrode material and improve the cycle performance of the positive electrode material.

[0038] Furthermore, the B2O3 coating layer may react with the Li2O formed during the sintering process of the positive electrode material to form a Li2O-B2O3 lithium ion conductor structure with good ionic conductivity. This composite lithium ion conductor structure facilitates the rapid transport and diffusion of lithium ions in the positive electrode material.

[0039] In some embodiments, the molecular formula of the positive electrode material can be Li a Mn b Ni 2-a-b Nb x B y , 1.1<a<1.3, 0<b<0.7, 0.1<x<0.15, 0.1<y<0.18. The positive electrode material provided in the present application can be a lithium-rich manganese-based positive electrode material mainly composed of Mn elements and free of Co elements, which can reduce costs, improve safety, and reduce dependence on scarce resources while providing good electrochemical performance.

[0040] In some embodiments, the particle size D50 of the positive electrode material is 6.0 μm to 8.5 μm, and further can be 7.0 μm to 8.0 μm, and can be 7.0 μm, 7.1 μm, 7.2 μm, 7.3 μm, 7.4 μm, 7.5 μm, 7.6 μm, 7.7 μm, 7.8 μm, 7.9 μm or 8.0 μm, etc. By controlling the particle size within the above-defined range, the positive electrode material has a suitable specific surface area and good consistency, which is conducive to optimizing the electrochemical performance of the positive electrode material and preventing the reduction of the electrochemical performance of the positive electrode material due to too small or too large particles.

[0041] Compared with the prior art, the positive electrode material provided in the embodiment of the present application has the following beneficial effects:

[0042] 1. The B element and the Nb element are co-doped in a certain ratio, where the Nb element forms a strong chemical bond with oxygen, effectively inhibiting the release of lattice oxygen and delaying phase transformation; the introduction of the B element alleviates the extra electrons brought by Nb doping, and reduces the metal dissolution and capacity loss caused by Nb doping. The synergistic effect of the B element and the Nb element improves the first coulomb efficiency and cycle performance of the positive electrode material.

[0043] 2. B element doping can generate B2O3 as a coating layer, which effectively prevents the corrosion of the electrolyte to the positive electrode material and improves the cycle performance of the positive electrode material.

[0044] 3. B2O3 can further react with Li2O to generate Li2O-B2O3 lithium ion conductor structure, thus improving the efficiency of lithium ion transmission.

[0045] 4. The positive electrode material provided in the embodiment of the present application is mainly composed of Mn element and does not contain Co element. It can reduce costs, improve safety, and reduce dependence on scarce resources while providing good electrochemical performance, which meets the sustainable development requirements of modern positive electrode material design.

[0046] See also Figure 1As shown, the preparation method of the cathode material provided by the embodiments of the present application specifically includes the following steps:

[0047] Step S1, mix a transition metal oxide precursor, a lithium source, a B source, and a Nb source to obtain a mixed material, where the molar ratio of the Nb source to the B source is 1:(1-2).

[0048] In some embodiments, the molar ratio of the transition metal oxide precursor, the lithium source, the Nb source, and the B source can be 1:(1.30-1.35):(0.1-0.15):(0.1-0.18), and further can be 1:(1.31-1.33):(0.1-0.13):(0.13-0.18). Exemplarily, it can be 1:1.33:0.1:0.15. Controlling the mixing ratio of the above raw materials can precisely adjust the proportion of each chemical component to optimize the physical and chemical properties of the target cathode material and ensure that the final cathode material meets the expected performance requirements. It should be noted that appropriate doping amounts of the B source and the Nb source are the key to the best synergistic effect of B and Nb. Excessive or too little ratio will lead to poor synergistic effect of B and Nb, causing a significant decline in the rate performance and cycling performance of the cathode material.

[0049] In some embodiments, the mixing in this step can be stepwise mixing. The stepwise mixing can be two-step mixing, including the first-step mixing and the second-step mixing. The rotation speed of the first-step mixing is 300 r / min - 500 r / min, and the time is 5 min - 10 min; the rotation speed of the second-step mixing is 500 r / min - 750 r / min, and the time is 5 min - 15 min. Exemplarily, a dry mixing process is used to mix the materials. First, run at a low speed for a certain time to achieve the purpose of macroscopic mixing of the materials in the mixer, and then run at a high speed for a period of time to achieve uniform mixing of the microparticles microscopically, so that the materials are mixed evenly without the need to add additional solvents. It can be understood that the mixing method includes but is not limited to the above method, as long as the purpose of uniform mixing is achieved.

[0050] In some embodiments, the molecular general formula of the transition metal oxide precursor can be Ni c Mn 1-c (OH)2, 0.3 < c < 0.4. Selecting nickel-manganese hydroxide as the precursor, with Mn as the main component and no Co element, can significantly improve the cost performance.

[0051] In some embodiments, the lithium source can be at least one of lithium hydroxide, lithium carbonate, and lithium oxalate.

[0052] Step S2, perform a first sintering on the mixed material in step S1 to obtain a first sintered material.

[0053] After the mixing is completed, a primary sintering is performed in a reaction device (such as a box furnace), and this step is performed by low-temperature sintering at 400°C to 600°C for 5h to 12h. Further, the temperature of the primary sintering can be 500°C to 550°C, and can be 400°C, 450°C, 500°C, 550°C or 600°C, etc. Low-temperature primary sintering can remove volatile substances, which is beneficial to subsequent process steps (such as dispersion and secondary sintering), aiming to improve the stability of the final positive electrode material.

[0054] Furthermore, before the primary sintering, pre-sintering can be carried out at 300°C to 700°C for 3h to 8h. Pre-sintering at 300°C to 700°C helps to reduce the thermal stress of the primary sintering, further control the particle size and morphology of the primary sintered material, and improve the uniformity and stability of the primary sintered material.

[0055] Step S3, dispersing the primary sintered material to obtain dispersed material.

[0056] Since the primary sintered material will have some agglomeration after the primary sintering, if the secondary sintering is performed directly without dispersion, it will affect the nucleation and grain growth of the material, thereby affecting the performance of the positive electrode material capacity. Specifically, the primary sintered material obtained in step S2 is put into a high-speed mixer, and the primary sintered material is dispersed according to certain parameters to prevent the material from agglomerating and causing uneven subsequent calcination.

[0057] In some embodiments, the dispersion speed may be 500 r / min to 700 r / min, and the dispersion time may be 6 min to 10 min. Within the above parameter range, effective dispersion of the primary sintering material can be achieved.

[0058] Step S4, performing secondary sintering on the dispersed material to obtain a positive electrode material, wherein during the secondary sintering process, the Nb element and the B element enter into the lattice of the positive electrode material.

[0059] Specifically, the dispersed material continues to be sintered in the main temperature zone of the box furnace. The material crystallizes and forms nuclei during this process to achieve the purpose of doping. The secondary sintered product is screened to remove iron and packaged to obtain a lithium-rich manganese-based positive electrode material.

[0060] In some embodiments, the temperature of the secondary sintering may be 700°C to 950°C, further 800°C to 900°C, illustratively 700°C, 750°C, 800°C, 850°C, 860°C, 900°C or 950°C. Appropriate sintering temperature is particularly important for the grain growth of the positive electrode material. If the temperature of the secondary sintering is too low (lower than 700°C), the grain growth of the positive electrode material will be incomplete and the layered structure will be incomplete; if the temperature of the secondary sintering is too high (higher than 950°C), the primary particles of the positive electrode material will be larger and the internal resistance will be higher, which will hinder the performance of the capacity of the positive electrode material.

[0061] In some embodiments, the secondary sintering time may be 5 h to 10 h, further may be 6 h to 10 h, illustratively may be 5 h, 6 h, 7 h, 8 h, 9 h or 10 h, etc. Controlling the sintering time within the above range is conducive to the complete growth of grains and the improvement of crystallinity, which can ensure the complete formation of the layered structure of the positive electrode material, thereby optimizing the electrochemical performance of the positive electrode material.

[0062] Compared with the prior art, the method for preparing the positive electrode material provided in the embodiment of the present application has the following beneficial effects:

[0063] 1. By controlling the doping amount of Nb and B in the positive electrode material, the synergistic doping effect of Nb and B can be fully exerted. Too much or too little doping of both will lead to poor synergistic effect, causing a significant decrease in the rate performance and cycle performance of the positive electrode material. Control the doping amount and accurately adjust the proportion of each chemical component to optimize the physical and chemical properties of the target positive electrode material and ensure that the final positive electrode material meets the expected performance requirements.

[0064] 2. By optimizing the sintering parameters of the secondary sintering, it is beneficial to the crystallization nucleation of the positive electrode material, ensuring the integrity of the layered structure, adjusting the primary particles of the positive electrode material, effectively achieving the doping purpose, and improving the first coulombic efficiency and cycle performance of the positive electrode material.

[0065] 3. This preparation method is simple, efficient, and low-cost, which is conducive to the large-scale production of positive electrode materials and has excellent commercial prospects.

[0066] See also Figure 2 As shown, the embodiment of the present application also provides an electrochemical device (such as a battery), the electrochemical device 100 includes a positive electrode sheet 10, a negative electrode sheet 20, a separator 30 and an electrolyte 40, wherein the positive electrode sheet 10 includes a positive electrode active material, and the positive electrode active material is the positive electrode material as described above. The electrochemical device 100 prepared using the above-mentioned positive electrode material has the advantages of high capacity, high initial efficiency, long cycle life and excellent rate performance.

[0067] The above-mentioned positive electrode material and its preparation method and electrochemical device are further described below through specific examples.

[0068] Example 1

[0069] Step 1: Ni 0.36 Mn 0.64 (OH)2, Li2CO3, Nb2O5 and H3BO3 were mixed in a molar ratio of 1:1.33:0.1:0.15, first mixed at a low speed of 450 r / min for 8 min, and then mixed at a high speed of 700 r / min for 10 min to obtain a mixed material.

[0070] Step 2: Sinter the mixture once in an air atmosphere. The sintering parameters are as follows: first, heat from room temperature to 300°C at a heating rate of 3°C / min, keep warm for 5 hours, then continue to heat to 550°C, keep warm for 12 hours, and naturally cool to room temperature to obtain a primary sintered product.

[0071] Step 3: Disperse the primary sintered material in a high-speed mixer at a rotation speed of 600 r / min for 8 min to obtain dispersed material.

[0072] Step 4: Under air atmosphere, the dispersed materials are subjected to secondary sintering. The sintering parameters are as follows: the temperature is first increased from room temperature to a secondary sintering temperature of 860°C at a heating rate of 3°C / min, and the temperature is kept for 6 hours. After naturally cooling to room temperature, the materials are mixed, iron is removed, and packaged to obtain a lithium-rich manganese-based positive electrode material.

[0073] Example 2

[0074] The specific process of the preparation process is referred to Example 1, and the difference from Example 1 is that: in step 1, Ni 0.36 Mn 0.64 (OH)2, Li2CO3, Nb2O5 and H3BO3 are mixed in a molar ratio of 1:1.33:0.1:0.13. The preparation method of the remaining positive electrode materials is basically the same as that in Example 1, and will not be described in detail here.

[0075] Example 3

[0076] The specific process of the preparation process is referred to Example 1, and the difference from Example 1 is that in step 1, Ni 0.36 Mn 0.64 (OH)2, Li2CO3, Nb2O5 and H3BO3 are mixed in a molar ratio of 1:1.33:0.1:0.18. The preparation method of the remaining positive electrode materials is basically the same as that in Example 1, and will not be described in detail here.

[0077] Example 4

[0078] The specific process of the preparation process refers to Example 1, and the difference from Example 1 is that the temperature of the secondary sintering in step 4 is 920° C. The preparation method of the remaining positive electrode materials is basically the same as that in Example 1, and will not be described in detail here.

[0079] Example 5

[0080] The specific process of the preparation process refers to Example 1, and the difference from Example 1 is that the temperature of the secondary sintering in step 4 is 700° C. The preparation method of the remaining positive electrode materials is basically the same as that of Example 1, and will not be described in detail here.

[0081] Comparative Example 1

[0082] The specific process of the preparation process is referred to Example 1, and the difference from Example 1 is that: in step 1, Ni 0.36 Mn 0.64 (OH)2, Li2CO3 and Nb2O5 are mixed in a molar ratio of 1:1.33:0.1 without doping with B. The preparation method of the remaining positive electrode materials is basically the same as that in Example 1, and will not be described in detail here.

[0083] Comparative Example 2

[0084] The specific process of the preparation process is referred to Example 1, and the difference from Example 1 is that: in step 1, Ni 0.36 Mn 0.64 (OH)2, Li2CO3 and H3BO3 are mixed in a molar ratio of 1:1.33:0.15 without being doped with Nb. The preparation method of the remaining positive electrode materials is basically the same as that in Example 1, and will not be described in detail here.

[0085] Comparative Example 3

[0086] The specific process of the preparation process is referred to Example 1, and the difference from Example 1 is that: in step 1, Ni 0.36 Mn 0.64 (OH)2, Li2CO3, Nb2O5 and H2WO4 are mixed in a molar ratio of 1:1.33:0.1:0.1, i.e., Nb and W are co-doped. The preparation method of the remaining positive electrode materials is basically the same as that in Example 1, and will not be described in detail here.

[0087] Comparative Example 4

[0088] The specific process of the preparation process is referred to Example 1, and the difference from Example 1 is that: in step 1, Ni 0.36 Mn 0.64 (OH)2, Li2CO3, Nb2O5 and H2MoO4 are mixed in a molar ratio of 1:1.33:0.1:0.1, i.e., Nb and Mo are co-doped. The preparation method of the remaining positive electrode materials is basically the same as that in Example 1, and will not be described in detail here.

[0089] Comparative Example 5

[0090] The specific process of the preparation process refers to Example 1. The difference from Example 1 is that step 3 is not performed, that is, dispersion treatment is not performed. The preparation method of the remaining positive electrode materials is basically the same as that of Example 1, and will not be described in detail here.

[0091] Comparative Example 6

[0092] The specific process of the preparation process is referred to Example 1, and the difference from Example 1 is that: in step 1, Ni 0.36 Mn 0.64(OH)2, Li2CO3, Nb2O5 and H3BO3 are mixed in a molar ratio of 1:1.33:0.1:0.08. The preparation method of the remaining positive electrode materials is basically the same as that in Example 1, and will not be described in detail here.

[0093] Comparative Example 7

[0094] The specific process of the preparation process is referred to Example 1, and the difference from Example 1 is that: in step 1, Ni 0.36 Mn 0.64 (OH)2, Li2CO3, Nb2O5 and H3BO3 are mixed in a molar ratio of 1:1.33:0.1:0.22. The preparation method of the remaining positive electrode materials is basically the same as that in Example 1, and will not be described in detail here.

[0095] Comparative Example 8

[0096] The specific process of the preparation process refers to Example 1, and the difference from Example 1 is that the temperature of the secondary sintering in step 4 is 670° C. The preparation method of the remaining positive electrode materials is basically the same as that in Example 1, and will not be described in detail here.

[0097] 1. The main parameters for preparing the positive electrode materials of Examples 1-5 and Comparative Examples 1-8 are shown in Table 1.

[0098] Table 1

[0099]

[0100] 2. The positive electrode materials obtained in Examples 1-5 and Comparative Examples 1-8 were subjected to the following tests.

[0101] The positive electrode material prepared in Example 1 was subjected to an X-ray diffraction test, and the results were as follows: Figure 3 The positive electrode material prepared in Example 1 was observed and tested by scanning electron microscope, and the results were as follows Figure 4 shown.

[0102] The electrical performance test conditions are as follows: the prepared positive electrode material, conductive carbon and binder polyvinylidene fluoride are mixed evenly in a mass ratio of 8:1:1 to form a button battery. The LAND battery test system is used for constant current charge and discharge tests. During the test, the operating voltage range is 2.3V to 4.55V, the charge and discharge rates are 0.1C / 0.1C and 0.5C / 1C, respectively, and the CV cutoff current is 0.01C. The first coulomb efficiency at 0.1C, the first discharge capacity, and the capacity retention rate after 50 cycles at 45°C of the batteries prepared with the positive electrode materials obtained in Examples 1-5 and Comparative Examples 1-8 are measured. The results are shown in Table 2; Figure 5 It is a comparison diagram of the first charge and discharge curves at 0.1C of the corresponding batteries of Example 1 and Comparative Example 1; Figure 6It is a comparison chart of the 45°C cycle capacity retention rate curves of the corresponding batteries of Example 1 and Comparative Example 1.

[0103] Table 2

[0104]

[0105] The above results show that:

[0106] The battery prepared with the positive electrode materials of Examples 1-5 has excellent electrical performance, among which the battery prepared with the positive electrode material in Example 1 has the best effect, with an initial discharge capacity of 225.1 mAh / g, an initial efficiency of up to 93.7%, and a capacity retention rate of 98.23% after 50 cycles. This is due to the following examples of the present application: (1) The strong binding energy between Nb and O inhibits the release of lattice oxygen and delays phase transition; (2) The introduction of B acts on the additional electrons brought by Nb doping, adjusts the electronic structure inside the material, and alleviates the disadvantages brought by Nb doping (transition metal dissolution, loss of capacity); (3) More importantly, the appropriate B doping amount generates Li2O-B2O3 on the surface of the material during the sintering process. Li2O-B2O3 is a lithium ion conductor and accelerates the lithium ion transmission efficiency. And without an additional coating process, B2O3 as a coating layer prevents the corrosion of the positive electrode material by the electrolyte and improves the cycle performance.

[0107] Comparative Examples 1 and 2 are single-element doping, and there is no B element to form a coating layer to protect the positive electrode material, so the rate performance and cycle performance of the corresponding batteries are relatively poor.

[0108] Comparative Examples 3 and 4 are dual-doped with Nb-W and Nb-Mo, respectively, but the electrical performance of the corresponding batteries is not as good as that of Example 1 (Nb-B), which proves that the introduction of B has a synergistic effect with Nb, which is beneficial to improving the rate performance and cycle performance of the positive electrode material.

[0109] The difference between Comparative Example 5 and Example 1 is that no dispersion is performed, and the electrical performance of the corresponding battery also decreases. This is because there will be some agglomeration after the first sintering. If the second sintering is performed directly without dispersion, it will affect the grain growth of the material, thereby affecting the capacity.

[0110] The difference between Comparative Examples 6 and 7 and Example 1 is that the amount of B added is different, so the doping ratio of Nb to B is not in the range of 1: (1-2). The imbalance in the doping ratio of Nb to B will lead to poor synergy between B and Nb, and the rate performance and cycle performance of the corresponding battery will be greatly reduced.

[0111] The difference between Comparative Example 8 and Example 1 is that the secondary sintering temperature is different. The secondary sintering is carried out at 670° C., and the temperature is too low, resulting in insufficient crystallinity of the positive electrode material, too small primary particles, and serious reduction in electrical performance.

[0112] It can be seen that compared with comparative examples 1-8, the positive electrode materials obtained in embodiments 1-5 are doped with appropriate proportions of Nb and B elements, as well as good sintering and dispersion processes, and the corresponding battery performance and electrochemical test results of the prepared positive electrode materials are excellent, indicating that the positive electrode materials in the embodiments of the present application have improved initial efficiency and cycle performance while maintaining high capacity.

[0113] It is to be understood that the above embodiments are merely exemplary embodiments used to illustrate the principles of the present invention, but the present invention is not limited thereto. For those of ordinary skill in the art, various modifications and improvements can be made without departing from the spirit and essence of the present invention, and these modifications and improvements are also considered to be within the scope of protection of the present invention.

Claims

1. A positive electrode material, It is characterized in that The positive electrode material contains Nb element and B element in its crystal lattice, and the molar ratio of the doping amount of Nb element to the doping amount of B element is 1:(1-2).

2. The positive electrode material according to claim 1, It is characterized in that In terms of molar percentage, the doping amount of the Nb element is 10% to 15%, and the doping amount of the B element is 10% to 18%.

3. The positive electrode material according to claim 1, It is characterized in that The surface of the positive electrode material is formed with B 2 O 3 Coating layer.

4. The positive electrode material according to claim 3, It is characterized in that B 2 O 3 The coating layer contains Li 2 OB 2 O 3 Lithium ion conductor structure.

5. The positive electrode material according to claim 1, It is characterized in that The particle size D50 of the positive electrode material is 6.0 μm to 8.5 μm.

6. A method for preparing a positive electrode material, It is characterized in that include: Mixing a transition metal oxide precursor, a lithium source, a B source and a Nb source to obtain a mixed material, wherein the molar ratio of the Nb source to the B source is 1:(1-2); sintering the mixed material once to obtain a primary sintered material; Dispersing the primary sintered material to obtain a dispersed material; as well as The dispersed material is subjected to secondary sintering to obtain the positive electrode material, wherein during the secondary sintering process, the Nb element and the B element enter into the crystal lattice of the positive electrode material.

7. The method for preparing the positive electrode material according to claim 6, It is characterized in that The molar ratio of the transition metal oxide precursor, the lithium source, the Nb source and the B source is 1: (1.30-1.35): (0.1-0.15): (0.1-0.18).

8. The method for preparing the positive electrode material according to claim 6, It is characterized in that The primary sintering temperature is 400°C to 600°C, and the primary sintering time is 5h to 12h; The temperature of the secondary sintering is 700° C. to 950° C., and the time of the secondary sintering is 5 h to 10 h.

9. The method for preparing the positive electrode material according to claim 6, It is characterized in that In the step of mixing the transition metal oxide precursor, the lithium source, the B source and the Nb source, a step-by-step mixing method is adopted, and the step-by-step mixing includes a first step mixing and a second step mixing, the first step mixing speed is 300r / min to 500r / min, the first step mixing time is 5min to 10min, the second step mixing speed is 500r / min to 750r / min, and the second step mixing time is 5min to 15min; In the step of dispersing the primary sintered material, the dispersing speed is 500 r / min to 700 r / min, and the dispersing time is 6 min to 10 min; The molecular formula of the transition metal oxide precursor is Ni c Mn 1-c (OH) 2 , 0.3 <c<0.4。 10. An electrochemical device, It is characterized in that The electrochemical device comprises a positive electrode sheet, a negative electrode sheet, a separator and an electrolyte, wherein the positive electrode sheet comprises a positive electrode active material, and the positive electrode active material is a positive electrode material as described in any one of claims 1 to 5 or a positive electrode material prepared by the preparation method of a positive electrode material as described in any one of claims 6 to 9.

Citation Information

Cited By

  • Secondary-sphere positive electrode active material and preparation method therefor, positive electrode, and battery

    WO2026158479A1