Method for preparing catalyst for hydrogen cyanide decomposition by using wastewater containing copper ions
By mixing copper ion-containing wastewater with nano-alumina and roasting to prepare a catalyst, the problem of catalyst poisoning and high cost in the hydrogen cyanide removal process in the existing technology is solved, and efficient and stable hydrogen cyanide decomposition is achieved.
Patent Information
- Application Number
- CN202410749015.1
- Authority / Receiving Office
- CN · China
- Patent Type
- Applications(China)
- Current Assignee / Owner
- Filing Date
- 2024-06-11
- Publication Date
- 2024-10-15
AI Technical Summary
Existing technologies have problems with catalyst poisoning, high costs, and safety risks of adsorbent activation when removing hydrogen cyanide, and the adsorbent cannot directly remove -CN species, resulting in the leakage of highly toxic substances.
By mixing copper ion-containing wastewater with nano-alumina, adjusting the pH value and roasting, a copper oxide-loaded catalyst is prepared and used to catalyze the decomposition of hydrogen cyanide.
The production of low-cost catalysts has been achieved, with excellent catalytic decomposition ability of hydrogen cyanide, able to completely remove hydrogen cyanide from industrial waste gas at 225°C, and with strong stability.
Smart Images

Figure CN118767915A_ABST
Abstract
Description
Technical Field
[0001] The invention belongs to the technical field of catalysts, and in particular relates to a method for preparing a catalyst for decomposing hydrogen cyanide by utilizing wastewater containing copper ions. Background Art
[0002] With the rapid development of industry, heavy metal ion pollution has seriously affected the survival and development of human society and has become a hot issue of concern to the world. Copper ions in the environment can easily enter the human body through the food chain, posing a serious threat to human health, causing headaches, breathing difficulties, intravascular hemolysis, and damage to the nervous system. Based on these hazards, people have studied many ways to treat copper ion waste liquid. People have developed a variety of ways to remove copper ions, such as precipitation, membrane filtration, ion exchange, electrolysis and adsorption. Among them, adsorption is the most commonly used method. This method is simple to operate, consumes less energy, is low in cost, and most importantly, has a high removal rate. Nanomaterials in adsorption materials have many adsorption advantages, so they are very popular.
[0003] Hydrogen cyanide (HCN), as a highly toxic chemical, is extremely harmful to human health and the living environment. However, HCN vapor is released into the air from various anthropogenic sources, including coal chemical industry, metal mining, synthetic fiber processing, and rubber industry. In recent years, wind power generation, as one of the clean energy sources, has also been vigorously developed. Carbon fiber is often used in the blades of wind turbines. In addition, in the medical, construction, aviation, and semiconductor industries, more and more metals are replaced by carbon fiber materials. However, the production of carbon fiber often faces HCN emissions. Therefore, with the continuous increase in HCN emissions, it is urgent to remove HCN, an unconventional pollutant in industrial waste gas.
[0004] Adsorption and catalytic oxidation are widely used methods for removing HCN. For the catalytic oxidation method, expensive catalysts and high reaction temperatures limit its industrial application. For the adsorption method, the adsorbent cannot directly remove -CN, which may lead to the leakage of highly toxic -CN species. In addition, the activation and transport of the adsorbent also face huge safety risks. Currently, activated carbon impregnated with metal salts is an effective adsorbent for removing hydrogen cyanide from the air, but -CN still exists. In industry, alkaline washing is often used to remove HCN in the gas phase. This method is simple and efficient, but the neutralization of HCN with alkaline solution easily forms more toxic NaCN or KCN. At present, most research focuses on the catalytic hydrolysis of HCN in the gas phase.
[0005] Pt, Pd, Rh, Ag, V2O5, WO3 and CuSO4 loaded on TiO2 particles are active centers in the catalytic hydrolysis reaction of HCN. However, due to the presence of precious metals, they often face the problem of catalyst poisoning after HCN decomposition and are expensive, so they are gradually eliminated. Summary of the invention
[0006] The object of the present invention is to provide a method for preparing a catalyst for decomposing hydrogen cyanide by using wastewater containing copper ions. The method provided by the present invention uses wastewater containing copper ions as a raw material, can reduce the production cost of the catalyst, and the obtained catalyst has excellent catalytic decomposition ability for hydrogen cyanide.
[0007] In order to achieve the above object, the present invention provides the following technical solutions:
[0008] The present invention provides a method for preparing a catalyst for decomposing hydrogen cyanide by using wastewater containing copper ions, comprising the following steps:
[0009] After adjusting the pH value of the copper ion-containing wastewater to 3-10, the wastewater is mixed with nano-alumina and dried to obtain a precursor material;
[0010] The precursor material is calcined to obtain the catalyst.
[0011] Preferably, the mass concentration of copper ions in the copper ion-containing wastewater is 5 to 15%.
[0012] Preferably, the usage ratio of the nano-alumina and the copper ion-containing wastewater is 1kg:0.1-1.5L.
[0013] Preferably, the particle size of the nano-alumina is 10-30 nm, and the specific surface area is ≥230 m 2 / g.
[0014] Preferably, the mixing is carried out under stirring, and the stirring time is 10 to 15 hours.
[0015] Preferably, the drying method is rotary evaporation; the temperature of the rotary evaporation is 60 to 90° C., the pressure is -0.08 to -0.1 MPa, and the rotation speed is 30 to 120 rpm.
[0016] Preferably, the calcination temperature is 450-550° C., the heating rate to the calcination temperature is 5-10° C. / min, and the holding time is 3-3.5 h.
[0017] Preferably, the catalyst comprises a nano-alumina carrier and copper oxide supported on the nano-alumina carrier.
[0018] Preferably, the copper oxide loading mass percentage is 1 to 30% based on the mass percentage of copper.
[0019] Preferably, the particle size of the copper oxide is 10 to 200 nm.
[0020] The present invention provides a method for preparing a catalyst for decomposing hydrogen cyanide by using wastewater containing copper ions, comprising the following steps: adjusting the pH value of the wastewater containing copper ions to 3 to 10, mixing with nano-alumina, and drying to obtain a precursor material; and calcining the precursor material to obtain the catalyst. The present invention adopts an impregnation method to absorb copper ions in the wastewater containing copper. Nano-alumina has a large specific surface area and good adsorption performance, can quickly absorb copper ions from the wastewater, is simple to operate, and is easy to scale up industrially. The catalyst prepared by the present invention using nano-alumina to absorb copper ions in the wastewater containing copper has a good catalytic effect on hydrogen cyanide, can completely convert hydrogen cyanide in industrial waste gas at 225°C, and has extremely strong stability. BRIEF DESCRIPTION OF THE DRAWINGS
[0021] Figure 1 The catalytic activity diagram of the catalyst obtained in Example 1 to hydrogen cyanide;
[0022] Figure 2 This is a diagram showing the catalytic activity of the catalyst obtained in Example 2 towards hydrogen cyanide. DETAILED DESCRIPTION
[0023] The present invention provides a method for preparing a catalyst for decomposing hydrogen cyanide by using wastewater containing copper ions, comprising the following steps:
[0024] After adjusting the pH value of the copper ion-containing wastewater to 3-10, the wastewater is mixed with nano-alumina and dried to obtain a precursor material;
[0025] The precursor material is calcined to obtain the catalyst.
[0026] In the present invention, unless otherwise specified, all preparation raw materials are commercially available products well known to those skilled in the art.
[0027] The present invention adjusts the pH value of copper ion-containing wastewater to 3-10, mixes it with nano-alumina, and dries it to obtain a precursor material.
[0028] The present invention has no special limitation on the source of the wastewater containing copper ions, and it can be used by those skilled in the art. In the present invention, the reagent used for adjusting the pH value is preferably a sodium hydroxide solution. The present invention has no special limitation on the concentration and dosage of the sodium hydroxide solution, and it can obtain the required pH value. In the present invention, the adsorption of copper ions by nano-alumina can be promoted by adjusting the pH value, and the destruction of the nano-alumina structure can be avoided.
[0029] In the present invention, the mass concentration of copper ions in the copper ion-containing wastewater is preferably 5-15%.
[0030] In the present invention, the particle size of the nano-alumina is preferably 10 to 30 nm, more preferably 20 to 25 nm; the specific surface area is preferably ≥ 230 m 2 In the present invention, the dosage ratio of the nano-alumina to the wastewater containing copper ions is preferably 1kg: 0.1-1.5L, and more preferably 1kg: 0.5-1.0L.
[0031] In the present invention, the mixing is preferably carried out under stirring conditions, and the stirring time is preferably 10 to 15 hours; the stirring is preferably carried out at room temperature.
[0032] In the present invention, the drying method is preferably rotary evaporation; the temperature of the rotary evaporation is preferably 60-90°C, more preferably 80°C; the pressure is preferably -0.08 to -0.1 MPa; the rotation speed is preferably 30-120rpm, more preferably 50-100rpm, and more preferably 60-80rpm.
[0033] After obtaining the precursor material, the present invention calcines the precursor material to obtain the catalyst.
[0034] In the present invention, the calcination temperature is preferably 450-550°C, more preferably 500°C, the heating rate to the calcination temperature is preferably 5-10°C / min, and the holding time is preferably 3-3.5h. In the present invention, the calcination is preferably carried out in a muffle furnace under air atmosphere.
[0035] In the present invention, after the water is drained by rotary evaporation, copper is loaded on the nano-alumina carrier in the form of hydroxide or salt. Further, the copper-containing compound is converted into copper oxide by roasting, and can be closely combined with the nano-alumina carrier; in addition, copper can be dispersed on the surface of the nano-alumina in the form of nano-scale copper clusters or single atoms by roasting, further improving its catalytic decomposition ability.
[0036] After the calcination, the present invention also preferably includes pressing the obtained powder. The present invention has no special limitation on the pressing process, and any method known to those skilled in the art can be used.
[0037] In the present invention, the catalyst preferably comprises a nano-alumina carrier and copper oxide supported on the nano-alumina carrier. In the present invention, the copper oxide loading mass percentage is preferably 1 to 30% based on the mass percentage of copper. In the present invention, the particle size of the copper oxide is preferably 10 to 200 nm.
[0038] In order to further illustrate the present invention, a method for preparing a catalyst for decomposing hydrogen cyanide using wastewater containing copper ions provided by the present invention is described in detail below in conjunction with the accompanying drawings and examples, but they should not be construed as limiting the scope of protection of the present invention.
[0039] Example 1
[0040] Take 1L of wastewater containing copper ions (wherein the mass concentration of copper ions is 10%), add sodium hydroxide solution to adjust the pH value of the wastewater to 6-7;
[0041] Then add 1kg of nano-alumina (particle size 20nm, specific surface area 240m 2 / g), stirred for 10 h, and then subjected to rotary evaporation, wherein the conditions for rotary evaporation are: rotary evaporation temperature is 80° C., pressure is -0.1 MPa, and rotation speed is 80 rpm, to obtain a precursor material;
[0042] The obtained precursor material is placed in a muffle furnace under an air atmosphere, heated to 500°C at a heating rate of 5°C / min for calcination, and kept warm for 3 hours. The obtained powder is pressed into shape to obtain the catalyst, wherein the mass percentage of copper oxide in the catalyst is 10% based on the mass percentage of copper.
[0043] Example 2
[0044] Take 1L of wastewater containing copper ions (wherein the mass concentration of copper ions is 8%), add sodium hydroxide solution to adjust the pH value of the wastewater to 7-8;
[0045] Then add 1kg of nano-alumina (particle size 25nm, specific surface area 250m 2 / g), stirred for 10 h, and then subjected to rotary evaporation, wherein the conditions for rotary evaporation are: rotary evaporation temperature is 90° C., pressure is -0.08 MPa, and rotation speed is 100 rpm, to obtain a precursor material;
[0046] The obtained precursor material is placed in a muffle furnace under an air atmosphere, heated to 550°C at a heating rate of 8°C / min for calcination, and kept warm for 3.5 hours. The obtained powder is pressed into shape to obtain the catalyst, wherein the mass percentage of copper oxide in the catalyst is 8% based on the mass percentage of copper.
[0047] Performance Testing
[0048] Testing the catalytic decomposition performance of the obtained catalyst on hydrogen cyanide;
[0049] The catalyst tablet obtained in Example 1 was crushed, passed through a 40-60 mesh sieve, 30 mg was weighed, placed in a tube furnace, and the temperature was raised by program control to 100-300°C, with a gradient of 25°C and a dwell time of 1 hour to obtain a stable product concentration; the gas flowing through the catalyst was HCN with a concentration of 80 ppm, containing 10% oxygen and nitrogen as a balance gas, and the total gas flow rate was 100 mL / min; the test results obtained are as follows Figure 1 As shown;
[0050] from Figure 1 It can be seen that the prepared catalyst achieves 100% hydrogen cyanide removal efficiency at 225°C and maintains a high conversion rate in the range of 225-300°C.
[0051] The catalyst tablet obtained in Example 2 was crushed, passed through a 40-60 mesh sieve, 30 mg was weighed, placed in a tube furnace, and the temperature was raised by program control to 100-300°C, with a gradient of 25°C and a dwell time of 1 hour to obtain a stable product concentration; the gas flowing through the catalyst was HCN with a concentration of 80 ppm, containing 10% oxygen and nitrogen as a balance gas, and the total gas flow rate was 100 mL / min; the test results obtained are as follows Figure 2 As shown;
[0052] from Figure 2 It can be seen that the prepared catalyst achieves 100% hydrogen cyanide removal efficiency at 225°C and maintains a high conversion rate in the range of 225-300°C.
[0053] Although the above embodiment describes the present invention in detail, it is only a part of the embodiments of the present invention, not all of the embodiments. Other embodiments can be obtained based on this embodiment without creativity, and these embodiments all fall within the protection scope of the present invention.
Claims
1. A method for preparing a catalyst for decomposing hydrogen cyanide using wastewater containing copper ions, characterized in that: The following steps are involved: After adjusting the pH value of the copper ion-containing wastewater to 3-10, the wastewater is mixed with nano-alumina and dried to obtain a precursor material; The precursor material is calcined to obtain the catalyst.
2. The method according to claim 1, characterized in that The mass concentration of copper ions in the copper ion-containing wastewater is 5-15%.
3. The method according to claim 2, characterized in that The dosage ratio of the nano-alumina and the copper ion-containing wastewater is 1kg: 0.1~1.5L。 4. The method according to claim 1 or 3, characterized in that: The particle size of the nano-alumina is 10-30nm, and the specific surface area is ≥230m 2 / g.
5. The method according to claim 1, characterized in that The mixing is carried out under stirring conditions, and the stirring time is 10 to 15 hours.
6. The method according to claim 1, characterized in that The drying method is rotary evaporation; the temperature of the rotary evaporation is 60 to 90° C., the pressure is -0.08 to -0.1 MPa, and the rotation speed is 30 to 120 rpm.
7. The method according to claim 1, characterized in that The calcination temperature is 450-550° C., the heating rate to the calcination temperature is 5-10° C. / min, and the heat preservation time is 3-3.5 hours.
8. The method according to claim 1, characterized in that The catalyst comprises a nano-alumina carrier and copper oxide supported on the nano-alumina carrier.
9. The method according to claim 8, characterized in that Calculated by the mass percentage of copper, the loading mass percentage of the copper oxide is 1 to 30%.
10. The method according to claim 8, characterized in that The particle size of the copper oxide is 10 to 200 nm.
Citation Information
Patent Citations
Catalyst for breaking cyanogen by air oxidation and preparation method thereof
CN106881088A
Removal method of cyanide-containing waste gas
CN107913594A
Heterogeneous nano-copper catalyst as well as preparation method and application thereof
CN113262786A
Core-shell structured catalyst, preparation method thereof and method for treating industrial tail gas
US11247197B1
Method for removing cyanide compounds from wastewater
WO2016120394A1
Cited By
Resource application method of zeolite-based material with two-stage synergism of heavy metal adsorption and antibiotic catalytic degradation