A sodium ion battery positive electrode material and its preparation method and application

Through anion and cation co-doping and lithium cobalt phosphate coating technology, the air stability and structural stability of sodium ion layered oxide positive electrode materials are solved, the capacity and cycle life of the battery are improved, and the efficient sodium ion battery is achieved performance.

CN118763209BActive Publication Date: 2024-11-19JIANGSU ZENIO NEW ENERGY BATTERY TECH CO LTD
View PDF 0 Cites 0 Cited by

Patent Information

Application Number
CN202411234773.6
Authority / Receiving Office
CN · China
Patent Type
Patents(China)
Current Assignee / Owner
Filing Date
2024-09-04
Publication Date
2024-11-19
Estimated Expiration
2044-09-04

AI Technical Summary

Technical Problem

The sodium ion layered oxide positive electrode material has poor air stability and structural stability problems, resulting in reduced battery capacity and short cycle life.

Method used

Through the coating of anion-cationic co-doping (such as zinc, titanium, fluorine) and lithium cobalt phosphate, the structural stability and kinetic performance of the layered oxide material are improved, and the cell capacity and cycle life are enhanced.

Benefits of technology

It realizes the high capacity and long cycle life of the positive electrode material of sodium ion battery, with high initial discharge capacity and excellent cycle performance.

✦ Generated by Eureka AI based on patent content.

Smart Images

  • Figure CN118763209B_ABST
    Figure CN118763209B_ABST
Patent Text Reader

Abstract

The present invention discloses a sodium ion battery positive electrode material and a preparation method and application thereof. The positive electrode material comprises a layered oxide material and a lithium cobalt phosphate layer coated on the surface of the layered oxide material; the chemical formula of the layered oxide material is Na w Ni x Fe y Mn z Zn p Ti q O m F n , wherein 0.2≤x≤0.4, 0.2≤y≤0.33, 0.3≤z≤0.4, 0≤p≤0.1, 0<q≤0.01, 1.8≤m≤2.2, 0<n≤0.4, 0.6≤w<1.2, and x+y+z+p+q=1. The above-mentioned sodium ion battery material effectively improves the gram capacity and structural stability of the positive electrode material through the co-doping of anions and cations and the coating of lithium cobalt phosphate, so that the battery containing the sodium ion battery positive electrode material can have both high capacity and long cycle life.
Need to check novelty before this filing date? Find Prior Art

Description

Technical Field

[0001] The present invention relates to the field of battery technology, and in particular to a sodium ion battery positive electrode material and a preparation method and application thereof. Background Art

[0002] Sodium ion layered oxide Na x TMO2 (TM stands for transition metal) has attracted widespread attention due to its composition diversity and controllability. At present, sodium-based layered oxide cathode active materials generally have poor air stability, and the dissolution of transition metal ions during the charge and discharge cycle causes the material structure to deteriorate in stability, and are prone to side reactions with the electrolyte, consuming the electrolyte and cathode active materials, resulting in reduced battery capacity and other problems. As a result, the commercial application of sodium-based cathode materials has been slow.

[0003] At present, the main method to enhance the structural stability of materials is through element doping, which is mainly through solid phase sintering or precursor doping to add doping elements into the lattice; for air stability, the air stability of layered sodium ion oxides is mainly improved by reducing the sodium ratio, but the reduction of sodium ratio will reduce the initial sodium content of the positive electrode active material, affecting the gram capacity of the material; in addition, the layered oxide positive electrode active material is coated with polymer materials to improve the air stability and structural stability of the material, but the use of polymer materials alone for coating will affect the ionic conductivity of the material and reduce the material rate performance and capacity. Summary of the invention

[0004] To solve the above problems, the present invention provides a sodium ion battery positive electrode material and a preparation method and application thereof. Through the co-doping of anions and cations and the coating of lithium cobalt phosphate, the gram capacity, structural stability and kinetic performance of the layered oxide positive electrode active material are effectively improved, so that the battery containing the sodium ion battery positive electrode material can have both high capacity and long cycle life.

[0005] Specifically, the following technical solutions are provided:

[0006] The first aspect of the present invention provides a sodium ion battery positive electrode material, comprising a layered oxide material and a lithium cobalt phosphate layer coated on the surface of the layered oxide material; the chemical formula of the layered oxide material is Na w Ni x Fe y Mn z Zn p Ti q O m F n ;

[0007] Among them, 0.2≤x≤0.4, 0.2≤y≤0.33, 0.3≤z≤0.4, 0≤p≤0.1, 0<q≤0.01, 1.8≤m≤2.2, 0<n≤0.4, 0.6≤w<1.2, and x+y+z+p+q=1.

[0008] Furthermore, when 0.6≤w<0.8, the layered oxide material is a P2 phase layered oxide; when 0.8≤w<1.2, the layered oxide material is an O3 phase layered oxide.

[0009] Furthermore, 0≤p≤0.8, for example, 0, 0.1, 0.2, 0.3, 0.4, 0.5, 0.6, 0.7, 0.8, etc., and more preferably 0.4.

[0010] Furthermore, the particle size D50 of the layered oxide material is 3.5-8.8 μm, for example, 3.5 μm, 4 μm, 4.5 μm, 5 μm, 5.5 μm, 6 μm, 6.5 μm, 7 μm, 7.5 μm, 8 μm, 8.5 μm, etc., including but not limited to the particle size values ​​listed above.

[0011] Furthermore, the thickness of the lithium cobalt phosphate layer is 1-20 nm, for example, 1 nm, 2 nm, 3 nm, 4 nm, 5 nm, 6 nm, 7 nm, 8 nm, 9 nm, 10 nm, 11 nm, 12 nm, 13 nm, 14 nm, 15 nm, 16 nm, 17 nm, 18 nm, 19 nm, 20 nm, etc., including but not limited to the thickness values ​​listed above.

[0012] The second aspect of the present invention provides a method for preparing the positive electrode material for a sodium ion battery according to the first aspect, comprising the following steps:

[0013] S1: weighing a metal source and a fluorine source according to a preset molar ratio and dissolving them in water to obtain a uniformly mixed solution, and subjecting the mixed solution to spray pyrolysis to obtain a layered oxide material; the metal source comprises at least a sodium source, a nickel source, an iron source, a manganese source and a titanium source;

[0014] S2: The layered oxide material described in S1 is mixed with lithium cobalt phosphate according to a preset mass ratio, and then the uniformly mixed powder is placed in an inert atmosphere for calcination to obtain the sodium ion battery positive electrode material.

[0015] Further, in S1, the fluorine source is preferably sodium fluoride and / or ammonium fluoride; the sodium source can be selected from one or more of sodium chloride, sodium acetate, and sodium nitrate; the nickel source can be selected from one or more of nickel chloride, nickel acetate, and nickel nitrate; the iron source can be selected from one or more of ferric chloride, ferric acetate, and ferric nitrate; the manganese source can be selected from one or more of manganese chloride, manganese acetate, and manganese nitrate; the titanium source is selected from one or more of titanium tetrachloride, titanium oxalate, and titanium nitrate.

[0016] Furthermore, the metal source further comprises a zinc source; the zinc source is selected from one or more of zinc chloride, zinc acetate, and zinc nitrate.

[0017] Furthermore, in S1, preferably, each metal source is dissolved in water to obtain an aqueous solution of each metal salt, and a fluorine source is dissolved in water to obtain a fluorine solution, and the aqueous solutions of each metal salt and the fluorine solution are uniformly mixed at 50-80° C. to obtain the mixed solution.

[0018] Furthermore, the total concentration of metal ions in the mixed solution is preferably 2-5 mol / L, for example 2 mol / L, 2.5 mol / L, 3 mol / L, 3.5 mol / L, 4 mol / L, 4.5 mol / L, 5 mol / L, etc., including but not limited to the concentration values ​​listed above; more preferably, the ratio of the concentration of sodium ions to the total concentration of other metal ions in the mixed solution is (1-1.1):1, for example 1.02:1, 1.05:1, etc., and other metal ions refer to other metal ions in the mixed solution except sodium ions.

[0019] Furthermore, in S1, in the step of spray pyrolysis treatment: the mixed liquid is introduced into a spray pyrolysis furnace for spray pyrolysis; the temperature of the spray pyrolysis furnace is preferably 700-1200°C; the spray pyrolysis is carried out in a mixed atmosphere, the mixed atmosphere comprises oxygen and fuel gas; preferably, the volume ratio of oxygen to fuel gas in the mixed atmosphere is 1:(0.5-3), and the flow rate of the oxygen introduced into the spray pyrolysis furnace is 1-10 m 3 / h.

[0020] Furthermore, in S2, the mass ratio of the layered oxide material to lithium cobalt phosphate in the powder is preferably 1:(0.001-0.01), for example, 1:0.001, 1:0.002, 1:0.003, 1:0.004, 1:0.005, 1:0.006, 1:0.007, 1:0.008, 1:0.009, 1:0.01, etc., including but not limited to the mass ratios listed above.

[0021] Further, in S2, the mixing method is preferably ball milling; more preferably, the rotation speed of the ball mill is 200-800 r / min, and the ball milling time is 2-10 h.

[0022] Furthermore, in S2, the mixed environment humidity is ≤5%.

[0023] Furthermore, in S2, in the calcination step: the heating rate is 1-10°C / min, the calcination temperature is 600-800°C, and the calcination time is 6-15 h; preferably, the calcination is carried out under an inert atmosphere.

[0024] Furthermore, in S2, the preparation method further comprises a step of cooling the temperature at a cooling rate of 1-5°C / min after the calcination treatment.

[0025] The third aspect of the present invention further provides a positive electrode plate, comprising the sodium ion battery positive electrode material prepared by the preparation method described in the second aspect.

[0026] A fourth aspect of the present invention provides a sodium ion battery, comprising the positive electrode sheet described in the third aspect.

[0027] Compared with the prior art, the present invention has the following beneficial effects:

[0028] The present invention provides a sodium ion battery positive electrode material, which effectively improves the gram capacity, structural stability and kinetic performance of the layered oxide positive electrode active material through co-doping of anions and cations (zinc, titanium, fluorine) and coating with lithium cobalt phosphate, so that the battery containing the sodium ion battery positive electrode material can have both high capacity and long cycle life.

[0029] The present invention also provides a method for preparing the above-mentioned sodium ion battery positive electrode material. After the metal sources and fluorine sources are evenly mixed, the anion- and cation-doped primary particles are directly synthesized by a spray pyrolysis method. This not only reduces the first sintering process and reduces the processing cost, but also the prepared primary particles have controllable particle size and good uniformity, and are suitable for batch preparation. BRIEF DESCRIPTION OF THE DRAWINGS

[0030] Figure 1 This is the SEM image of the sodium ion battery positive electrode material prepared in Example 1. DETAILED DESCRIPTION

[0031] Unless otherwise defined, all technical and scientific terms used herein have the same meaning as commonly understood by those skilled in the art to which the present invention belongs. The terms used herein in the specification of the present invention are for the purpose of describing specific embodiments only and are not intended to limit the present invention. The term "and / or" used herein includes any and all combinations of one or more related listed items. The "include" or "comprising" described in the present invention means that in addition to the components described, other components may also be included or contained. The "include" or "comprising" described in the present invention may also be replaced by the closed "for" or "consisting of...".

[0032] As described in the background technology, sodium ion layered oxides have problems such as poor air stability and poor structural stability. Currently, the structural stability of layered oxides is enhanced mainly by element doping, the air stability of layered oxides is improved by reducing sodium ligands, or the air stability and structural stability of layered oxides are improved by coating with polymer materials. However, the above methods all affect the gram capacity or rate performance of the material to a certain extent, and cannot effectively improve its stability while maintaining high rate performance and high gram capacity.

[0033] To solve the above problems, the present invention provides a sodium ion battery positive electrode material in some embodiments, including a layered oxide material and a lithium cobalt phosphate layer coated on the surface of the layered oxide material; the chemical formula of the layered oxide material is Na w Ni x Fe y Mn z Zn p Ti q O m F n ;

[0034] Among them, 0.2≤x≤0.4, 0.2≤y≤0.33, 0.3≤z≤0.4, 0≤p≤0.1, 0<q≤0.01, 1.8≤m≤2.2, 0<n≤0.4, 0.6≤w<1.2, and x+y+z+p+q=1.

[0035] The present invention provides a novel sodium ion battery positive electrode material to solve the problems of poor air stability and poor structural stability during cyclic charge and discharge of sodium ion layered oxide materials, which is obtained by coating anion and cation co-doped layered oxide materials with lithium cobalt phosphate. The present invention improves the structural stability of the layered oxide by doping a certain amount of titanium to form a stable Ti-O octahedral structure with oxygen in the layered oxide, and at the same time introduces strongly electronegative fluorine to replace part of the oxygen, and further improves the structural stability of the layered oxide material through the strong bonding between Ti and F, and inhibits the dissolution of transition metal ions during the charge and discharge cycle. On the basis of co-doping of Ti and F, the gram capacity of the layered oxide material is further increased by doping an appropriate amount of Zn, thereby obtaining a layered oxide material with high gram capacity and good structural stability. Furthermore, lithium cobalt phosphate with good high-voltage stability is used to coat the anion-cation co-doped layered oxide material, which improves the structural stability of the layered oxide material under high pressure, improves the kinetics of ion transfer, and inhibits the occurrence of side reactions, thereby improving the interface stability of the positive electrode material. At the same time, the lithium cobalt phosphate coating layer introduces lithium ions, which can provide a portion of the capacity, thereby minimizing the effect of the coating layer on the gram capacity of the material. Under the synergistic effect of the above-mentioned anion-cation co-doping and lithium cobalt phosphate coating, a sodium ion battery positive electrode material with high gram capacity, good kinetic performance, and good structure and air stability is obtained.

[0036] In the present invention, when 0.6≤w<0.8, the layered oxide material is a P2 phase layered oxide; when 0.8≤w<1.2, the layered oxide material is an O3 phase layered oxide.

[0037] In the present invention, the doping amount of Zn will affect the gram capacity and structural stability of the above-mentioned Ti, F co-doped and lithium cobalt phosphate-coated layered oxide material. The gram capacity of the prepared positive electrode material shows a trend of first increasing, then decreasing, and then increasing again with the increase of the Zn doping amount, while the structural stability of the positive electrode material decreases significantly with the increase of the Zn doping amount. A positive electrode material with both high gram capacity and structural stability is obtained. It is preferred that the doping amount of Zn is controlled in the range of 0≤p≤0.8, for example, 0, 0.1, 0.2, 0.3, 0.4, 0.5, 0.6, 0.7, 0.8, etc., more preferably 0.4.

[0038] In the present invention, the particle size D50 of the layered oxide material is preferably 3.5-8.8 μm, for example, 3.5 μm, 4 μm, 4.5 μm, 5 μm, 5.5 μm, 6 μm, 6.5 μm, 7 μm, 7.5 μm, 8 μm, 8.5 μm, etc., including but not limited to the particle size values ​​listed above; the thickness of the lithium cobalt phosphate layer is preferably 1-20 nm, for example, 1 nm, 2 nm, 3 nm, 4 nm, 5 nm, 6 nm, 7 nm, 8nm, 9 nm, 10 nm, 11 nm, 12 nm, 13 nm, 14 nm, 15 nm, 16 nm, 17 nm, 18 nm, 19 nm, 20 nm, etc., including but not limited to the thickness values ​​listed above. The thickness (amount) of the lithium cobalt phosphate layer coated on the surface of the layered oxide material will affect the stability, kinetic properties and gram capacity of the material. The lithium cobalt phosphate layer should not be too thick or too thin. If the coating layer is too thin, the air stability of the material and the structural stability under high pressure cannot be effectively improved. However, it should not be too thick either. If the coating layer is too thick, the gram capacity of the prepared positive electrode material will be low, and impedance anomalies are likely to occur under full charge voltage. Therefore, preferably, the thickness of the lithium cobalt phosphate layer is controlled at about 1-20 nm.

[0039] The present invention also provides a method for preparing the above-mentioned sodium ion battery positive electrode material, comprising the following steps:

[0040] S1: weighing a metal source and a fluorine source according to a preset molar ratio and dissolving them in water to obtain a uniformly mixed solution, and subjecting the mixed solution to spray pyrolysis to obtain a layered oxide material; the metal source comprises at least a sodium source, a nickel source, an iron source, a manganese source and a titanium source;

[0041] S2: The layered oxide material described in S1 is mixed with lithium cobalt phosphate according to a preset mass ratio, and then the uniformly mixed powder is placed in an inert atmosphere for calcination to obtain the sodium ion battery positive electrode material.

[0042] In the present invention, the above-mentioned metal source and fluorine source are all water-soluble salts, including but not limited to the types listed below, for example: the fluorine source is sodium fluoride and / or ammonium fluoride; the sodium source can be selected from one or more of sodium chloride, sodium acetate, and sodium nitrate; the nickel source can be selected from one or more of nickel chloride, nickel acetate, and nickel nitrate; the iron source can be selected from one or more of ferric chloride, ferric acetate, and ferric nitrate; the manganese source can be selected from one or more of manganese chloride, manganese acetate, and manganese nitrate; the titanium source can be selected from one or more of titanium tetrachloride, titanium oxalate, and titanium nitrate.

[0043] In the present invention, the metal source further comprises a zinc source, wherein the zinc source can be selected from one or more of zinc chloride, zinc acetate and zinc nitrate.

[0044] In some preferred embodiments of the present invention, each metal source is first dissolved in water to obtain an aqueous solution of each metal salt, and a fluorine source is dissolved in water to obtain a fluorine solution. The aqueous solutions of each metal salt and the fluorine solution are uniformly mixed at 50-80° C. to obtain the above-mentioned mixed solution.

[0045] In the present invention, the total concentration of metal ions in the above-mentioned mixed solution is preferably 2-5 mol / L, for example, 2 mol / L, 2.5 mol / L, 3 mol / L, 3.5 mol / L, 4 mol / L, 4.5 mol / L, 5 mol / L, etc., including but not limited to the concentration values ​​listed above; more preferably, the ratio of the concentration of sodium ions in the mixed solution to the total concentration of other metal ions is (1-1.1):1, for example, 1.02:1, 1.05:1, etc., and other metal ions refer to other metal ions in the mixed solution except sodium ions.

[0046] In the present invention, in the step of spray pyrolysis treatment: the mixed liquid is introduced into a spray pyrolysis furnace, the furnace temperature is controlled at 700-1200 ° C, and spray pyrolysis is performed under a mixed atmosphere; wherein the mixed atmosphere contains oxygen and fuel gas, the volume ratio of oxygen to LNG fuel gas is preferably 1: (0.5-3), and the flow rate of oxygen introduced into the spray pyrolysis furnace is 1-10 m 3 / h. The present invention directly synthesizes anion- and cation-doped primary particles by a spray pyrolysis method, which can reduce a sintering process and reduce processing costs. The prepared primary particles have controllable particle size, good uniformity, and strong process controllability.

[0047] In the present invention, the mass ratio of the layered oxide material to the lithium cobalt phosphate in the powder of step S2 is preferably 1: (0.001-0.01), such as 1: 0.001, 1: 0.002, 1: 0.003, 1: 0.004, 1: 0.005, 1: 0.006, 1: 0.007, 1: 0.008, 1: 0.009, 1: 0.01, etc., including but not limited to the mass ratios listed above. The present invention controls the thickness of the lithium cobalt phosphate coating layer by controlling the feed ratio of the layered oxide material to the lithium cobalt phosphate, and preferably controls the feed ratio of the two in the range of 1: (0.001-0.01), and more preferably in the range of 1: (0.0025-0.0075).

[0048] In the present invention, the mixing in step S2 is performed under an environment with an ambient humidity of ≤5%. In some preferred embodiments, ball milling is used for the mixing process; more preferably, the rotation speed of the ball milling is 200-800 r / min, and the ball milling time is 2-10 h.

[0049] In the present invention, in the calcination step: the heating rate is preferably 1-10°C / min, the calcination temperature is preferably 600-800°C, the calcination time is preferably 6-15 h, and the calcination atmosphere is an inert atmosphere; more preferably, it also includes a step of cooling at a cooling rate of 1-5°C / min after the calcination.

[0050] The embodiments of the present invention also provide a positive electrode sheet comprising the above-mentioned sodium ion battery positive electrode material.

[0051] In some preferred embodiments, the positive electrode sheet comprises a current collector and a positive electrode active layer disposed on at least one side of the current collector along the thickness direction, wherein the positive electrode active layer comprises the above-mentioned sodium ion battery positive electrode material.

[0052] The embodiments of the present invention also provide a sodium ion battery comprising the above-mentioned positive electrode plate, which exhibits high initial discharge capacity and excellent cycle performance.

[0053] The present invention is further described below in conjunction with specific embodiments so that those skilled in the art can better understand the present invention and implement it, but the embodiments are not intended to limit the present invention. Example 1

[0054] This embodiment relates to the preparation of a positive electrode material for a sodium ion battery, and the specific operations are as follows:

[0055] According to the metal ion molar ratio of sodium: (nickel + iron + manganese + zinc + titanium) = 1.05:1, nickel: iron: manganese: zinc: titanium: fluorine = 0.32: 0.3: 0.33: 0.04: 0.01: 0.4, sodium chloride, nickel chloride, ferric chloride, manganese chloride, zinc chloride, titanium tetrachloride and ammonium fluoride were weighed, and then dissolved in water to prepare aqueous solutions of each source, which were stored in each raw liquid storage tank; a high-precision flow meter was used to transport the solutions in each raw liquid storage tank to a mixing tank for mixing to obtain a mixed solution, and the liquid inlet volume of each raw liquid was controlled to be 1 m 3 / h, using a jacketed water bath to heat, the temperature in the mixing tank is controlled at 70 °C, and the concentration of total metal ions in the mixed solution is 4 mol / L; then the mixed solution in the mixing tank is transported to the spray pyrolysis furnace by a centrifugal pump for spray pyrolysis, the furnace temperature is controlled at 1000 °C, the volume ratio of oxygen to LNG fuel gas is controlled at 2:1, and the oxygen flow rate is 1 m 3 / h, and the obtained layered oxide material NaNi is collected in the collecting hopper at the bottom of the spray pyrolysis furnace. 0.32 Fe 0.3 Mn 0.33 Zn 0.04 Ti 0.01 O 1.8 F 0.4 .

[0056] The layered oxide material and lithium cobalt phosphate prepared in step (1) were weighed according to a mass ratio of 1:0.005, and were placed in a ball mill at a rotation speed of 500 r / min for 5 h to make them uniformly mixed. The uniformly mixed powder was then placed in a tubular furnace at a heating rate of 3°C / min and sintered at 800°C for 5 h. After cooling (cooling rate of 4°C / min), a lithium cobalt phosphate-coated fluorine-titanium-zinc co-doped sodium ion battery positive electrode material was obtained. Example 2

[0057] This embodiment relates to the preparation of a sodium ion battery positive electrode material, which is different from Example 1 only in that the molar ratio of metal ions in the layered oxide material is: according to the metal ion molar ratio of sodium: (nickel + iron + manganese + zinc + titanium) = 1.05: 1, nickel: iron: manganese: zinc: titanium: fluorine = 0.31: 0.3: 0.33: 0.05: 0.01: 0.4, weigh sodium chloride, nickel chloride, iron chloride, manganese chloride, zinc chloride, titanium tetrachloride and ammonium fluoride. The rest of the operations are the same, and a sodium ion battery positive electrode material co-doped with fluorine, titanium and zinc coated with lithium cobalt phosphate is prepared. Example 3

[0058] This embodiment relates to the preparation of a sodium ion battery positive electrode material, and the only difference from Example 1 is that the molar ratio of metal ions in the layered oxide material is: according to the metal ion molar ratio of sodium: (nickel + iron + manganese + zinc + titanium) = 1.05: 1, nickel: iron: manganese: zinc: titanium: fluorine = 0.3: 0.3: 0.33: 0.06: 0.01: 0.4, weigh sodium chloride, nickel chloride, iron chloride, manganese chloride, zinc chloride, titanium tetrachloride and ammonium fluoride. The rest of the operations are the same, and a sodium ion battery positive electrode material co-doped with fluorine, titanium and zinc coated with lithium cobalt phosphate is prepared. Example 4

[0059] This embodiment relates to the preparation of a sodium ion battery positive electrode material, and the only difference from Example 1 is that the molar ratio of metal ions in the layered oxide material is: according to the metal ion molar ratio of sodium: (nickel + iron + manganese + zinc + titanium) = 1.05: 1, nickel: iron: manganese: zinc: titanium: fluorine = 0.29: 0.3: 0.33: 0.07: 0.01: 0.4, weigh sodium chloride, nickel chloride, iron chloride, manganese chloride, zinc chloride, titanium tetrachloride and ammonium fluoride. The rest of the operations are the same, and a sodium ion battery positive electrode material co-doped with fluorine, titanium and zinc coated with lithium cobalt phosphate is prepared. Example 5

[0060] This embodiment relates to the preparation of a sodium ion battery positive electrode material, which is different from Example 1 only in that the molar ratio of metal ions in the layered oxide material is as follows: according to the metal ion molar ratio of sodium: (nickel + iron + manganese + zinc + titanium) = 1.05: 1, nickel: iron: manganese: zinc: titanium: fluorine = 0.28: 0.3: 0.33: 0.08: 0.01: 0.4, sodium chloride, nickel chloride, iron chloride, manganese chloride, zinc chloride, titanium tetrachloride and ammonium fluoride are weighed. The rest of the operations are the same, and a sodium ion battery positive electrode material co-doped with fluorine, titanium and zinc coated with lithium cobalt phosphate is prepared. Example 6

[0061] This embodiment relates to the preparation of a positive electrode material for a sodium ion battery, and the only difference from Example 1 is that the molar ratio of metal ions in the layered oxide material is as follows: according to the molar ratio of metal ions sodium: (nickel + iron + manganese + zinc + titanium) = 1.05: 1, nickel: iron: manganese: zinc: titanium: fluorine = 0.27: 0.3: 0.33: 0.09: 0.01: 0.4, sodium chloride, nickel chloride, iron chloride, manganese chloride, zinc chloride, titanium tetrachloride and ammonium fluoride are weighed. The rest of the operations are the same, and a sodium ion battery positive electrode material co-doped with fluorine, titanium and zinc coated with lithium cobalt phosphate is prepared. Example 7

[0062] This embodiment relates to the preparation of a sodium ion battery positive electrode material, which differs from Example 1 only in that the molar ratio of metal ions in the layered oxide material is as follows: according to the metal ion molar ratio of sodium: (nickel + iron + manganese + zinc + titanium) = 1.05: 1, nickel: iron: manganese: zinc: titanium: fluorine = 0.26: 0.3: 0.33: 0.1: 0.01: 0.4, sodium chloride, nickel chloride, iron chloride, manganese chloride, zinc chloride, titanium tetrachloride and ammonium fluoride are weighed. The rest of the operations are the same, and a sodium ion battery positive electrode material co-doped with fluorine, titanium and zinc coated with lithium cobalt phosphate is prepared. Example 8

[0063] This embodiment relates to the preparation of a positive electrode material for a sodium ion battery. The only difference from Embodiment 1 is that the mass ratio of the layered oxide material to the lithium cobalt phosphate in step (2) is as follows: the layered oxide material and the lithium cobalt phosphate prepared in step (1) are weighed according to a mass ratio of 1:0.0025; the remaining operations are the same as those in Embodiment 1, and a fluorine-titanium-zinc co-doped sodium ion battery positive electrode material coated with lithium cobalt phosphate is prepared. Example 9

[0064] This embodiment relates to the preparation of a positive electrode material for a sodium ion battery. The only difference from Embodiment 1 is that the mass ratio of the layered oxide material to the lithium cobalt phosphate in step (2) is as follows: the layered oxide material and the lithium cobalt phosphate prepared in step (1) are weighed according to a mass ratio of 1:0.0075; the remaining operations are the same as those in Embodiment 1, and a fluorine-titanium-zinc co-doped sodium ion battery positive electrode material coated with lithium cobalt phosphate is prepared. Example 10

[0065] This embodiment relates to the preparation of a positive electrode material for a sodium ion battery. The only difference from Embodiment 1 is that the mass ratio of the layered oxide material to the lithium cobalt phosphate in step (2) is as follows: the layered oxide material and the lithium cobalt phosphate prepared in step (1) are weighed according to a mass ratio of 1:0.01; the remaining operations are the same as those in Embodiment 1, and a fluorine-titanium-zinc co-doped sodium ion battery positive electrode material coated with lithium cobalt phosphate is prepared. Embodiment 11

[0066] This embodiment relates to the preparation of a positive electrode material for a sodium ion battery, and the only difference from the embodiment 1 is that the layered oxide material prepared in step (1) does not contain Zn, specifically: according to the metal ion molar ratio of sodium: (nickel + iron + manganese + titanium) = 1.05: 1, nickel: iron: manganese: titanium: fluorine = 0.36: 0.3: 0.33: 0.01: 0.4, sodium chloride, nickel chloride, iron chloride, manganese chloride, zinc chloride, titanium tetrachloride and ammonium fluoride are weighed. The remaining operations are the same, and a sodium ion battery positive electrode material co-doped with fluorine and titanium coated with lithium cobalt phosphate is prepared. Comparative Example 1

[0067] This embodiment relates to a sodium ion battery positive electrode material NaNi 0.34 Fe 0.33 Mn 0.33 The preparation of O2 is as follows:

[0068] According to the metal ion molar ratio of sodium: (nickel + iron + manganese) = 1.05:1, nickel: iron: manganese = 0.34: 0.33: 0.33, weigh sodium chloride, nickel chloride, ferric chloride, and manganese chloride, and then dissolve them in water to prepare aqueous solutions of each source, which are stored in each raw liquid storage tank; a high-precision flow meter is used to transport the solutions in each raw liquid storage tank to a mixing tank for mixing to obtain a mixed solution, and the liquid inlet volume of each raw liquid is controlled to be 1 m 3 / h, using a jacketed water bath to heat, the temperature in the mixing tank is controlled at 70 °C, and the concentration of total metal ions in the mixed solution is 4 mol / L; then the mixed solution in the mixing tank is transported to the spray pyrolysis furnace by a centrifugal pump for spray pyrolysis, the furnace temperature is controlled at 1000 °C, the volume ratio of oxygen to LNG fuel gas is controlled at 2:1, and the oxygen flow rate is 1 m 3 / h, and the obtained layered oxide material NaNi is collected in the collecting hopper at the bottom of the spray pyrolysis furnace. 0.34 Fe 0.33 Mn 0.33 O2. Comparative Example 2

[0069] This comparative example relates to the preparation of a sodium ion battery positive electrode material, which differs from Example 9 only in that the layered oxide material prepared in step (1) does not contain Ti, specifically, according to the metal ion molar ratio of sodium: (nickel + iron + manganese + titanium) = 1.05: 1, nickel: iron: manganese: zinc: fluorine = 0.34: 0.3: 0.33: 0.03: 0.4, weigh sodium chloride, nickel chloride, iron chloride, manganese chloride, zinc chloride, titanium tetrachloride and ammonium fluoride. The remaining operations are the same, and a sodium ion battery positive electrode material co-doped with fluorine and zinc coated with lithium cobalt phosphate is prepared. Comparative Example 3

[0070] This comparative example relates to the preparation of a positive electrode material for a sodium ion battery, and the only difference from Example 1 is that the prepared layered oxide material is not subjected to a cobalt phosphate lithium coating treatment. Comparative Example 4

[0071] This comparative example relates to the preparation of a sodium ion battery positive electrode material, and the only difference from Example 9 is that an equal amount of lithium iron phosphate is used to replace lithium cobalt phosphate, and the other operations are the same, to prepare a lithium iron phosphate-coated fluorine-zinc co-doped sodium ion battery positive electrode material.

[0072] Application and performance testing

[0073] The sodium ion battery positive electrode materials prepared in the above examples and comparative examples are respectively used to construct sodium ion button batteries, and the specific operations are as follows:

[0074] Positive electrode sheet: Grind the positive electrode material, conductive carbon black and PVDF binder in a mass ratio of 8:1:1, add appropriate amount of NMP to make slurry, coat with aluminum foil, dry in a forced air drying oven at 80 °C for 1 h, dry in a vacuum drying oven at 120 °C for 12 h, and cut into 14 mm round positive electrode sheets;

[0075] Negative electrode: Sodium metal sheet with a diameter of 14 mm and a thickness of 0.15 mm;

[0076] Diaphragm: Whatman GF / F glass fiber with a diameter of 16 mm;

[0077] Electrolyte: The electrolyte is sodium perchlorate with a concentration of 0.1 mol / L, and the solvent is ethylene carbonate / dimethyl carbonate (volume ratio of 3:7);

[0078] The positive electrode sheet, separator, negative electrode sheet and electrolyte were assembled in a glove box filled with high-purity argon to obtain a CR2025 button cell.

[0079] The following electrochemical performance tests were performed on the CR2025 button cells constructed with different sodium ion battery cathode materials:

[0080] Initial discharge capacity and cycle performance test: In a constant temperature box, set the temperature to 25 °C, let stand for 10 minutes, use 1 C rate for constant current charging to 4.0 V, then charge at 4.0 V constant voltage to a cut-off current of 0.03 C, let stand for 15 minutes, use 1 C rate for constant current discharge, the discharge cut-off voltage is 2.0 V, and record the initial discharge capacity. Repeat the above charge and discharge operation for 500 cycles, record the discharge capacity of the 500th cycle, and the 500-cycle capacity retention rate = (discharge capacity of the 500th cycle / initial discharge capacity) × 100%.

[0081] The test results are shown in Table 1 below:

[0082] Table 1

[0083]

[0084] It can be seen from Table 1 that the sodium ion batteries prepared by using the Ti, F co-doped and lithium cobalt phosphate coated modified layered oxide materials as positive electrode materials prepared in Examples 1-11 have a high initial discharge capacity, wherein the Zn doping amount in the positive electrode materials prepared in Examples 1-5 and Examples 8-11 is 0-0.08, and the sodium ion batteries constructed by this type of positive electrode material have both high initial discharge capacity and excellent cycle performance.

[0085] It can be seen from Examples 1-7 and 11 that the gram capacity of the layered oxide material can be further increased by doping a certain amount of Zn in the above-mentioned Ti, F co-doped and lithium cobalt phosphate coated modified layered oxide material, but the increase in gram capacity shows a trend of first increasing, then decreasing, and then increasing again with the increase in the amount of Zn doping in the positive electrode material, and the cycle performance of the constructed sodium ion battery also increases first and then significantly decreases with the increase in the amount of Zn doping. Therefore, in order to construct a sodium ion battery with both high initial discharge capacity and excellent cycle performance, the amount of Zn ion doping in the positive electrode material needs to be controlled within a certain range, preferably 0.04-0.08. In addition, it can be seen from Examples 1 and 8-10 that the initial discharge capacity and cycle stability of the sodium ion battery first increase and then decrease with the increase in the amount of lithium cobalt phosphate coating.

[0086] It can be seen from Example 11 and Comparative Example 2 that the performance of the layered oxide material co-doped with Zn and F and coated with lithium cobalt phosphate is far inferior to that of the layered oxide material co-doped with Ti and F and coated with lithium cobalt phosphate, and the capacity retention rate of the sodium ion battery constructed with the positive electrode material prepared in Comparative Example 2 after 500 cycles is lower than that of the sodium ion battery prepared by the unmodified layered oxide.

[0087] It can be seen from Examples 1, 9 and Comparative Examples 3 and 4 that compared with the layered oxide material NaNi 0.32 Fe 0.3 Mn 0.33 Zn 0.04 Ti 0.01 O 1.8 F 0.4 , the layered oxide material coated with lithium cobalt phosphate or lithium iron phosphate can improve the cycle performance of the battery, among which the sodium ion battery constructed with a layered oxide material coated with an appropriate amount of lithium cobalt phosphate has better cycle performance. This is because lithium cobalt phosphate has better structural stability under high pressure than lithium iron phosphate, so that the layered oxide coated by it can better maintain structural stability under high voltage, thereby improving the cycle life of the sodium ion battery. However, the sodium ion battery constructed with the layered oxide material coated with lithium iron phosphate (Comparative Example 4) as the positive electrode active material will reduce the initial discharge capacity of the battery, while the initial discharge capacity of the sodium ion battery constructed with the layered oxide material coated with lithium cobalt phosphate (Example 9) as the positive electrode active material is not significantly reduced, and when the mass ratio of lithium cobalt phosphate to the layered oxide material is in the range of 0.0025-0.0075, the initial discharge capacity of the constructed sodium ion battery is improved.

[0088] The above-described embodiments are only preferred embodiments for fully illustrating the present invention, and the protection scope of the present invention is not limited thereto. Equivalent substitutions or changes made by those skilled in the art based on the present invention are within the protection scope of the present invention. The protection scope of the present invention shall be subject to the claims.

Claims

1. A sodium ion battery positive electrode material, characterized in that: It includes a layered oxide material and a lithium cobalt phosphate layer coated on the surface of the layered oxide material; The chemical formula of the layered oxide material is Na w Ni x Fe y Mn z Zn p Ti q O m F n ; Among them, 0.2≤x≤0.4, 0.2≤y≤0.33, 0.3≤z≤0.4, 0≤p≤0.1, 0<q≤0.01, 1.8≤m≤2.2, 0<n≤0.4, 0.6≤w<1.2, and x+y+z+p+q=1.

2. The sodium ion battery positive electrode material according to claim 1, characterized in that The particle size D50 of the layered oxide material is 3.5-8.8 μm; The thickness of the lithium cobalt phosphate layer is 1-20 nm.

3. A method for preparing a positive electrode material for a sodium ion battery according to claim 1 or 2, characterized in that: The following steps are involved: S1: weighing a metal source and a fluorine source according to a preset molar ratio and dissolving them in water to obtain a uniformly mixed solution, and subjecting the mixed solution to spray pyrolysis to obtain a layered oxide material; the metal source comprises at least a sodium source, a nickel source, an iron source, a manganese source and a titanium source; S2: The layered oxide material described in S1 is mixed with lithium cobalt phosphate according to a preset mass ratio, and then the uniformly mixed powder is placed in an inert atmosphere for calcination to obtain the sodium ion battery positive electrode material.

4. The preparation method according to claim 3, characterized in that: In S1, the fluorine source is sodium fluoride and / or ammonium fluoride; the sodium source is selected from one or more of sodium chloride, sodium acetate, and sodium nitrate; the nickel source is selected from one or more of nickel chloride, nickel acetate, and nickel nitrate; the iron source is selected from one or more of ferric chloride, ferric acetate, and ferric nitrate; the manganese source is selected from one or more of manganese chloride, manganese acetate, and manganese nitrate; the titanium source is selected from one or more of titanium tetrachloride, titanium oxalate, and titanium nitrate; The metal source further comprises a zinc source; the zinc source is selected from one or more of zinc chloride, zinc acetate and zinc nitrate.

5. The preparation method according to claim 3 or 4, characterized in that: The total concentration of metal ions in the mixed solution is 2-5 mol / L; The ratio of the concentration of sodium ions in the mixed solution to the total concentration of other metal ions is (1-1.1):

1.

6. The preparation method according to claim 3, characterized in that: In S1, in the step of spray pyrolysis treatment: the mixed liquid is introduced into a spray pyrolysis furnace for spray pyrolysis; the temperature of the spray pyrolysis furnace is 700-1200°C; the spray pyrolysis is carried out in a mixed atmosphere, and the mixed atmosphere contains oxygen and fuel gas; The volume ratio of oxygen to fuel gas in the mixed atmosphere is 1:(0.5-3), and the flow rate of oxygen introduced into the spray pyrolysis furnace is 1-10 m 3 / h.

7. The preparation method according to claim 3, characterized in that: In S2, the mass ratio of the layered oxide material to lithium cobalt phosphate in the powder is 1:(0.001-0.01).

8. The preparation method according to claim 3, characterized in that: In S2, the mixing method is ball milling; the rotation speed of the ball mill is 200-800 r / min, and the ball milling time is 2-10 h; In the calcination step: the heating rate is 1-10 °C / min, the calcination temperature is 600-800 °C, and the calcination time is 6-15 h; The preparation method further comprises a step of cooling the temperature at a cooling rate of 1-5°C / min after the calcination treatment.

9. A positive electrode sheet, characterized in that: The invention comprises the sodium ion battery positive electrode material according to claim 1 or 2, or the sodium ion battery positive electrode material prepared by the preparation method according to any one of claims 3 to 8.

10. A sodium ion battery, characterized in that: Including the positive electrode sheet as described in claim 9.