A kind of Al V Moving bed spherical alumina carrier and preparation method and application thereof

By grafting the AlV site on the surface of the spherical alumina support, the sintering and phase separation problems of the PtSn catalyst are solved, the catalytic performance and mechanical strength are improved, and it is suitable for propane dehydrogenation and continuous reforming processes.

CN118767904BActive Publication Date: 2024-11-19SHANDONG XINBO CHEMICAL TECHNOLOGY CO LTD +1
View PDF 0 Cites 0 Cited by

Patent Information

Application Number
CN202411244627.1
Authority / Receiving Office
CN · China
Patent Type
Patents(China)
Current Assignee / Owner
Filing Date
2024-09-06
Publication Date
2024-11-19
Estimated Expiration
2044-09-06

AI Technical Summary

Technical Problem

Commercial PtSn catalysts are prone to Pt particle sintering and Pt-Sn phase separation during propane dehydrogenation and continuous reforming, and the prior art is difficult to controllably construct AlV sites on the surface of spherical alumina support, affecting catalytic performance. .

Method used

By mixing high-purity slimeite with modifier and water, and calcining after hydrothermal crystallization, AlV-containing alumina powder is prepared, and the AlV-containing alumina powder is combined using composite glue liquid molding technology to form alumina powders. Branches to the surface of the spherical alumina support, combined with the regulation of the calcining atmosphere and temperature, ensuring the mechanical strength of the catalyst and the distribution of AlV sites.

Benefits of technology

The controllable distribution of the AlV site on the surface of the spherical alumina support is achieved, which avoids sintering of Pt particles and separation of Pt-Sn phase, improves the conversion rate and selectivity of the catalyst, maintains the mechanical strength of the spherical alumina support, and is suitable for Propane dehydrogenation and continuous reforming process.

✦ Generated by Eureka AI based on patent content.

Smart Images

  • Figure CN118767904B_ABST
    Figure CN118767904B_ABST
Patent Text Reader

Abstract

The present invention relates to a method comprising V The invention discloses a moving bed spherical alumina carrier and its preparation method and application, belonging to the technical field of catalytic materials. The invention solves the technical problem that commercial PtSn catalysts are prone to Pt particle sintering and Pt-Sn phase separation in the prior art. The preparation method of the invention firstly hydrothermally crystallizes high-purity pseudo-boehmite, a modifier and water; then, the obtained alumina precursor is roasted, ground and sieved to obtain an Al-containing V Alumina powder; high-purity pseudo-boehmite, gelatin, gum arabic and water are mixed evenly to prepare a composite glue liquid; finally, the composite glue liquid is dripped into a liquid column composed of an upper oil phase and a lower curing agent solution to form a mold until it is completely solidified, and then dried and calcined to obtain an Al-containing V The preparation method comprises a moving bed spherical alumina carrier. V Alumina powder is grafted on the surface of spherical alumina without reducing the mechanical strength. V Content and mechanical strength are adjustable.
Need to check novelty before this filing date? Find Prior Art

Description

Technical Field

[0001] The invention belongs to the technical field of catalytic materials and particularly relates to a catalyst containing Al V (penta-coordinated aluminum ion) moving bed spherical alumina carrier and its preparation method and application, especially the one containing Al V Application of moving bed spherical alumina carrier in propane dehydrogenation or continuous reforming. Background Art

[0002] Propane dehydrogenation and continuous reforming are important refining and chemical processes. Propane dehydrogenation can be used to produce propylene and clean hydrogen. Continuous reforming is mainly used to produce high-octane gasoline, BTX aromatics and by-product hydrogen. Both processes use moving bed technology and PtSn / Al 2 O 3 Catalysts. It is of great significance to develop spherical alumina supports suitable for moving bed technology and to meet the requirements of propane dehydrogenation / continuous reforming.

[0003] Commercial PtSn catalysts generally face the problems of Pt particle sintering and PtSn phase separation. V sites, which can inhibit the sintering of Pt particles and promote the interaction between Pt and Sn, which is beneficial to improve the conversion rate and selectivity at the same time. V The site-specific moving bed spherical alumina is a technical challenge for optimizing commercial PtSn catalysts. This technology requires the coupling of the molding and surface modification of the moving bed spherical alumina.

[0004] CN 113289595 B discloses a process for preparing spherical alumina using one or more aluminum sources selected from pseudo-boehmite, boehmite, metallic aluminum, aluminum salts, and alcohol aluminum. The average particle size of the spherical alumina is between 1.8 and 1.85 mm, and the average strength is between 35 and 75 N / particle. However, this spherical alumina does not contain Al V .

[0005] CN 116747851 B and CN 116803512 B disclose a method for synthesizing low bulk ratio spherical alumina based on two powders. The technical methods disclosed in CN 116747851 B and CN 116803512 B are only applicable to optimizing the internal structure of spherical alumina such as pores, specific surface area, bulk ratio, etc.

[0006] For a moving bed spherical alumina carrier suitable for propane dehydrogenation / continuous reforming, Al VThe sites exist on the surface of the spherical alumina rather than inside. This is because the sites existing inside have little effect on the reaction performance of the spherical catalyst. In addition, as emphasized in CN 116747851 B and CN 116803512 B, the porous alumina powder added has low peptization solubility, and excessive porous alumina powder doped into the interior of the spherical alumina will significantly reduce the mechanical strength. Therefore, how to controllably add Al V It is a technical difficulty in this field to graft alumina powder onto the surface of spherical alumina without reducing its mechanical strength. Summary of the invention

[0007] In view of this, the present invention provides a PtSn catalyst containing Al to solve the technical problem that Pt particles are easily sintered and Pt-Sn phases are easily separated in the commercial PtSn catalyst in the prior art. V Moving bed spherical alumina carrier and its preparation method and application, containing Al V The alumina powder is grafted onto the surface of the spherical alumina without reducing its mechanical strength.

[0008] In order to achieve the above technical objectives, the present invention adopts the following technical solutions:

[0009] The Al-containing V The preparation method of the moving bed spherical alumina carrier comprises the following steps:

[0010] (1) mixing high-purity pseudo-boehmite, a modifier and water, performing hydrothermal crystallization, filtering, washing and drying the obtained solid to obtain an alumina precursor;

[0011] The modifier is one or two of ammonium acetate, ammonium nitrate, ammonium chloride, ammonium sulfate, ammonium citrate, ammonium tartrate, ammonium carbonate, ammonium bicarbonate, urea and ammonium oxalate;

[0012] (2) The alumina precursor obtained in step (1) is heated in NH 3 、N 2 , CO 2 , air or H 2 In a nitrogen (bubbling method) atmosphere, the temperature is raised to 500-900°C at a heating rate of 1-5°C / min, and calcined for 1-2h. The obtained powder is ground and sieved to a particle size of 60-180 mesh to obtain Al-containing V Alumina powder;

[0013] (3) first dispersing high-purity pseudo-boehmite in water, and after forming a sol, adding water, stirring evenly, and adjusting the pH to 7-8 to obtain a slurry with a concentration of 5wt%-10wt% of high-purity pseudo-boehmite;

[0014] Then, the slurry is heated to 50-60°C, gelatin, gum arabic and water are added, and mixed evenly to prepare a composite glue solution;

[0015] (4) The composite glue solution is dripped into the liquid column composed of the upper oil phase and the lower curing agent solution to form a solidified gel ball, which is then dried and calcined to obtain an Al-containing gel ball. V A moving bed spherical alumina carrier;

[0016] The curing agent solution contains Al V Alumina powder, aldehyde and surfactant, and the curing agent solution contains Al V The content of alumina powder is total Al 2 O 3 Feeding amount (the curing agent solution contains Al V 5wt%-20wt% of the total amount of high-purity pseudo-boehmite in the alumina powder and composite colloid.

[0017] Preferably, in step (1), the purity of the high-purity pseudo-boehmite is greater than 99.99%.

[0018] Preferably, in step (1), the mass ratio of the high-purity pseudo-boehmite, the modifier and water is 12.5:2:30.

[0019] Preferably, in step (1), the temperature of the hydrothermal crystallization is 140 o C, the hydrothermal crystallization time is 12-24h.

[0020] Preferably, in step (1), the container for hydrothermal crystallization is a hydrothermal kettle.

[0021] Preferably, in step (1), the drying temperature is 80° C. and the drying time is 12 h.

[0022] Preferably, in step (1), water is used for washing.

[0023] Preferably, in step (3), the purity of the high-purity pseudo-boehmite is greater than 99.99%.

[0024] Preferably, in step (3), the mass ratio of the high-purity pseudo-boehmite, gelatin, gum arabic and water is 100:20:20:500, and the water is the water added to the slurry after the slurry is heated to 50-60°C.

[0025] Preferably, in step (3), nitric acid and aqueous ammonia are used to adjust the pH.

[0026] Preferably, in step (4), the aldehyde is formaldehyde or glutaraldehyde, and the aldehyde content in the curing agent solution is 1wt%-2wt%.

[0027] Preferably, in step (4), the surfactant is AEO-6, Peregal O-6 or penetrant JFC, and the content of the surfactant in the curing agent solution is 0.2wt%-0.4wt%.

[0028] Preferably, in step (4), the composite adhesive solution is immersed in the lower layer of curing agent solution for 5-60 minutes after passing through the upper layer of oil phase.

[0029] Preferably, in step (4), the pH of the curing agent solution is adjusted to 4 using nitric acid.

[0030] Preferably, in step (4), the temperature in the liquid column is 5-10°C.

[0031] Preferably, in step (4), the drying temperature is 100°C.

[0032] Preferably, in step (4), the calcination temperature is 550°C.

[0033] The present invention also provides Al-containing prepared by the above preparation method V Moving bed spherical alumina carrier.

[0034] Preferably, the Al-containing V The specific surface area of ​​the moving bed spherical alumina carrier is 170-210m 2 / g, pore volume is between 0.38-0.54cm 3 / g, Al V The proportion is between 5.52wt%-19.60wt%, and the mechanical strength is 35-75N / particle.

[0035] The present invention also provides the above-mentioned Al-containing V Application of moving bed spherical alumina carrier in propane dehydrogenation or continuous reforming.

[0036] Preferably, the Al V The moving bed spherical alumina carrier is loaded with PtSn and used for propane dehydrogenation or continuous reforming.

[0037] Preferably, the Al-containing V The moving bed spherical alumina carrier is immersed in an ethanol solution containing chloroplatinic acid and stannous chloride for 2-10 hours, dried at 50-80°C for 12 hours, and calcined at 500°C for 3 hours to obtain a spherical alumina carrier loaded with PtSn for propane dehydrogenation or continuous reforming.

[0038] The principle of the present invention is:

[0039] (1) Al V The sites are generated from the decomposition of the alumina precursor, but the alumina precursor decomposes rapidly, or CO2 NH 3 , H 2 Gases such as O will react with low coordination sites, which will significantly change the Al V Therefore, controlled decomposition of the alumina precursor is required to construct Al V On the one hand, the heating rate and calcination temperature change the decomposition rate of the alumina precursor in a temperature-adjusting manner. On the other hand, the decomposition of the alumina precursor produces CO 2 NH 3 , H 2 O and other gases, the decomposition of alumina precursor in different atmospheres will change the decomposition behavior and induce the evolution of surface functional groups. Therefore, adjusting the heating rate, calcination temperature and calcination atmosphere can adjust the decomposition behavior of alumina precursor, thereby affecting the obtained Al-containing V Al in alumina powder V The mass ratio of high-purity pseudo-boehmite, modifier and water, hydrothermal temperature, hydrothermal time, etc. can regulate the crystal phase evolution of the alumina precursor. The crystal phase difference of the alumina precursor will determine whether the calcined amorphous alumina, γ-Al 2 O 3 or θ-Al 2 O 3 One or more of the following. The crystal phase of aluminum oxide determines the Al V This further requires the preparation of alumina precursors under appropriate conditions and the decomposition of the precursors at appropriate temperatures (heating rate of 1-5 °C / min, heating to 500-900 °C) to prepare Al-containing V of aluminum oxide.

[0040] (2) Containing Al V Alumina powder can provide Al V sites, but will reduce the mechanical strength of the spherical carrier. V The particle size of alumina powder and the formula of curing agent solution can promote the V The alumina powder is evenly dispersed, which will be beneficial to obtain both Al V sites and high mechanical strength of spherical alumina. Therefore, it is necessary to V content and mechanical strength requirements, reasonably choose Al V The content of alumina powder.

[0041] (3) The droplets of the composite glue will shrink into balls in the oil phase, and after passing through the oil-water interface and entering the curing agent solution, a gelation reaction will occur to form composite gel spheres. At the same time, the Al-containing VThe aluminum oxide powder is adsorbed and grafted onto the surface of the composite gel ball. The gel ball is further immersed in the curing agent solution for 5-60 minutes until it is completely cured; the cured gel ball is taken out, dried, and calcined to obtain Al-containing V Moving bed spherical alumina carrier.

[0042] Compared with the prior art, the present invention has the following beneficial effects:

[0043] The Al-containing V A method for preparing a moving bed spherical alumina carrier, wherein the Al-containing V The alumina powder is grafted onto the surface of the spherical alumina carrier in the moving bed; and by adjusting the viscosity of the curing agent solution and the content of Al V The particle size of alumina powder is V The aluminum oxide powder is evenly dispersed in the curing agent solution. During the molding process, the spherical aluminum oxide precursor that has passed through the oil phase stays in the curing agent solution for a certain period of time and absorbs the aluminum-containing V Alumina powder, so that the Al-containing V The present invention is to prepare alumina powder grafted onto the surface of spherical alumina. V The moving bed spherical alumina support provides technical support for site and mechanical strength.

[0044] The Al-containing V The moving bed spherical alumina carrier specifically solves the problem of Pt particle sintering and Pt-Sn phase separation in commercial PtSn catalysts. V The sites are controllably concentrated on the surface of the spherical alumina, thus avoiding the problem of surface site waste. At the same time, there is a large amount of commercial alumina inside the spherical alumina, which better maintains the mechanical strength of the spherical alumina carrier.

[0045] The Al-containing V The moving bed spherical alumina carrier can be used in propane dehydrogenation and continuous reforming. Experimental tests show that when used for propane dehydrogenation, the propane conversion rate is 40.2% and the propylene selectivity is 96.9%; when used for continuous reforming, the aromatics yield is 141% and the hydrogen purity is 94%. BRIEF DESCRIPTION OF THE DRAWINGS

[0046] In order to more clearly illustrate the technical solutions in the embodiments of the present invention, the drawings required for use in the embodiments will be briefly introduced below. Obviously, the drawings described below are only some specific implementation methods of the present invention. For ordinary technicians in this field, other drawings can be obtained based on these drawings without paying creative work.

[0047] Figure 1 XRD diagrams of Examples 1, 2, 3, 4, 5, 6 and Comparative Example 1 of the present invention;

[0048] Figure 2 The nitrogen adsorption-desorption isotherms of Examples 1, 2, 3, 4, 5, 6 and Comparative Example 1 of the present invention;

[0049] Figure 3 The pore size distribution diagrams of Examples 1, 2, 3, 4, 5, 6 and Comparative Example 1 of the present invention are shown;

[0050] Figure 4 For Examples 1, 2, 3, 4, 5, 6 of the present invention and Comparative Example 1 27 Al MAS NMR spectra;

[0051] Figure 5 The reaction performance of using the moving bed spherical alumina obtained in Example 3 of the present invention and Comparative Example 1 as a carrier to load PtSn for propane dehydrogenation. DETAILED DESCRIPTION

[0052] In order to enable those skilled in the art to better understand the technical solution of the present invention, the present invention will be further described in detail below in conjunction with embodiments.

[0053] In the following examples, various processes and methods not described in detail are conventional methods known in the art. Unless otherwise specified, the materials, reagents, devices, instruments, equipment, etc. used in the following examples can be obtained from commercial sources.

[0054] Example 1

[0055] The Al-containing V The method for preparing a moving bed spherical alumina carrier comprises the following steps:

[0056] (1) At room temperature, urea: high-purity pseudo-boehmite: water in a mass ratio of 12.5:2:30 was added to a hydrothermal reactor. Hydrothermal crystallization was performed at 140°C for 24 hours. The solid obtained after hydrothermal crystallization was filtered, washed (with water), and dried at 80°C for 12 hours to obtain an alumina precursor. The alumina precursor was heated to 40°C in N 2 In an atmosphere, the temperature was raised to 500°C at a rate of 2°C / min, and then calcined for 2 hours. The obtained solid was ground and sieved to 60 mesh to obtain Al-containing V of alumina powder.

[0057] (2) Disperse 100 g of SB powder (pseudo-boehmite produced by Sasol, Germany) in 400 g of deionized water. After the SB powder is completely converted into a sol, add 500 g of deionized water and stir evenly. Then, use nitric acid and ammonia water to adjust the pH to 7-8 to obtain a slurry.

[0058] (3) Heat the slurry to 60°C, add 500g of water, 20g of gelatin and 20g of gum arabic, stir thoroughly to dissolve, and prepare a composite glue solution; drip the composite glue solution into a liquid column composed of white oil on the upper layer and curing agent solution on the lower layer to form a curing agent solution. The curing agent solution contains 1wt% glutaraldehyde, 0.4wt% surfactant (AEO-6), and 25g Al V Alumina powder (20wt% of total alumina content); adjust the pH of the curing agent solution to 4 with nitric acid; control the temperature in the liquid column to 5-10°C. After the composite glue passes through the upper oil phase, it is immersed in the lower curing agent solution for 5-60 minutes until it is completely solidified. The obtained solid is dried at 100°C and calcined at 550°C to obtain Al-containing V The moving bed spherical alumina carrier; named Al 2 O 3 -11.26.

[0059] After determination, the Al-containing V The average particle size of the moving bed spherical alumina carrier is 1.7 mm, the average strength is 35 N / particle, and the pore volume is 0.40 cm 3 / g, specific surface area is 195m 2 / g,Al V The content is 11.26wt%.

[0060] Example 2

[0061] The Al-containing V The method for preparing a moving bed spherical alumina carrier comprises the following steps:

[0062] (1) The preparation method of the aluminum oxide precursor is as in Example 1. The aluminum oxide precursor is heated to 700°C at a heating rate of 3°C / min in an air atmosphere, calcined for 2 hours, and ground and sieved to 100 mesh to obtain an aluminum oxide precursor. V of alumina powder.

[0063] (2) The preparation method of the slurry is the same as that in Example 1.

[0064] (3) Heat the slurry to 60°C, add 500g water, 20g gelatin and 20g gum arabic, stir thoroughly to dissolve, and prepare a composite glue solution; drip the composite glue solution into a liquid column composed of white oil on the upper layer and curing agent solution on the lower layer to form a curing agent solution. The curing agent solution contains 2wt% formaldehyde, 0.2wt% surfactant (peregal O-6), and 20g Al V Alumina powder (accounting for 16.7wt% of the total alumina content). The subsequent operations were carried out according to Example 1 to obtain Al VThe moving bed spherical alumina carrier; named Al 2 O 3 -15.58.

[0065] After determination, the Al-containing V The average particle size of the moving bed spherical alumina carrier is 1.8 mm, the average strength is 55 N / particle, and the pore volume is 0.49 cm 3 / g, specific surface area is 207m 2 / g,Al V The content is 15.58wt%.

[0066] Example 3

[0067] The Al-containing V The method for preparing a moving bed spherical alumina carrier comprises the following steps:

[0068] (1) The preparation method of aluminum oxide precursor is as in Example 1. The aluminum oxide precursor is heated in CO 2 In the atmosphere, the temperature was raised to 600℃ at a rate of 1℃ / min, calcined for 2h, and ground and sieved to 80 mesh to obtain Al-containing V of alumina powder.

[0069] (2) The preparation method of the slurry is the same as that in Example 1.

[0070] (3) Heat the slurry to 60°C, add 500g water, 20g gelatin and 20g gum arabic, stir thoroughly to dissolve, and prepare a composite glue solution; drip the composite glue solution into a liquid column composed of white oil on the upper layer and curing agent solution on the lower layer to form a solid. The curing agent solution contains 1wt% formaldehyde, 0.2wt% surfactant (penetrant JFC), and 15g Al V Alumina powder (13wt% of total alumina content) was obtained by performing subsequent operations according to Example 1. V The moving bed spherical alumina carrier, named Al 2 O 3 -19.60.

[0071] After determination, the Al-containing V The average particle size of the moving bed spherical alumina carrier is 1.8 mm, the average strength is 75 N / particle, and the pore volume is 0.53 cm 3 / g, specific surface area is 210m 2 / g,Al V The content is 19.60wt%.

[0072] Example 4

[0073] The Al-containingV The method for preparing a moving bed spherical alumina carrier comprises the following steps:

[0074] (1) The preparation method of aluminum oxide precursor is as in Example 1. The aluminum oxide precursor is heated in NH 3 In the atmosphere, the temperature was raised to 900℃ at a rate of 5℃ / min, calcined for 2h, and ground and sieved to 150 mesh to obtain Al-containing V of alumina powder.

[0075] (2) The preparation method of the slurry is the same as that in Example 1.

[0076] (3) Heat the slurry to 60°C, add 500g water, 20g gelatin and 20g gum arabic, stir thoroughly to dissolve, and prepare a composite glue solution; drip the composite glue solution into a liquid column composed of white oil on the upper layer and curing agent solution on the lower layer to form a solid. The curing agent solution contains 2wt% formaldehyde, 0.2wt% surfactant (peregal O-6), and 5g Al V Alumina powder (accounting for 5wt% of the total alumina content). The subsequent operations were carried out according to Example 1 to obtain Al V The moving bed spherical alumina carrier, named Al 2 O 3 -5.52.

[0077] After determination, the Al-containing V The average particle size of the moving bed spherical alumina carrier is 1.7 mm, the average strength is 65 N / particle, and the pore volume is 0.42 cm 3 / g, specific surface area is 170m 2 / g,Al V The content is 5.52wt%.

[0078] Example 5

[0079] The Al-containing V The method for preparing a moving bed spherical alumina carrier comprises the following steps:

[0080] (1) The preparation method of aluminum oxide precursor is the same as that in Example 1. 2 O nitrogen (bubbling method), the temperature was raised to 800℃ at a rate of 4℃ / min, calcined for 2h, and ground and sieved to 120 mesh to obtain Al-containing V of alumina powder.

[0081] (2) The preparation method of the slurry is the same as that in Example 1.

[0082] (3) Heat the slurry to 60°C, add 500g water, 20g gelatin and 20g gum arabic, stir thoroughly to dissolve, and prepare a composite glue solution; drip the composite glue solution into a liquid column composed of white oil on the upper layer and curing agent solution on the lower layer to form a solid. The curing agent solution contains 1wt% glutaraldehyde, 0.2wt% surfactant (penetrant JFC), and 10g Al V Alumina powder (accounting for 10wt% of the total alumina content). The subsequent operations were carried out according to Example 1 to obtain Al V The moving bed spherical alumina carrier, named Al 2 O 3 -18.35.

[0083] After determination, the Al-containing V The average particle size of the moving bed spherical alumina carrier is 1.8 mm, the average strength is 55 N / particle, and the pore volume is 0.51 cm 3 / g, specific surface area is 210m 2 / g,Al V The content is 18.35wt%.

[0084] Example 6

[0085] The Al-containing V The method for preparing a moving bed spherical alumina carrier comprises the following steps:

[0086] (1) The preparation method of the aluminum oxide precursor is as in Example 1. The aluminum oxide precursor is heated to 550°C at a heating rate of 2°C / min in an air atmosphere, calcined for 2 hours, and ground and sieved to 180 mesh to obtain an aluminum oxide precursor. V of alumina powder.

[0087] (2) The preparation method of the slurry is the same as that in Example 1.

[0088] (3) Heat the slurry to 60°C, add 500g of water, 20g of gelatin and 20g of gum arabic, stir thoroughly to dissolve, and prepare a composite glue solution; drip the composite glue solution into a liquid column composed of white oil on the upper layer and curing agent solution on the lower layer to form a curing agent solution. The curing agent solution contains 1wt% formaldehyde, 0.2wt% surfactant (AEO-6), and 15g Al V Alumina powder (accounting for 13wt% of the total alumina content) was obtained according to Example 1. V The moving bed spherical alumina carrier, named Al 2 O 3 -13.64.

[0089] After determination, the Al-containingV The average particle size of the moving bed spherical alumina carrier is 1.7 mm, the average strength is 55 N / particle, and the pore volume is 0.52 cm 3 / g, specific surface area is 180m 2 / g,Al V The content is 13.64wt%.

[0090] Comparative Example 1

[0091] (1) The slurry preparation method is the same as that in Example 1.

[0092] (2) Heat the slurry to 60°C, add 500g of water, 20g of gelatin and 20g of gum arabic, stir thoroughly to dissolve, and prepare a composite glue solution; drip the composite glue solution into a liquid column composed of white oil on the upper layer and curing agent solution on the lower layer to form a solid. The curing agent solution contains 1wt% glutaraldehyde, 0.4wt% surfactant (penetrant JFC), and 0g Al V The subsequent operations were carried out according to Example 1 to obtain a moving bed spherical alumina carrier, named Al 2 O 3 -0.

[0093] The results show that the average particle size of the moving bed spherical alumina carrier prepared in this comparative example is 1.7 mm, the average strength is 55 N / particle, and the pore volume is 0.52 cm 3 / g, specific surface area is 217m 2 / g,Al V The content is 0wt%.

[0094] The moving bed spherical alumina carriers prepared in Examples 1, 2, 3, 4, 5, 6 and Comparative Example 1 were subjected to XRD detection, nitrogen adsorption and desorption detection, pore size distribution analysis, and 27 Al MAS NMR detection. Characterization description: According to Figure 1 It can be found that the obtained moving bed spherical alumina has γ-Al 2 O 3 Crystalline phase, according to Figure 2 The nitrogen adsorption and desorption results show that the specific surface area of ​​these spherical aluminas is between 170 and 210 m 2 / g, pore volume is between 0.38-0.54cm 3 / g. Figure 3 It can be concluded that the pore size of all samples is about 10nm. Figure 4 The Al content in the sample can be calculated V content, and found that Al V The content varies between 5.52-19.60wt%.

[0095] Example 7

[0096] This example uses the moving bed spherical alumina carrier obtained in Example 3 and Comparative Example 1 to load PtSn for propane dehydrogenation.

[0097] (1) The moving bed spherical alumina support was impregnated in an ethanol solution containing chloroplatinic acid and stannous chloride by an equal volume impregnation method for 2 hours. The Pt loading (loading refers to the mass percentage of the metal in the catalyst) was 0.30wt%, and the Sn loading was 0.15wt%. Subsequently, after drying at 50°C for 12 hours, it was calcined at 500°C for 3 hours to obtain a propane dehydrogenation catalyst.

[0098] (2) The activity of the prepared propane dehydrogenation catalyst was evaluated as follows:

[0099] ① Catalyst activation: Take 2 g of propane dehydrogenation catalyst and place it in 40 ml / min H 2 The mixture was reduced at 400 °C for 1 h.

[0100] ② Catalyst activity evaluation: The propane dehydrogenation catalyst was evaluated at 550°C in a reaction gas flow of 300 ml / min (propane / nitrogen = 5 / 95).

[0101] Figure 5 Compared with the use of Al V Spherical alumina carrier (Example 3) and Al-free V The propane dehydrogenation performance of the spherical alumina support (Comparative Example 1) after loading PtSn was found to be V The sites significantly improved the propane conversion and propylene selectivity of the catalyst.

[0102] Example 8

[0103] This example uses the Al-containing V The moving bed spherical alumina carrier loaded with PtSn was used for continuous reforming.

[0104] (1) Containing Al V The moving bed spherical alumina carrier was impregnated in an ethanol solution containing chloroplatinic acid and stannous chloride by an equal volume impregnation method for 2 hours. The Pt loading was 0.30wt% and the Sn loading was 0.30wt%. Subsequently, after drying at 50°C for 12 hours, it was calcined at 500°C for 3 hours to obtain a continuous reforming catalyst.

[0105] (2) The activity of the prepared continuous reforming catalyst was evaluated as follows:

[0106] In the micro-reactor evaluation device, 3 ml of continuous reforming catalyst was loaded, and the catalyst performance was evaluated using n-heptane as the raw material. The reaction conditions were controlled as follows: reaction temperature 510 °C, pressure 0.7 MPa, hydrogen-to-oil molar ratio 5, feed liquid volume space velocity 5 h -1 .

[0107] (3) Reaction results: The yield of aromatics was 141% and the purity of hydrogen was 94%.

[0108] Obviously, the above embodiments are merely examples for clear explanation, and are not intended to limit the embodiments. For those skilled in the art, other different forms of changes or modifications can be made based on the above description. It is not necessary and impossible to list all the embodiments here. The obvious changes or modifications derived from them are still within the protection scope of the invention.

Claims

1. Contains Al V A method for preparing a moving bed spherical alumina carrier, characterized in that: Here are the steps: (1) mixing high-purity pseudo-boehmite, a modifier and water, performing hydrothermal crystallization, filtering, washing and drying the obtained solid to obtain an alumina precursor; The modifier is one or two of ammonium acetate, ammonium nitrate, ammonium chloride, ammonium sulfate, ammonium citrate, ammonium tartrate, ammonium carbonate, ammonium bicarbonate, urea and ammonium oxalate; (2) The alumina precursor obtained in step (1) is heated to 500-900°C in an atmosphere of NH3, N2, CO2, air or nitrogen containing H2O at a heating rate of 1-5°C / min, and calcined for 1-2h. The obtained powder is ground and sieved to a particle size of 60-180 mesh to obtain Al-containing V Alumina powder; (3) first dispersing high-purity pseudo-boehmite in water, and after forming a sol, adding water, stirring evenly, and adjusting the pH to 7-8 to obtain a slurry with a concentration of 5wt%-10wt% of high-purity pseudo-boehmite; Then, the slurry is heated to 50-60°C, gelatin, gum arabic and water are added, and mixed evenly to prepare a composite glue solution; (4) The composite glue solution is dripped into the liquid column composed of the upper oil phase and the lower curing agent solution to form a solidified gel ball, which is then dried and calcined to obtain an Al-containing gel ball. V A moving bed spherical alumina carrier; The curing agent solution contains Al V Alumina powder, aldehyde and surfactant, and the curing agent solution contains Al V The content of alumina powder is the content of Al in the curing agent solution. V 5wt%-20wt% of the total amount of high-purity pseudo-boehmite in the alumina powder and the composite colloid.

2. The Al-containing V A method for preparing a moving bed spherical alumina carrier, characterized in that: In step (1), The purity of the high-purity pseudo-boehmite is greater than 99.99%; The mass ratio of the high-purity pseudo-boehmite, the modifier and water is 12.5:2:30; The hydrothermal crystallization temperature is 140 o C, hydrothermal crystallization time is 12-24h; Wash with water.

3. The Al-containing V A method for preparing a moving bed spherical alumina carrier, characterized in that: In step (3), The purity of the high-purity pseudo-boehmite is greater than 99.99%; The mass ratio of the high-purity pseudo-boehmite, gelatin, gum arabic and water is 100:20:20:500, and the water is the water added to the slurry after the slurry is heated to 50-60° C.; The pH was adjusted with nitric acid and ammonia.

4. The Al-containing V A method for preparing a moving bed spherical alumina carrier, characterized in that: In step (4), The aldehyde is formaldehyde or glutaraldehyde, and the aldehyde content in the curing agent solution is 1wt%-2wt%; The surfactant is AEO-6, Peregal O-6 or penetrant JFC, and the content of the surfactant in the curing agent solution is 0.2wt%-0.4wt%.

5. The Al-containing V A method for preparing a moving bed spherical alumina carrier, characterized in that: In step (4), After the composite adhesive solution passes through the upper oil phase, it is immersed in the lower curing agent solution for 5-60 minutes; The pH of the curing agent solution is adjusted to 4 with nitric acid; The temperature in the liquid column is 5-10°C; The drying temperature is 100°C; The calcination temperature is 550°C.

6. Al-containing prepared by the preparation method according to any one of claims 1 to 5 V Moving bed spherical alumina carrier.

7. The Al-containing V The moving bed spherical alumina carrier is characterized in that The Al-containing V The specific surface area of ​​the moving bed spherical alumina carrier is 170-210m 2 / g, pore volume is between 0.38-0.54cm 3 / g, Al V The proportion is between 5.52wt%-19.60wt%, and the mechanical strength is 35-75N / particle.

8. The Al-containing V Application of moving bed spherical alumina carrier in propane dehydrogenation or continuous reforming.

9. The Al-containing V The invention discloses a moving bed spherical alumina carrier for use in propane dehydrogenation or continuous reforming, characterized in that: Containing Al V The moving bed spherical alumina carrier is loaded with PtSn and used for propane dehydrogenation or continuous reforming.

10. The Al-containing V The invention discloses a moving bed spherical alumina carrier for use in propane dehydrogenation or continuous reforming, characterized in that: Containing Al V The moving bed spherical alumina carrier is immersed in an ethanol solution containing chloroplatinic acid and stannous chloride for 2-10 hours, dried at 50-80°C for 12 hours, and calcined at 500°C for 3 hours to obtain a spherical alumina carrier loaded with PtSn for propane dehydrogenation or continuous reforming.