Asymmetric porous membrane for all-vanadium liquid flow battery and preparation method thereof

Through the grafting and cross-linking modification technology of asymmetric porous membranes, the problems of high cost of perfluorosulfonic acid membrane and vanadium ion permeability are solved, and the porous membrane with low cost, high resistance vanadium and high proton transmission are achieved, which improves the Coulomb and energy efficiency of all vanadium flow batteries.

CN118767697BActive Publication Date: 2024-11-19HANGZHOU DEHAI AIKE ENERGY TECH CO LTD
View PDF 0 Cites 0 Cited by

Patent Information

Application Number
CN202411253393.7
Authority / Receiving Office
CN · China
Patent Type
Patents(China)
Current Assignee / Owner
Filing Date
2024-09-09
Publication Date
2024-11-19
Estimated Expiration
2044-09-09

AI Technical Summary

Technical Problem

The existing perfluorosulfonic acid films are costly to be used in all vanadium flow batteries and have a serious permeability of vanadium ion, which affects the performance of the battery. The proton transfer rate of common porous membranes decreases when increasing the vanadium resistance rate, making it difficult to achieve low-cost, high-resistance vanadium resistance. And a porous membrane with high proton transport capability.

Method used

The asymmetric porous membrane preparation method is used to modify the membrane through grafting and cross-linking reactions to form an asymmetric porous membrane. The permeability of vanadium ions is reduced by the principle of charge repulsion and heterogeneous absorption, and the permeability of vanadium ions is regulated by the principle of pore size screening. Proton transmission efficiency.

Benefits of technology

A porous membrane with low cost, high resistance vanadium and high proton transmission capability is realized, which improves the Coulomb efficiency and energy efficiency of the battery, balances ion selectivity and conductivity, and improves the overall performance of the battery.

✦ Generated by Eureka AI based on patent content.

Smart Images

  • Figure CN118767697B_ABST
    Figure CN118767697B_ABST
Patent Text Reader

Abstract

The present invention relates to the technical field of all-vanadium liquid flow battery diaphragm, and discloses a method for preparing an asymmetric porous membrane for all-vanadium liquid flow battery, comprising the following steps: preparing a porous base membrane by phase separation of a high molecular polymer with a porogen added, and hydroxylating the porous base membrane by an activator; grafting and crosslinking one side of the porous base membrane with olefin chloride and olefin sulfonic acid to make the membrane surface negatively charged; grafting and modifying the other side of the porous base membrane with halogen imidazole to make the membrane surface positively charged. The porous membrane for all-vanadium liquid flow battery prepared by the present invention has asymmetry of surface charge, which can improve the vanadium resistance rate of the porous membrane and improve the coulomb efficiency of the battery; different modification methods on both sides of the porous membrane can regulate the pore size of the porous membrane, which can increase the proton transmission efficiency while improving the vanadium resistance rate, and improve the voltage efficiency and energy efficiency of the battery.
Need to check novelty before this filing date? Find Prior Art

Description

Technical Field

[0001] The invention belongs to the technical field of all-vanadium liquid flow battery diaphragms, and in particular relates to a method for preparing an asymmetric porous membrane for an all-vanadium liquid flow battery. Background Art

[0002] As the core component of all-vanadium flow battery technology, the ion exchange membrane is mainly used to prevent the mutual penetration of positive and negative electrolytes, block the passage of vanadium ions, and transfer protons. The diaphragm used in the current all-vanadium flow battery technology is mainly perfluorosulfonic acid membrane, which has the disadvantages of high cost and severe vanadium ion permeability, which seriously affects the further development of all-vanadium flow batteries.

[0003] Considering that porous membranes can simultaneously screen vanadium ions through the Donan effect and the pore size screening effect, which can reduce the permeability of vanadium ions, porous membranes are expected to replace perfluorosulfonic acid membranes. Although the cost is reduced, the pore size of common porous membranes is relatively large and the charges on both sides of the membrane are consistent, which will increase the vanadium resistance rate while also causing a decrease in the proton transmission rate. Therefore, the development of a low-cost porous membrane with high vanadium resistance and high proton transmission capacity and its preparation method has become an urgent problem to be solved. Summary of the invention

[0004] In view of the above-mentioned deficiencies in the prior art, the present invention provides a method for preparing an asymmetric porous membrane for an all-vanadium liquid flow battery.

[0005] The present invention specifically adopts the following technical solutions:

[0006] A method for preparing an asymmetric porous membrane for an all-vanadium liquid flow battery is carried out according to the following steps:

[0007] S1. Add 4-6 parts by weight of a high molecular weight polymer and 2-3 parts by weight of a porogen to 11-14 parts by weight of a solvent, heat and stir, and after complete dissolution, vacuum degassing to obtain a casting solution; apply the casting solution on a clean glass plate, and then soak it in deionized water to obtain a base film; soak the base film in an activator solution at a temperature of 30-50° C. for 0.5-3 h to obtain an activated base film;

[0008] S2, dissolving olefin chloride substances in an organic solution to prepare a grafting monomer solution; dissolving olefin sulfonic acid substances and catalysts in deionized water to prepare a crosslinking monomer solution; coating the grafting monomer solution on one side of the activated base film in S1 to carry out a grafting reaction, removing the liquid on the membrane surface after the reaction is completed, and drying naturally, coating the crosslinking monomer solution on the same side, carrying out a crosslinking reaction under the action of a catalyst, and removing the residual liquid on the membrane surface after the reaction is completed; heat-treating the membrane to complete the modification of one side of the membrane surface to obtain a single-sided negatively charged membrane;

[0009] S3, dissolving the halogen imidazole substance in an organic solvent to prepare a halogen imidazole substance solution; pouring the halogen imidazole substance solution onto the other side surface of the activated base membrane coated in S1 to react, removing the surface liquid after the reaction is completed, and heat-treating the membrane to obtain an asymmetric porous membrane.

[0010] Preferably, in step S1, the high molecular polymer is one of polyethersulfone (PES), polysulfone (PSU), polyvinylidene fluoride (PVDF), and polyacrylonitrile (PAN); the porogen is one of polyvinylpyrrolidone (PVP), polyethylene glycol (PEG), glycerol, and water; the solvent is one of N,N-dimethylacetamide (DMAc), N,N-dimethylformamide (DMF), N-methylpyrrolidone (NMP), and triethyl phosphate (TEP);

[0011] Preferably, the activator solution in step S1 is one of potassium persulfate solution, ammonium persulfate solution, potassium permanganate solution and potassium hydroxide solution, with a mass fraction of 0.5% to 1.5%.

[0012] Preferably, in step S2, the olefin chloride substance is one of crotonoyl chloride, propylene chloride, 4-pentenoyl chloride, but-3-enoyl chloride, 1,4-phenylenedipropylene chloride, 3-N,N-dimethylaminomethylpropylene chloride, and 3-ethoxypropylene chloride; the organic solvent is one of n-hexane, toluene, and cyclohexane; and the mass concentration of the olefin chloride substance in the grafting monomer solution is 1% to 9%.

[0013] Preferably, in step S2, the olefin sulfonic acid substance is one or more of sodium allyl sulfonate, disodium 4,4'-diisothiocyanato-2,2'-styrene sulfonate, allyl vinyl sulfonic acid, and sodium methacrylate sulfonate; the mass concentration of the olefin sulfonic acid substance in the cross-linking monomer solution is 1% to 7%; the catalyst is one of potassium persulfate and ammonium persulfate, and the mass concentration of the catalyst in the cross-linking monomer solution is 0.1% to 2%.

[0014] Preferably, in step S2, the grafting reaction time is 10 to 60 min; the cross-linking reaction time is 60 to 240 min; the heat treatment temperature is 40 to 80° C., and the heat treatment time is 5 to 10 min.

[0015] Preferably, the halogen imidazole substance in step S3 is one of 4-chloroimidazole, 4,5-dichloroimidazole, 2-bromo-4,5-dichloroimidazole, 6-bromoimidazo[1,2-A]pyridine-3-carboxamide, 7-bromoimidazo[2,1-F][1,2,4]triazine-4-amine, 4-bromoimidazole, 2,4-dibromoimidazole, 2,4,5-tribromoimidazole, and 4-(6-bromoimidazo[1,2-a]pyridin-3-yl)pyrimidine-2-amine; the organic solvent is one of dichloromethane, chloroform, and dimethyl sulfoxide; and the mass concentration of the halogen imidazole substance in the halogen imidazole substance solution is 1% to 11%.

[0016] Preferably, in step S3, the reaction time is 30-120 min; the heat treatment temperature is 40-80° C., and the heat treatment time is 5-10 min.

[0017] An asymmetric porous membrane for all-vanadium liquid flow battery is prepared by the above preparation method.

[0018] Compared with the prior art, the present invention has the following beneficial effects:

[0019] 1. The present invention modifies the porous membrane by a grafting method. The charges on both sides of the modified porous membrane are asymmetric. Based on the principle that like charges repel each other and opposite charges attract each other, the permeability of vanadium ions is reduced and the coulombic efficiency of the battery is improved.

[0020] 2. The present invention modifies the membrane surface by a cross-linking method. The cross-linking of the membrane surface can regulate the pore size of the membrane surface. Through the pore size screening principle, it can prevent the transmembrane transfer of vanadium ions, improve the transmission efficiency of protons, and improve the energy efficiency of the battery. BRIEF DESCRIPTION OF THE DRAWINGS

[0021] Figure 1 It is a schematic diagram of a method for preparing an asymmetric porous membrane for all-vanadium liquid flow battery of the present invention;

[0022] Figure 2 It is a Zeta potential curve diagram of both sides of the asymmetric porous membrane prepared in Example 1. DETAILED DESCRIPTION

[0023] In order to make the purpose, technical scheme and advantages of the present invention clearer, the present invention is further described in detail below through embodiments. The specific embodiments described herein are only used to explain the present invention and are not intended to limit the scope of the present invention. In addition, in the following description, the description of known structures and technologies is omitted to avoid unnecessary confusion of the concept of the present invention.

[0024] A method for preparing an asymmetric porous membrane for an all-vanadium liquid flow battery comprises the following steps:

[0025] S1. Add 4-6 parts by weight of a high molecular polymer and 2-3 parts by weight of a porogen to 11-14 parts by weight of a solvent, heat and stir, and after complete dissolution, vacuum degassing to obtain a casting solution; apply the casting solution on a clean glass plate, and then soak it in deionized water to obtain a base film; soak the base film in an activator solution with a concentration of 0.5%-1.5%, at a temperature of 30-50° C. for 0.5-3 h to obtain an activated base film;

[0026] S2, dissolving olefin chloride substances in an organic solution to prepare a grafting monomer solution with a mass concentration of 1% to 9%; dissolving olefin sulfonic acid substances and catalysts in deionized water to prepare a cross-linking monomer solution with a mass concentration of 1% to 7%, wherein the mass concentration of the catalyst is 0.1% to 2%; coating the grafting monomer solution on one side of the activated base membrane in S1 to carry out a grafting reaction, the reaction ends after 10min to 60min, the liquid on the membrane surface is removed, and the membrane is naturally dried, and the cross-linking monomer solution is coated on the same side, and a cross-linking reaction is carried out under the action of a catalyst, the reaction ends after 60min to 240min, and the residual liquid on the membrane surface is removed; heat-treating the membrane at 40°C to 80°C, and completing the modification of the surface of one side of the membrane after 5min to 10min to obtain a single-sided negatively charged membrane;

[0027] S3. Dissolve the halogen imidazole substance in an organic solvent to prepare a halogen imidazole solution with a mass concentration of 1% to 11%; pour the halogen imidazole solution onto the other surface of the activated base membrane coated in S1 to react. After 30 minutes to 120 minutes, the reaction is completed and the surface liquid is removed. The membrane is heat-treated at 40°C to 80°C to obtain an asymmetric porous membrane after 5 minutes to 10 minutes.

[0028] Embodiment 1:

[0029] S1: Add 4 parts by mass of high molecular polymer PAN and 2 parts by mass of water to 11 parts by mass of DMAc, heat and stir, and after complete dissolution, vacuum degassing to obtain a uniform and bubble-free casting solution; use a scraper to scrape the degassing casting solution on a clean glass plate, and quickly immerse the scraped glass plate in deionized water to complete the preparation of the base film; prepare a potassium persulfate solution with a mass concentration of 0.5%, hydroxylate the base film at 30°C, and complete the preparation of the activated base film after 3 hours;

[0030] S2: dissolving crotonyl chloride in n-hexane to prepare a grafting monomer solution with a mass concentration of 1%;

[0031] Sodium allyl sulfonate and catalyst potassium persulfate are dissolved in deionized water to prepare a cross-linking monomer solution with a mass concentration of 7%, wherein the mass concentration of the catalyst is 0.1%; the grafting monomer solution is coated on the surface of one side of the activated base membrane in S1 to carry out a grafting reaction, the reaction ends after 60 minutes, the liquid on the surface of the membrane is removed, and the membrane is naturally dried, and the cross-linking monomer solution is coated on the same side, and a cross-linking reaction is carried out under the action of the catalyst, the reaction ends after 240 minutes, and the residual liquid on the surface of the membrane is removed; the membrane is heat-treated at 80°C, and the surface modification of one side of the membrane is completed after 5 minutes to obtain a single-sided negatively charged membrane;

[0032] S3: dissolving 4-chloroimidazole in dichloromethane to prepare a halogen imidazole solution with a mass concentration of 1%; pouring the halogen imidazole solution onto the other side of the activated base film coated in S1 to react, removing the surface liquid after the reaction is completed after 120 minutes, and heat-treating the film at 40°C to obtain an asymmetric porous membrane after 10 minutes;

[0033] The asymmetric porous membranes prepared in different steps of this example were subjected to Zeta potential tests. Figure 2 In the middle, a is the Zeta potential of a single-sided negatively charged membrane. It can be seen that under acidic conditions, the membrane exhibits negative charge; Figure 2 b is the Zeta potential of a single-sided positively charged membrane, and it can be seen that under acidic conditions, the membrane exhibits positive charge. Therefore, it is shown that the preparation method of this embodiment successfully prepares a porous membrane with asymmetric charges on both sides.

[0034] Embodiment 2:

[0035] S1: Add 6 parts by mass of high molecular polymer PVDF and 3 parts by mass of glycerol to 14 parts by mass of DMF, heat and stir, and after complete dissolution, vacuum degassing to obtain a uniform and bubble-free casting liquid; use a scraper to scrape the degassing casting liquid on a clean glass plate, and quickly immerse the scraped glass plate in deionized water to complete the preparation of the base film; prepare a potassium hydroxide solution with a mass concentration of 1.5%, hydroxylate the base film at 50°C, and after 0.5h, complete the preparation of the activated base film;

[0036] S2: dissolving acryloyl chloride in toluene to prepare a grafting monomer solution with a mass concentration of 9%;

[0037] Disodium 4,4'-diisothiocyanato-2,2'-styrene sulfonate and catalyst ammonium persulfate are dissolved in deionized water to prepare a cross-linking monomer solution with a mass concentration of 1%, wherein the mass concentration of the catalyst is 2%; the grafting monomer solution is coated on one side of the activated base membrane in S1 to carry out a grafting reaction, and the reaction ends after 10 minutes. The liquid on the membrane surface is removed and the membrane is naturally dried, and the cross-linking monomer solution is coated on the same side to carry out a cross-linking reaction under the action of the catalyst. The reaction ends after 60 minutes and the residual liquid on the membrane surface is removed; the membrane is heat-treated at 40°C, and the surface modification of one side of the membrane is completed after 10 minutes to obtain a single-sided negatively charged membrane;

[0038] S3: Dissolve 4,5-dichloroimidazole in chloroform to prepare a halogen imidazole solution with a mass concentration of 11%; pour the halogen imidazole solution onto the other side of the activated base membrane coated in S1 to react. After 30 minutes, the reaction is completed and the surface liquid is removed. The membrane is heat-treated at 80°C to obtain an asymmetric porous membrane after 5 minutes.

[0039] Embodiment 3:

[0040] S1: Add 5 parts by mass of high molecular weight polymer PES and 2.5 parts by mass of PVP to 13 parts by mass of NMP, heat and stir, and after complete dissolution, vacuum degassing to obtain a uniform and bubble-free casting solution; use a scraper to scrape the degassing casting solution on a clean glass plate, and quickly immerse the scraped glass plate in deionized water to complete the preparation of the base film; prepare a potassium permanganate solution with a mass concentration of 1%, hydroxylate the base film at 40°C, and after 1.75 hours, complete the preparation of the activated base film;

[0041] S2: dissolving 4-pentenoyl chloride in cyclohexane to prepare a grafting monomer solution with a mass concentration of 5%;

[0042] Allyl vinyl sulfonic acid and catalyst potassium persulfate are dissolved in deionized water to prepare a cross-linking monomer solution with a mass concentration of 4%, wherein the mass concentration of the catalyst is 1.05%; the grafting monomer solution is coated on one side of the surface of the activated base membrane in S1 to carry out a grafting reaction, the reaction ends after 35 minutes, the liquid on the surface of the membrane is removed, and the membrane is naturally dried, and the cross-linking monomer solution is coated on the same side, and a cross-linking reaction is carried out under the action of the catalyst, the reaction ends after 150 minutes, and the residual liquid on the surface of the membrane is removed; the membrane is heat-treated at 60°C, and the surface modification of one side of the membrane is completed after 7.5 minutes to obtain a single-sided negatively charged membrane;

[0043] S3: Dissolve 2-bromo-4,5-dichloroimidazole in dimethyl sulfoxide to prepare a halogen imidazole solution with a mass concentration of 6%; pour the halogen imidazole solution onto the other side of the activated base membrane coated in S1 to react. After 75 minutes, the reaction is completed and the surface liquid is removed. The membrane is heat-treated at 60°C to obtain an asymmetric porous membrane after 7.5 minutes.

[0044] Embodiment 4:

[0045] S1: 4 parts by weight of high molecular weight polymer PSU and 2 parts by weight of PEG are added to 11 parts by weight of TEP, heated and stirred, and after being completely dissolved, vacuum degassing is performed to obtain a uniform and bubble-free casting solution; the degassing casting solution is scraped on a clean glass plate by a scraping knife, and the scraped glass plate is quickly immersed in deionized water to complete the preparation of the base film; an ammonium persulfate solution with a mass concentration of 1.5% is prepared, and the base film is hydroxylated and modified at 40°C. After 1.75 hours, the preparation of the activated base film is completed;

[0046] S2: dissolving but-3-enoyl chloride in cyclohexane to prepare a grafting monomer solution with a mass concentration of 1%;

[0047] Sodium methyl methacrylate sulfonate and catalyst ammonium persulfate are dissolved in deionized water to prepare a cross-linking monomer solution with a mass concentration of 7%, wherein the mass concentration of the catalyst is 0.8%; the grafting monomer solution is coated on one side of the surface of the activated base membrane in S1 to carry out a grafting reaction, the reaction ends after 60 minutes, the liquid on the surface of the membrane is removed, and the membrane is naturally dried, and the cross-linking monomer solution is coated on the same side, and a cross-linking reaction is carried out under the action of the catalyst, the reaction ends after 100 minutes, and the residual liquid on the surface of the membrane is removed; the membrane is heat-treated at 80°C, and the surface modification of one side of the membrane is completed after 5 minutes to obtain a single-sided negatively charged membrane;

[0048] S3: Dissolve 6-bromoimidazole [1,2-A] pyridine-3-carboxamide in dichloromethane to prepare a halogen imidazole solution with a mass concentration of 1%; pour the halogen imidazole solution onto the other side of the activated base membrane coated in S1 to react. After 120 minutes, the reaction is completed and the surface liquid is removed. The membrane is heat-treated at 40°C to obtain an asymmetric porous membrane after 10 minutes.

[0049] Embodiment 5:

[0050] S1: 6 parts by mass of high molecular weight polymer PAN and 3 parts by mass of water are added to 14 parts by mass of DMAc, heated and stirred, and after complete dissolution, vacuum degassing is performed to obtain a uniform and bubble-free casting solution; the degassing casting solution is scraped on a clean glass plate by a scraping knife, and the scraped glass plate is quickly immersed in deionized water to complete the preparation of the base film; a potassium persulfate solution with a mass concentration of 0.5% is prepared, and the base film is hydroxylated and modified at 30°C. After 3 hours, the preparation of the activated base film is completed;

[0051] S2: Dissolve 1,4-phenylenediacryl chloride in n-hexane to prepare a grafting monomer solution with a mass concentration of 9%; dissolve sodium allyl sulfonate and catalyst potassium persulfate in deionized water to prepare a cross-linking monomer solution with a mass concentration of 1%, wherein the mass concentration of the catalyst is 0.1%; apply the grafting monomer solution to one side of the activated base membrane in S1 to carry out a grafting reaction, the reaction ends after 10 minutes, remove the liquid on the membrane surface, dry it naturally, apply the cross-linking monomer solution on the same side, carry out a cross-linking reaction under the action of the catalyst, the reaction ends after 240 minutes, and remove the residual liquid on the membrane surface; heat treat the membrane at 40°C, and complete the modification of one side of the membrane surface after 10 minutes to obtain a single-sided negatively charged membrane;

[0052] S3: Dissolve 7-bromoimidazole [2,1-F] [1,2,4] triazine-4-amine in chloroform to prepare a halogen imidazole solution with a mass concentration of 11%; pour the halogen imidazole solution onto the other side of the activated base membrane coated in S1 to react. After 30 minutes, the reaction is completed and the surface liquid is removed. The membrane is heat-treated at 80°C to obtain an asymmetric porous membrane after 5 minutes.

[0053] Embodiment 6:

[0054] S1: 5 parts by mass of high molecular weight polymer PVDF and 2.5 parts by mass of glycerol are added to 13 parts by mass of DMF, heated and stirred, and after being completely dissolved, vacuum degassing is performed to obtain a uniform and bubble-free casting liquid; the degassing casting liquid is scraped on a clean glass plate by a scraping knife, and the scraped glass plate is quickly immersed in deionized water to complete the preparation of the base film; a potassium hydroxide solution with a mass concentration of 1.5% is prepared, and the base film is hydroxylated at 50°C. After 0.5h, the preparation of the activated base film is completed;

[0055] S2: Dissolve 3-N,N-dimethylaminomethyl acryloyl chloride in toluene to prepare a grafting monomer solution with a mass concentration of 1%; dissolve disodium 4,4'-diisothiocyanato-2,2'-styrene sulfonate and catalyst ammonium persulfate in deionized water to prepare a cross-linking monomer solution with a mass concentration of 7%, wherein the mass concentration of the catalyst is 2%; apply the grafting monomer solution to the surface of one side of the activated base membrane in S1 to carry out a grafting reaction, the reaction ends after 60 minutes, remove the liquid on the surface of the membrane, dry it naturally, apply the cross-linking monomer solution on the same side, carry out a cross-linking reaction under the action of the catalyst, the reaction ends after 60 minutes and the residual liquid on the surface of the membrane is removed; heat treat the membrane at 60°C, and complete the modification of the surface of one side of the membrane after 7.5 minutes to obtain a single-sided negatively charged membrane;

[0056] S3: Dissolve 4-bromoimidazole in dimethyl sulfoxide to prepare a halogen imidazole solution with a mass concentration of 6%; pour the halogen imidazole solution onto the other side of the activated base membrane coated in S1 to react. After 75 minutes, the reaction is completed and the surface liquid is removed. The membrane is heat-treated at 60°C, and an asymmetric porous membrane is obtained after 7.5 minutes.

[0057] Embodiment 7:

[0058] S1: 4 parts by weight of high molecular weight polymer PES and 2 parts by weight of PVP are added to 13 parts by weight of NMP, heated and stirred, and after being completely dissolved, vacuum degassing is performed to obtain a uniform and bubble-free casting solution; the degassing casting solution is scraped on a clean glass plate by a scraping knife, and the scraped glass plate is quickly immersed in deionized water to complete the preparation of the base film; a potassium permanganate solution with a mass concentration of 1% is prepared, and the base film is hydroxylated and modified at 40°C. After 1.75 hours, the preparation of the activated base film is completed;

[0059] S2: 3-ethoxyacryloyl chloride is dissolved in cyclohexane to prepare a grafting monomer solution with a mass concentration of 5%; allyl vinyl sulfonic acid and catalyst potassium persulfate are dissolved in deionized water to prepare a cross-linking monomer solution with a mass concentration of 4%, wherein the mass concentration of the catalyst is 1.05%; the grafting monomer solution is coated on one side of the surface of the activated base membrane in S1 to carry out a grafting reaction, the reaction ends after 35 minutes, the liquid on the surface of the membrane is removed, and the membrane is naturally dried, and the cross-linking monomer solution is coated on the same side, and a cross-linking reaction is carried out under the action of the catalyst, and the reaction ends after 150 minutes, and the residual liquid on the surface of the membrane is removed; the membrane is heat-treated at 80°C, and the surface modification of one side of the membrane is completed after 5 minutes to obtain a single-sided negatively charged membrane;

[0060] S3: Dissolve 2,4-dibromoimidazole in dichloromethane to prepare a halogen imidazole solution with a mass concentration of 11%; pour the halogen imidazole solution onto the other side of the activated base membrane coated in S1 to react. After 30 minutes, the reaction is completed and the surface liquid is removed. The membrane is heat-treated at 40°C to obtain an asymmetric porous membrane after 10 minutes.

[0061] Embodiment 8:

[0062] S1: Add 5 parts by mass of high molecular weight polymer PES and 2.5 parts by mass of PVP to 13 parts by mass of DMAc, heat and stir, and after complete dissolution, vacuum degassing is performed to obtain a uniform and bubble-free casting solution; the degassing casting solution is scraped on a clean glass plate by a scraping knife, and the scraped glass plate is quickly immersed in deionized water to complete the preparation of the base film; a potassium persulfate solution with a mass concentration of 0.5% is prepared, and the base film is hydroxylated and modified at 30°C. After 3 hours, the preparation of the activated base film is completed;

[0063] S2: dissolve crotonyl chloride in n-hexane to prepare a grafting monomer solution with a mass concentration of 1%; dissolve sodium allyl sulfonate and catalyst potassium persulfate in deionized water to prepare a cross-linking monomer solution with a mass concentration of 7%, wherein the mass concentration of the catalyst is 0.1%; apply the grafting monomer solution to the surface of one side of the activated base membrane in S1 to carry out a grafting reaction, the reaction ends after 60 minutes, remove the liquid on the surface of the membrane, dry it naturally, apply the cross-linking monomer solution on the same side, carry out a cross-linking reaction under the action of the catalyst, the reaction ends after 240 minutes, and remove the residual liquid on the surface of the membrane; heat treat the membrane at 40°C, and complete the modification of the surface of one side of the membrane after 10 minutes to obtain a single-sided negatively charged membrane;

[0064] S3: Dissolve 2,4,5-tribromoimidazole in chloroform to prepare a halogen imidazole solution with a mass concentration of 1%; pour the halogen imidazole solution onto the other side of the activated base membrane coated in S1 to react. After 120 minutes, the reaction is completed and the surface liquid is removed. The membrane is heat-treated at 80°C to obtain an asymmetric porous membrane after 5 minutes.

[0065] Embodiment 9:

[0066] S1: Add 6 parts by mass of high molecular polymer PAN and 3 parts by mass of glycerol to 14 parts by mass of DMF, heat and stir, and after complete dissolution, vacuum degassing to obtain a uniform and bubble-free casting liquid; use a scraper to scrape the degassing casting liquid on a clean glass plate, and quickly immerse the scraped glass plate in deionized water to complete the preparation of the base film; prepare an ammonium persulfate solution with a mass concentration of 1.5%, hydroxylate the base film at 50°C, and after 0.5h, complete the preparation of the activated base film;

[0067] S2: dissolve acryloyl chloride in toluene to prepare a grafting monomer solution with a mass concentration of 9%; dissolve disodium 4,4'-diisothiocyanato-2,2'-styrene sulfonate and catalyst ammonium persulfate in deionized water to prepare a cross-linking monomer solution with a mass concentration of 1%, wherein the mass concentration of the catalyst is 2%; apply the grafting monomer solution to the surface of one side of the activated base membrane in S1 to carry out a grafting reaction, the reaction ends after 10 minutes, remove the liquid on the surface of the membrane, dry it naturally, apply the cross-linking monomer solution on the same side, carry out a cross-linking reaction under the action of the catalyst, the reaction ends after 60 minutes, and remove the residual liquid on the surface of the membrane; heat treat the membrane at 60°C, and complete the modification of the surface of one side of the membrane after 7.5 minutes to obtain a single-sided negatively charged membrane;

[0068] S3: Dissolve 4-(6-bromoimidazo[1,2-a]pyridin-3-yl)pyrimidin-2-amine in dimethyl sulfoxide to prepare a halogen imidazole solution with a mass concentration of 6%; pour the halogen imidazole solution onto the other side of the activated base membrane coated in S1 to react. After 75 minutes, the reaction is completed and the surface liquid is removed. The membrane is heat-treated at 60°C to obtain an asymmetric porous membrane after 7.5 minutes.

[0069] Comparative Example 1:

[0070] The preparation process of this comparative example is different from that of Example 1 in that only step S1 is performed, and steps S2 and S3 are not performed.

[0071] Comparative Example 2:

[0072] The difference between the preparation process of this comparative example and that of Example 1 is that step S1 and step S2 are performed, but step S3 is not performed.

[0073] Comparative Example 3:

[0074] The difference between the preparation process of this comparative example and that of Example 1 is that step S1 and step S3 are performed, but step S2 is not performed.

[0075] The porous membranes prepared in Examples 1 to 9 and Comparative Examples 1 to 3 were stacked and tested under the same test conditions to record the coulombic efficiency, energy efficiency, voltage efficiency and capacity retention rate after 200 charge and discharge cycles of the battery. The test results are shown in Table 1:

[0076] Table 1 Performance test results of porous membranes of examples and comparative examples

[0077]

[0078] As can be seen from Table 1, compared with Comparative Example 1, Examples 1-9 and Comparative Examples 2-3 have higher coulombic efficiency, energy efficiency, voltage efficiency and capacity retention rate, indicating that the membrane prepared by the present invention has a Trade-Off effect in ion selectivity and ion conductivity, and the asymmetry of the charges on both sides of the membrane and the adjustability of the membrane pore size can balance the ion selectivity and ion conductivity to a certain extent, thereby improving the coulombic efficiency, energy efficiency, voltage efficiency and capacity retention rate of the battery.

[0079] Compared with Comparative Example 2, Examples 1 to 9 have higher coulombic efficiency, energy efficiency, voltage efficiency and capacity retention rate because the present invention grafts halogen imidazole monomers on the membrane surface to make the membrane surface positively charged, thereby improving vanadium resistance and increasing the proton transfer rate through the principle of charge opposites attracting each other.

[0080] Compared with Comparative Example 3, Examples 1 to 9 have higher coulombic efficiency, energy efficiency, voltage efficiency and capacity retention rate. Since the membrane surface is first grafted with olefin chloride monomers and then cross-linked with olefin sulfonic acid monomers, the membrane surface is negatively charged and the membrane pore size is adjusted. Through the pore screening principle, the transmembrane transfer of vanadium ions can be prevented, the proton transmission efficiency is improved, and the energy efficiency of the battery is improved.

[0081] The above description is only a preferred embodiment of the present invention and is not intended to limit the present invention. Any modification, equivalent substitution or improvement made within the spirit and principle of the present invention should be included in the protection scope of the present invention.

Claims

1. A method for preparing an asymmetric porous membrane for an all-vanadium redox flow battery, characterized in that: Proceed as follows: S1. Add 4-6 parts by mass of a high molecular polymer and 2-3 parts by mass of a porogen to 11-14 parts by mass of a solvent, heat and stir, and after complete dissolution, vacuum degassing to obtain a casting solution; apply the casting solution on a clean glass plate, and then soak it in deionized water to obtain a base film; soak the base film in an activator solution at a temperature of 30-50° C. for 0.5-3 h to obtain an activated base film; the activator solution is one of potassium persulfate solution, ammonium persulfate solution, potassium permanganate solution, and potassium hydroxide solution, with a mass fraction of 0.5%-1.5%; S2, dissolving olefin chloride substances in an organic solution to prepare a grafting monomer solution; Dissolving olefin sulfonic acid substances and catalysts in deionized water to prepare a cross-linking monomer solution; The grafting monomer solution is coated on one side of the activated base film in S1 to carry out a grafting reaction. After the reaction is completed, the liquid on the membrane surface is removed and the membrane is naturally dried. The cross-linking monomer solution is coated on the same side to carry out a cross-linking reaction under the action of a catalyst. After the reaction is completed, the residual liquid on the membrane surface is removed; the membrane is heat-treated to complete the modification of one side of the membrane surface to obtain a single-sided negatively charged membrane; S3, dissolving the halogen imidazole substance in an organic solvent to prepare a halogen imidazole substance solution; The halogen imidazole substance solution is poured onto the other side surface of the activated base membrane coated in S1 to react. After the reaction is completed, the surface liquid is removed and the membrane is heat-treated to obtain an asymmetric porous membrane.

2. The method for preparing an asymmetric porous membrane for an all-vanadium redox flow battery according to claim 1, characterized in that: In step S1, the high molecular polymer is one of polyethersulfone, polysulfone, polyvinylidene fluoride, and polyacrylonitrile; the porogen is one of polyvinyl pyrrolidone, polyethylene glycol, glycerol, and water; and the solvent is one of N,N-dimethylacetamide, N,N-dimethylformamide, N-methylpyrrolidone, and triethyl phosphate.

3. The method for preparing the asymmetric porous membrane for all-vanadium redox flow battery according to claim 1, characterized in that: In step S2, the olefin chloride substance is one of crotonoyl chloride, propylene chloride, 4-pentenoyl chloride, but-3-enoyl chloride, 1,4-phenylenedipropylene chloride, 3-N,N-dimethylaminomethylpropylene chloride, and 3-ethoxypropylene chloride; the organic solvent is one of n-hexane, toluene, and cyclohexane; and the mass concentration of the olefin chloride substance in the grafting monomer solution is 1% to 9%.

4. The method for preparing the asymmetric porous membrane for all-vanadium redox flow battery according to claim 1, characterized in that: In step S2, the olefin sulfonic acid substance is one or more of sodium allyl sulfonate, disodium 4,4'-diisothiocyanato-2,2'-styrene sulfonate, allyl vinyl sulfonic acid, and sodium methacrylate sulfonate; the mass concentration of the olefin sulfonic acid substance in the cross-linking monomer solution is 1% to 7%; the catalyst is one of potassium persulfate and ammonium persulfate, and the mass concentration of the catalyst in the cross-linking monomer solution is 0.1% to 2%.

5. The method for preparing the asymmetric porous membrane for all-vanadium redox flow battery according to claim 1, characterized in that: In step S2, the grafting reaction time is 10 to 60 minutes; the cross-linking reaction time is 60 to 240 minutes; the heat treatment temperature is 40 to 80° C., and the heat treatment time is 5 to 10 minutes.

6. The method for preparing the asymmetric porous membrane for all-vanadium redox flow battery according to claim 1, characterized in that: In step S3, the halogen imidazole substance is one of 4-chloroimidazole, 4,5-dichloroimidazole, 2-bromo-4,5-dichloroimidazole, 6-bromoimidazo[1,2-A]pyridine-3-carboxamide, 7-bromoimidazo[2,1-F][1,2,4]triazine-4-amine, 4-bromoimidazole, 2,4-dibromoimidazole, 2,4,5-tribromoimidazole, and 4-(6-bromoimidazo[1,2-a]pyridin-3-yl)pyrimidine-2-amine; the organic solvent is one of dichloromethane, chloroform, and dimethyl sulfoxide; and the mass concentration of the halogen imidazole substance in the halogen imidazole substance solution is 1% to 11%.

7. The method for preparing the asymmetric porous membrane for all-vanadium redox flow battery according to claim 1, characterized in that: In step S3, the reaction time is 30-120 min; the heat treatment temperature is 40-80° C., and the heat treatment time is 5-10 min.

8. An asymmetric porous membrane for all-vanadium liquid flow battery, characterized in that: The asymmetric porous membrane for all-vanadium redox flow battery is prepared by the method for preparing an asymmetric porous membrane for all-vanadium redox flow battery as described in any one of claims 1 to 7.