Carbon-coated lanthanum cobalt oxide heterojunction nano-catalyst as well as preparation method and application thereof

By preparing carbon-coated lanthanum-cobalt oxide heterojunction nanocatalysts, the problem of insufficient catalytic activity and stability of cobalt-based nanocatalysts in activating persulfate to degrade organic pollutants was solved, and efficient and long-lasting degradation of organic pollutants was achieved. Effect.

CN118767927APending Publication Date: 2024-10-15HUNAN UNIV

Patent Information

Application Number
CN202410839126.1
Authority / Receiving Office
CN · China
Patent Type
Applications(China)
Current Assignee / Owner
Filing Date
2024-06-26
Publication Date
2024-10-15

AI Technical Summary

Technical Problem

Existing cobalt-based nanocatalysts have problems such as low catalytic activity, poor stability, metal leakage and low electron transfer efficiency when activating persulfate to degrade organic pollutants, and cannot effectively and quickly degrade organic pollutants in complex water bodies.

Method used

The preparation method of carbon-coated lanthanum-cobalt oxide heterojunction nanocatalyst is used to form a bimetallic organic compound through the solvothermal reaction of a mixed solution of terephthalic acid and N,N-dimethylformamide with lanthanum salt and cobalt salt. The precursor is framed and calcined in an air atmosphere to prepare a carbon-coated lanthanum cobalt oxide heterojunction nanocatalyst. The interaction between La-O-Co asymmetric active units and amorphous carbon is used to regulate the electronic structure and interface electron transfer.

Benefits of technology

It improves the catalytic activity, degradation efficiency and stability of the catalyst, reduces the leaching of metal ions, and forms a mesoporous structure in which nanoparticles are uniformly stacked and arranged, adapting to the catalytic needs of complex environments and achieving efficient degradation of organic pollutants.

✦ Generated by Eureka AI based on patent content.

Smart Images

  • Figure CN118767927A_ABST
    Figure CN118767927A_ABST
Patent Text Reader

Abstract

The invention discloses a carbon-coated lanthanum cobalt oxide heterojunction nano-catalyst and a preparation method and application thereof, the preparation method comprises the following steps: S1, mixing terephthalic acid and N, N-dimethylformamide to obtain a mixed solution; s2, the mixed solution, lanthanum salt and cobalt salt are mixed, a solvothermal reaction is carried out, a bimetallic organic framework precursor is obtained, and the molar ratio of the lanthanum salt to the cobalt salt is (6-9): (1-4); and S3, in an air atmosphere, calcining the bimetal organic framework precursor to obtain the carbon-coated lanthanum cobalt oxide heterojunction nano-catalyst. The carbon-coated lanthanum cobalt oxide heterojunction nano-catalyst has the advantages of being good in catalytic activity, high in degradation efficiency, good in stability, high in anti-interference performance, low in metal ion leaching rate and the like, has the advantages of being easy and convenient to operate, good in degradation effect, low in cost and the like when being used for treating organic pollutant wastewater, and is suitable for various complex and changeable practical application scenes.
Need to check novelty before this filing date? Find Prior Art

Description

Technical Field

[0001] The invention belongs to the field of advanced oxidation water treatment, and specifically relates to a carbon-coated lanthanum cobalt oxide heterojunction nanocatalyst and a preparation method and application thereof. Background Art

[0002] Persulfate advanced oxidation technology has become a research hotspot in the field of environmental catalysis in recent years due to its strong oxidation ability, low cost and wide application range. Transition metal-activated persulfate homogeneous catalytic reaction has high catalytic efficiency, but faces key technical limitations such as difficulty in metal ion recovery, easy to cause secondary pollution, slow metal circulation kinetics, poor stability and low removal rate of actual complex water bodies. Transition metal-based heterogeneous catalysts are considered to be a good alternative. Among them, cobalt-based nanocatalysts have outstanding effects in activating persulfate to degrade organic pollutants due to their unique electronic structure. However, the catalyst activity of a single metal is low, the prepared catalyst is easy to agglomerate, the active sites are insufficient, and there are problems such as metal leakage and poor stability. It is not enough to meet practical applications and is urgently needed to be further improved to enhance its catalytic performance. Introducing a second metal to prepare a bimetallic catalyst is a potential solution. However, the electron transfer efficiency of the bimetallic catalyst prepared by the existing preparation method is still low, and it is impossible to effectively activate persulfate to efficiently produce active substances and thus quickly degrade organic pollutants. Therefore, how to prepare a catalyst with an electronic structure regulated by a heterogeneous interface, rich mesoporous structure and active sites, high efficiency and lasting stability, and adaptability to complex environments is still a great challenge. Summary of the invention

[0003] The technical problem to be solved by the present invention is to overcome the deficiencies of the prior art and provide a carbon-coated lanthanum cobalt oxide heterojunction nanocatalyst with good catalytic activity, high degradation efficiency, good stability, strong anti-interference ability and low metal ion leaching rate, as well as a preparation method and application thereof.

[0004] In order to solve the above technical problems, the present invention adopts the following technical solutions.

[0005] A method for preparing a carbon-coated lanthanum cobalt oxide heterojunction nanocatalyst comprises the following steps:

[0006] S1, mixing terephthalic acid and N,N-dimethylformamide to obtain a mixed solution;

[0007] S2, mixing the mixed solution obtained in step S1, lanthanum salt and cobalt salt, and performing a solvothermal reaction to obtain a bimetallic organic framework precursor; the molar ratio of the lanthanum salt to the cobalt salt is 6-9:1-4;

[0008] S3. Under air atmosphere, calcining the bimetallic organic framework precursor obtained in step (2) to obtain a carbon-coated lanthanum cobalt oxide heterojunction nanocatalyst.

[0009] The above preparation method is further improved in that the molar ratio of terephthalic acid to lanthanum salt is 5 to 15:8.

[0010] The above preparation method is further improved, in step S2, the temperature of the dissolution heat reaction is 100°C to 150°C, and the time of the dissolution heat reaction is 18h to 30h.

[0011] The above preparation method is further improved, in step S3, the calcination temperature is 700°C to 900°C, the calcination time is 1h to 3h, and the heating rate during the calcination process is 3°C / min to 8°C / min.

[0012] The above preparation method is further improved, in step S1, the ratio of terephthalic acid to N,N-dimethylformamide is 0.831g-2.492g:40mL, the mixing is carried out under stirring conditions, and the stirring speed is 400rpm-600rpm.

[0013] The above preparation method is further improved, in step S2, the lanthanum salt is lanthanum nitrate, the cobalt salt is cobalt nitrate hexahydrate, the mixing is carried out under stirring conditions, the stirring speed is 300rpm~500rpm, and the stirring time is 20min~40min; the bimetallic organic framework precursor also includes the following treatments before use: centrifuging, washing, and drying the bimetallic organic framework precursor; the washing is carried out using N,N-dimethylformamide and methanol, the centrifugal speed is 6000rpm~8000rpm, the centrifugal time is 5min~7min, the drying is carried out under vacuum conditions, the drying temperature is 50℃~80℃, and the drying time is 10h~14h;

[0014] In step S3, the following treatments are further performed after the calcination: the calcined product is washed, centrifuged, and dried; the washing is performed 2 to 3 times with water or ethanol, the centrifugal speed is 6000 rpm to 8000 rpm, the centrifugal time is 5 min to 7 min, the drying is performed under vacuum conditions, the drying temperature is 50° C. to 80° C., and the drying time is 10 h to 14 h.

[0015] As a general technical concept, the present invention also provides a carbon-coated lanthanum cobalt oxide heterojunction nanocatalyst prepared by the above-mentioned preparation method of the carbon-coated lanthanum cobalt oxide heterojunction nanocatalyst.

[0016] As a general technical concept, the present invention also provides an application of the above-mentioned carbon-coated lanthanum cobalt oxide heterojunction nanocatalyst in treating organic pollutants.

[0017] The above application is further improved and includes the following steps: mixing the carbon-coated lanthanum cobalt oxide heterojunction nanocatalyst and water containing organic pollutants, adding persulfate to carry out degradation reaction, and realizing the degradation of organic pollutants in the water; the ratio of the carbon-coated lanthanum cobalt oxide heterojunction nanocatalyst to the water containing organic pollutants is 0.02g~0.15g:1L.

[0018] The above application is further improved, wherein the amount of persulfate added is 0.3 mmol to 1.5 mmol per liter of water containing organic pollutants, the persulfate is potassium hydrogen persulfate, the organic pollutants in the water containing organic pollutants include at least one of antibiotics and dyes, the antibiotic is at least one of carbamazepine, tetracycline hydrochloride and ciprofloxacin, the dye is at least one of rose red B and methylene blue, the concentration of organic pollutants in the water containing organic pollutants is ≤20 mg / L, and the degradation reaction time is ≥5 min.

[0019] Compared with the prior art, the advantages of the present invention are:

[0020] (1) The present invention provides a method for preparing a carbon-coated lanthanum cobalt oxide heterojunction nanocatalyst. First, a mixed solution of terephthalic acid and N,N-dimethylformamide is used as an organic ligand solution, and the molar ratio of lanthanum salt to cobalt salt is adjusted to 6-9:1-4. Lanthanum cobalt metals are efficiently coupled to form a stable lanthanum cobalt bimetallic organic framework structure as a precursor through a solvent thermal reaction; then, the lanthanum cobalt bimetallic organic framework precursor is calcined in an air atmosphere to obtain a carbon-coated lanthanum cobalt oxide heterojunction nanocatalyst. The carbon-coated lanthanum cobalt oxide heterojunction nanocatalyst of the present invention is mainly based on La(OH)3-Co3O4 heterostructure, and its surface is coated with amorphous carbon. On the one hand, by forming La-O-Co asymmetric active units at the grain boundaries, the interaction of 4f-2p-3d orbital hybridization is used to regulate the electronic orbital occupancy and interface electron transfer process of the Co active site, expose more active sites and greatly improve the electron transfer rate, thereby more efficiently activating persulfate to produce free radicals and non-free radical active substances, and achieving the comprehensive effect of high oxidation efficiency, high selectivity and high mineralization rate; on the other hand, the amorphous carbon coated on the periphery not only improves the conductivity of the catalyst, but also greatly reduces the leaching of metal ions during the degradation reaction of organic pollutants, and enhances the stability of the catalyst. In addition, the carbon-coated lanthanum cobalt oxide heterojunction nanocatalyst of the present invention presents a nanoplate layered structure in which nanoparticles are evenly stacked and arranged, and has a mesoporous structure, which is more conducive to the adsorption activation and rapid mass transfer of persulfate and pollutants. The preparation method of the present invention has the advantages of simple process, safe raw materials, low cost, and mass production; the carbon-coated lanthanum cobalt oxide heterojunction nanocatalyst prepared therefrom has the advantages of good catalytic activity, high degradation efficiency, good stability, strong anti-interference ability, and low metal ion leaching rate.

[0021] (2) The present invention also provides an application of a carbon-coated lanthanum cobalt oxide heterojunction nanocatalyst in treating organic pollutants. By directly mixing the carbon-coated lanthanum cobalt oxide heterojunction nanocatalyst and organic pollutant water, and adding persulfate for degradation reaction, the organic pollutants in the water can be effectively degraded. The method has the advantages of simple operation, good degradation effect, low cost, etc., and is suitable for various complex and changeable practical application scenarios. BRIEF DESCRIPTION OF THE DRAWINGS

[0022] Figure 1 SEM images of the carbon-coated lanthanum cobalt oxide heterojunction nanocatalyst (CL-2 / 8) in Example 1 of the present invention, the carbon-coated lanthanum oxide catalyst (CL-0 / 10) in Comparative Example 1, the carbon-coated lanthanum cobalt oxide catalyst (CL-5 / 5) in Comparative Example 2, the carbon-coated lanthanum cobalt oxide catalyst (CL-8 / 2) in Comparative Example 3, and the carbon-coated cobalt oxide catalyst (CL-10 / 0) ​​in Comparative Example 4.

[0023] Figure 2TEM images of the carbon-coated lanthanum cobalt oxide heterojunction nanocatalyst (CL-2 / 8) in Example 1 of the present invention, the carbon-coated lanthanum oxide catalyst (CL-0 / 10) in Comparative Example 1, and the carbon-coated cobalt oxide catalyst (CL-10 / 0) ​​in Comparative Example 4.

[0024] Figure 3 XRD patterns of the carbon-coated lanthanum cobalt oxide heterojunction nanocatalyst (CL-2 / 8) in Example 1 of the present invention, the carbon-coated lanthanum oxide catalyst (CL-0 / 10) in Comparative Example 1, the carbon-coated lanthanum cobalt oxide catalyst (CL-5 / 5) in Comparative Example 2, the carbon-coated lanthanum cobalt oxide catalyst (CL-8 / 2) in Comparative Example 3, and the carbon-coated cobalt oxide catalyst (CL-10 / 0) ​​in Comparative Example 4.

[0025] Figure 4 Isothermal adsorption-desorption curves and pore size distribution diagrams of the carbon-coated lanthanum cobalt oxide heterojunction nanocatalyst (CL-2 / 8) in Example 1 of the present invention, the carbon-coated lanthanum oxide catalyst (CL-0 / 10) in Comparative Example 1, the carbon-coated lanthanum cobalt oxide catalyst (CL-5 / 5) in Comparative Example 2, the carbon-coated lanthanum cobalt oxide catalyst (CL-8 / 2) in Comparative Example 3, and the carbon-coated cobalt oxide catalyst (CL-10 / 0) ​​in Comparative Example 4.

[0026] Figure 5 It is the full XPS spectrum of the carbon-coated lanthanum cobalt oxide heterojunction nanocatalyst (CL-2 / 8) in Example 1 of the present invention, the carbon-coated lanthanum oxide catalyst (CL-0 / 10) in Comparative Example 1, the carbon-coated lanthanum cobalt oxide catalyst (CL-5 / 5) in Comparative Example 2, the carbon-coated lanthanum cobalt oxide catalyst (CL-8 / 2) in Comparative Example 3, and the carbon-coated cobalt oxide catalyst (CL-10 / 0) ​​in Comparative Example 4.

[0027] Figure 6 This is a diagram showing the effects of activating persulfate to degrade carbamazepine in Example 2 of the present invention using carbon-coated lanthanum cobalt oxide heterojunction nanocatalysts (CL-2 / 8), carbon-coated lanthanum oxide catalysts (CL-0 / 10), carbon-coated lanthanum cobalt oxide catalysts (CL-5 / 5), carbon-coated lanthanum cobalt oxide catalysts (CL-8 / 2), and carbon-coated cobalt oxide catalysts (CL-10 / 0).

[0028] Figure 7 The figure shows the effect of activating persulfate to degrade carbamazepine by the carbon-coated lanthanum oxide catalyst in Example 2 of the present invention, which is recorded as (CL-0 / 10(N2)), carbon-coated lanthanum cobalt oxide catalyst (CL-2 / 8(N2)), carbon-coated lanthanum cobalt oxide catalyst (CL-5 / 5(N2)), carbon-coated lanthanum cobalt oxide catalyst (CL-8 / 2(N2)), and carbon-coated cobalt oxide catalyst (CL-10 / 0(N2)).

[0029] Figure 8 This is a comparison chart of the removal effects of persulfate activation for the degradation of tetracycline hydrochloride, ciprofloxacin, Rose Bengal B, and methylene blue in Example 3 of the present invention using the carbon-coated lanthanum cobalt oxide heterojunction nanocatalyst (CL-2 / 8). DETAILED DESCRIPTION

[0030] The present invention is further described below in conjunction with the accompanying drawings and specific preferred embodiments, but the protection scope of the present invention is not limited thereby. The materials and instruments used in the following embodiments are all commercially available.

[0031] Embodiment 1:

[0032] A method for preparing a carbon-coated lanthanum cobalt oxide heterojunction nanocatalyst of the present invention comprises the following steps:

[0033] (1) 1.661 g of terephthalic acid was dissolved in 40 mL of N,N-dimethylformamide and stirred vigorously at a stirring speed of 500 rpm until the terephthalic acid was completely dissolved to obtain a mixed solution.

[0034] (2) 0.582 g of cobalt nitrate hexahydrate and 2.6 g of lanthanum nitrate (chemical formula: La(NO3)3) were dissolved in the mixed solution obtained in step (1), and the mixture was stirred evenly at a stirring speed of 400 rpm for 30 min to obtain a clear solution; the clear solution was transferred to a 100 mL polytetrafluoroethylene-lined autoclave, and a solvent thermal reaction was carried out at 120°C for 24 h. After the reaction was completed and naturally cooled, the reaction product was collected by centrifugation at a speed of 7000 rpm for 6 min, washed twice with N,N-dimethylformamide solvent, and then washed once with methanol solvent. After centrifugation and collection in the same manner, it was dried in a vacuum drying oven at 60°C for 12 h to obtain a bimetallic organic framework precursor.

[0035] (3) The bimetallic organic framework precursor powder obtained in step (2) is loaded into an alumina crucible with a lid, placed in a tube furnace, and heated to 800°C at a heating rate of 5°C / min for calcination in a static air atmosphere, and kept at 800°C for 2 hours. After the tube furnace is cooled to room temperature, it is taken out and ground; the ground product is washed three times with deionized water, collected by centrifugation at a speed of 7000 rpm for 6 minutes, and dried in a vacuum drying oven at 60°C for 12 hours to obtain a carbon-coated lanthanum cobalt oxide heterojunction nanocatalyst, which is recorded as CL-2 / 8.

[0036] Comparative Example 1:

[0037] A carbon-coated lanthanum oxide catalyst, the preparation method of which is basically the same as the preparation method of the carbon-coated lanthanum cobalt oxide heterojunction nanocatalyst (CL-2 / 8) in Example 1, the only difference being that in step (2), no cobalt nitrate hexahydrate is added, and the amount of lanthanum nitrate used is 3.25 g; the prepared carbon-coated lanthanum oxide catalyst is recorded as CL-0 / 10.

[0038] Comparative Example 2:

[0039] A carbon-coated lanthanum cobalt oxide catalyst, the preparation method of which is basically the same as the preparation method of the carbon-coated lanthanum cobalt oxide heterojunction nanocatalyst (CL-2 / 8) in Example 1, the only difference being that in step (2), the amount of cobalt nitrate hexahydrate is 1.455 g, and the amount of lanthanum nitrate is 1.625 g; the prepared carbon-coated lanthanum cobalt oxide catalyst is recorded as CL-5 / 5.

[0040] Comparative Example 3:

[0041] A carbon-coated lanthanum cobalt oxide catalyst, the preparation method of which is basically the same as the preparation method of the carbon-coated lanthanum cobalt oxide heterojunction nanocatalyst (CL-2 / 8) in Example 1, the only difference being that in step (2), the amount of cobalt nitrate hexahydrate is 2.328 g, and the amount of lanthanum nitrate is 0.65 g; the prepared carbon-coated lanthanum cobalt oxide catalyst is recorded as CL-8 / 2.

[0042] Comparative Example 4:

[0043] A carbon-coated cobalt oxide catalyst, the preparation method of which is basically the same as the preparation method of the carbon-coated lanthanum cobalt oxide heterojunction nanocatalyst (CL-2 / 8) in Example 1, the only difference being that in step (2), no lanthanum nitrate is added, and the amount of cobalt nitrate hexahydrate used is 2.91 g; the obtained carbon-coated cobalt oxide catalyst is recorded as CL-10 / 0.

[0044] Comparative Example 5:

[0045] A carbon-coated lanthanum oxide catalyst, the preparation method of which is basically the same as the preparation method of the carbon-coated lanthanum oxide catalyst (CL-0 / 10) in Comparative Example 1, the only difference being that in step (3), the calcination atmosphere is nitrogen; the obtained carbon-coated lanthanum oxide catalyst is recorded as CL-0 / 10 (N2).

[0046] Comparative Example 6:

[0047] A carbon-coated lanthanum cobalt oxide catalyst, the preparation method of which is basically the same as the preparation method of the carbon-coated lanthanum cobalt oxide heterojunction nanocatalyst (CL-2 / 8) in Example 1, with the only difference being that in step (3), the calcination atmosphere is nitrogen; the obtained carbon-coated lanthanum cobalt oxide catalyst is recorded as CL-2 / 8 (N2).

[0048] Comparative Example 7:

[0049] A carbon-coated lanthanum cobalt oxide catalyst, the preparation method of which is basically the same as the preparation method of the carbon-coated lanthanum cobalt oxide catalyst (CL-5 / 5) in Comparative Example 2, with the only difference being that in step (3), the calcination atmosphere is nitrogen; the obtained carbon-coated lanthanum cobalt oxide catalyst is recorded as CL-5 / 5 (N2).

[0050] Comparative Example 8:

[0051] A carbon-coated lanthanum cobalt oxide catalyst, the preparation method of which is basically the same as the preparation method of the carbon-coated lanthanum cobalt oxide catalyst (CL-8 / 2) in Comparative Example 3, with the only difference being that in step (3), the calcination atmosphere is nitrogen; the obtained carbon-coated lanthanum cobalt oxide catalyst is recorded as CL-8 / 2 (N2).

[0052] Comparative Example 9:

[0053] A carbon-coated cobalt oxide catalyst, whose preparation method is basically the same as the preparation method of the carbon-coated cobalt oxide catalyst (CL-8 / 2) in Comparative Example 4, with the only difference being that in step (3), the calcination atmosphere is nitrogen; the obtained carbon-coated cobalt oxide catalyst is recorded as CL-10 / 0 (N2).

[0054] Figure 1 SEM images of the carbon-coated lanthanum cobalt oxide heterojunction nanocatalyst (CL-2 / 8) in Example 1 of the present invention, the carbon-coated lanthanum oxide catalyst (CL-0 / 10) in Comparative Example 1, the carbon-coated lanthanum cobalt oxide catalyst (CL-5 / 5) in Comparative Example 2, the carbon-coated lanthanum cobalt oxide catalyst (CL-8 / 2) in Comparative Example 3, and the carbon-coated cobalt oxide catalyst (CL-10 / 0) ​​in Comparative Example 4. Figure 1 Among them, (A) is CL-2 / 8, (B) is CL-0 / 10, (C) is CL-5 / 5, (D) is CL-8 / 2, and (E) is CL-10 / 0. Figure 1 It can be seen that the morphology of CL-2 / 8, CL-5 / 5, and CL-8 / 2 is a layered structure with uniformly stacked nanoparticles, which has good structural stability and anti-breakage properties; CL-0 / 10 is randomly stacked with nanoparticles without forming a layered structure; CL-10 / 0 presents a continuous and disordered structure with large pores, which indicates that the catalyst prepared with only a single metal precursor does not have a specific layered structure, while the intrinsic interaction of the bimetallic precursors can ensure that the morphology of the catalyst after high-temperature calcination presents a hierarchical arrangement structure.

[0055] Figure 2TEM images of the carbon-coated lanthanum cobalt oxide heterojunction nanocatalyst (CL-2 / 8) in Example 1 of the present invention, the carbon-coated lanthanum oxide catalyst (CL-0 / 10) in Comparative Example 1, and the carbon-coated cobalt oxide catalyst (CL-10 / 0) ​​in Comparative Example 4. Figure 2 Among them, (A) and (B) are CL-2 / 8, (C) and (D) are CL-0 / 10, and (E) and (F) are CL-10 / 0. Figure 2 It can be seen that CL-2 / 8, CL-0 / 10, and CL-10 / 0 all present a certain crystal particle structure, with nanoparticles stacked or continuously arranged; CL-2 / 8 exhibits a heterogeneous interface structure of La(OH)3 and Co3O4 composite, that is, the (101) crystal plane with a crystal plane spacing of 0.311nm and the (311) crystal plane with a crystal plane spacing of 0.244nm are exposed, respectively, and an amorphous carbon layer is coated on the periphery; while CL-0 / 10 and CL-10 / 0 expose the (101) crystal plane with a crystal plane spacing of 0.311nm and the (311) crystal plane with a crystal plane spacing of 0.244nm, respectively, corresponding to the synthesis of crystalline La(OH)3 and Co3O4, respectively.

[0056] Figure 3 The XRD patterns of the carbon-coated lanthanum cobalt oxide heterojunction nanocatalyst (CL-2 / 8) in Example 1 of the present invention, the carbon-coated lanthanum oxide catalyst (CL-0 / 10) in Comparative Example 1, the carbon-coated lanthanum cobalt oxide catalyst (CL-5 / 5) in Comparative Example 2, the carbon-coated lanthanum cobalt oxide catalyst (CL-8 / 2) in Comparative Example 3, and the carbon-coated cobalt oxide catalyst (CL-10 / 0) ​​in Comparative Example 4 are shown in FIG. Figure 3 It can be seen that CL-2 / 8, CL-5 / 5, and CL-8 / 2 all show sharp diffraction peaks, which indicates that these catalysts have good crystal structures. In addition, the diffraction patterns of CL-0 / 10 and CL-10 / 0 correspond to the standard PDF cards of La(OH)3 (PDF#86-1481) and Co3O4 (PDF#74-2120), respectively; the diffraction peaks of CL-2 / 8, CL-5 / 5, and CL-8 / 2 show a mixed composition of the two, further indicating that a heterogeneous structure of lanthanum cobalt oxide is formed in the catalyst.

[0057] Figure 4 Isothermal adsorption-desorption curves and pore size distribution diagrams of the carbon-coated lanthanum cobalt oxide heterojunction nanocatalyst (CL-2 / 8) in Example 1 of the present invention, the carbon-coated lanthanum oxide catalyst (CL-0 / 10) in Comparative Example 1, the carbon-coated lanthanum cobalt oxide catalyst (CL-5 / 5) in Comparative Example 2, the carbon-coated lanthanum cobalt oxide catalyst (CL-8 / 2) in Comparative Example 3, and the carbon-coated cobalt oxide catalyst (CL-10 / 0) ​​in Comparative Example 4. Figure 4In the figure, (A) is the isothermal adsorption-desorption curve, and (B) is the pore size distribution diagram. Figure 4 As can be seen from (A), the adsorption and desorption isotherms of N2 show significant consistency with the properties of the type III isotherm and H3 hysteresis loop under the IUPAC classification, which indicates that the prepared catalyst not only has a mesoporous structure, but also has a large number of narrow pores. Figure 4 As can be seen in (B), most of the pore sizes in CL-2 / 8, CL-5 / 5, and CL-8 / 2 are concentrated in the range of 0-50nm, which corresponds to the pore size of the mesoporous structure; while CL-10 / 0 only has macropores, without mesopores and micropores. The carbon-coated lanthanum cobalt oxide heterojunction nanocatalyst (CL-2 / 8) of the present invention has the best layered structure, the largest number of mesopores and the corresponding maximum pore adsorption capacity, which is conducive to the adsorption and activation of PMS on the catalyst surface and the oxidation and degradation of organic pollutants by active substances near the catalyst surface, thereby showing high organic pollutant removal efficiency and reaction kinetics.

[0058] Figure 5 The full XPS spectra of the carbon-coated lanthanum cobalt oxide heterojunction nanocatalyst (CL-2 / 8) in Example 1 of the present invention, the carbon-coated lanthanum oxide catalyst (CL-0 / 10) in Comparative Example 1, the carbon-coated lanthanum cobalt oxide catalyst (CL-5 / 5) in Comparative Example 2, the carbon-coated lanthanum cobalt oxide catalyst (CL-8 / 2) in Comparative Example 3, and the carbon-coated cobalt oxide catalyst (CL-10 / 0) ​​in Comparative Example 4. Figure 5 It can be seen that CL-0 / 10 is composed of La3d, O1s and C1s, CL-10 / 0 is composed of Co2p, O1s and C1s, and CL-2 / 8, CL-5 / 5 and CL-8 / 2 are all composed of La3d, Co2p, O1s and C1s. The results of the XPS full spectrum are consistent with the characterization results of SEM, TEM and XRD, which indicates the successful preparation of carbon-coated lanthanum cobalt oxide heterojunction nanocatalysts.

[0059] Embodiment 2:

[0060] An application of the carbon-coated lanthanum cobalt oxide heterojunction nanocatalyst of the present invention in treating organic pollutants, specifically using the carbon-coated lanthanum cobalt oxide heterojunction nanocatalyst to degrade carbamazepine in water, comprising the following steps:

[0061] The carbon-coated lanthanum cobalt oxide heterojunction nanocatalyst (CL-2 / 8) in Example 1, the carbon-coated lanthanum oxide catalyst (CL-0 / 10) in Comparative Example 1, the carbon-coated lanthanum cobalt oxide catalyst (CL-5 / 5) in Comparative Example 2, the carbon-coated lanthanum cobalt oxide catalyst (CL-8 / 2) in Comparative Example 3, the carbon-coated cobalt oxide catalyst (CL-10 / 0) ​​in Comparative Example 4, the carbon-coated lanthanum oxide catalyst (CL-0 / 10 (N2)) in Comparative Example 5, the carbon-coated lanthanum cobalt oxide catalyst (CL-2 / 8 (N2)) in Comparative Example 6, the carbon-coated lanthanum cobalt oxide catalyst (CL-7) in Comparative Example 7, and the carbon-coated lanthanum cobalt oxide catalyst (CL-8 / 2) in Comparative Example 3. 10 mg of each of the catalyst (CL-5 / 5(N2)), the carbon-coated lanthanum cobalt oxide catalyst (CL-8 / 2(N2)) in Comparative Example 8, and the carbon-coated cobalt oxide catalyst (CL-10 / 0(N2)) in Comparative Example 9 were added to 100 mL of a carbamazepine (CBZ) solution with a concentration of 10 mg / L and a pH of 6.40, and 1 mL of a 100 mM potassium persulfate solution was added and mixed evenly so that the concentration of potassium persulfate in the reaction system was 1 mM. The catalytic reaction was carried out at room temperature and a rotation speed of 400 rpm for 15 min to achieve the degradation of carbamazepine.

[0062] Figure 6 The effect diagram of the carbon-coated lanthanum cobalt oxide heterojunction nanocatalyst (CL-2 / 8), carbon-coated lanthanum oxide catalyst (CL-0 / 10), carbon-coated lanthanum cobalt oxide catalyst (CL-5 / 5), carbon-coated lanthanum cobalt oxide catalyst (CL-8 / 2), and carbon-coated cobalt oxide catalyst (CL-10 / 0) ​​in Example 2 of the present invention on the activation of persulfate to degrade carbamazepine. Figure 6 It can be seen that the removal rate of carbon-coated lanthanum cobalt oxide heterojunction nanocatalyst (CL-2 / 8) for activating PMS to degrade carbamazepine within 10 minutes is 99.5%, while the removal rates of CL-0 / 10, CL-5 / 5, CL-8 / 2, and CL-10 / 0 for activating PMS to degrade carbamazepine within 10 minutes are 32%, 76.5%, 60.5%, and 19.6%, respectively. It can be seen that the carbon-coated lanthanum cobalt oxide heterojunction nanocatalyst (CL-2 / 8) of the present invention has the best degradation efficiency and reaction kinetics, which is mainly attributed to the mesoporous structure and abundant active sites provided by its hierarchical arrangement structure, and the formed lanthanum cobalt oxide heterostructure promotes interfacial electron transfer. Specifically, on the one hand, the CL-2 / 8 catalyst has the best morphology structure, and has a higher specific surface area to expose more active sites for catalytic reaction. On the other hand, the appropriate metal ratio makes the proportion of active Co (II) on the surface of the CL-2 / 8 catalyst larger, so that PMS can be efficiently activated to produce active oxygen species and then quickly degrade carbamazepine.

[0063] Figure 7The effect diagram of the carbon-coated lanthanum oxide catalyst (CL-0 / 10(N2)), carbon-coated lanthanum cobalt oxide catalyst (CL-2 / 8(N2)), carbon-coated lanthanum cobalt oxide catalyst (CL-5 / 5(N2)), carbon-coated lanthanum cobalt oxide catalyst (CL-8 / 2(N2)), and carbon-coated cobalt oxide catalyst (CL-10 / 0(N2)) in Example 2 of the present invention on the activation of persulfate to degrade carbamazepine. Figure 7 It can be seen that within 20 minutes, the removal rates of carbamazepine by CL-0 / 10(N2), CL-2 / 8(N2), CL-5 / 5(N2), CL-8 / 2(N2) and CL-10 / 0(N2) were between 17% and 60%, which were significantly lower than those of the catalysts prepared by calcination under air conditions. This indicates that the calcination atmosphere has a great influence on the structure and catalytic activity of the catalyst, and the catalysts calcined under nitrogen atmosphere are not ideal for the degradation of organic pollutants.

[0064] Embodiment 3:

[0065] An application of the carbon-coated lanthanum cobalt oxide heterojunction nanocatalyst of the present invention in treating organic pollutants, specifically using the carbon-coated lanthanum cobalt oxide heterojunction nanocatalyst to degrade tetracycline hydrochloride (TC), ciprofloxacin (CIP), rose bengal B (RhB) and methylene blue (MB) in water, comprising the following steps:

[0066] Take 4 portions of 10 mg of the carbon-coated lanthanum cobalt oxide heterojunction nanocatalyst (CL-2 / 8) in Example 1 and add them to 100 mL of tetracycline hydrochloride solution, ciprofloxacin solution, Rose Bengal B solution and methylene blue solution, respectively, wherein the concentration of the tetracycline hydrochloride solution is 10 mg / L, the concentration of the ciprofloxacin solution is 10 mg / L, the concentration of the Rose Bengal B solution is 20 mg / L, and the concentration of the methylene blue solution is 20 mg / L. 1 mL of 100 mM potassium persulfate solution is added and mixed evenly so that the concentration of potassium persulfate in the reaction system is 1 mM. The catalytic reaction is carried out at room temperature and a rotation speed of 400 rpm for 15 min to achieve the degradation of tetracycline hydrochloride, ciprofloxacin, Rose Bengal B and methylene blue.

[0067] Figure 8 This is a comparison chart of the removal effects of persulfate activated by carbon-coated lanthanum cobalt oxide heterojunction nanocatalyst (CL-2 / 8) in Example 3 of the present invention on the degradation of tetracycline hydrochloride, ciprofloxacin, Rose Bengal B, and methylene blue. Figure 7It can be seen that within 15 minutes, the carbon-coated lanthanum cobalt oxide heterojunction nanocatalyst (CL-2 / 8) completely degraded ciprofloxacin and Rose Bengal B, and the removal rates of tetracycline hydrochloride and methylene blue were 90% and 86%, respectively. It can be seen that the carbon-coated lanthanum cobalt oxide heterojunction nanocatalyst (CL-2 / 8) of the present invention has excellent ability to activate PMS to degrade organic pollutants, shows wide applicability, and has certain practical application potential.

[0068] The above is only a preferred embodiment of the present invention and does not limit the present invention in any form. Although the present invention has been disclosed as above in the preferred embodiment, it is not used to limit the present invention. Any technician familiar with the art can make many possible changes and modifications to the technical solution of the present invention by using the methods and technical contents disclosed above without departing from the spirit and technical solution of the present invention, or modify it into an equivalent embodiment of equivalent changes. Therefore, any simple modification, equivalent replacement, equivalent change and modification made to the above embodiments according to the technical essence of the present invention without departing from the content of the technical solution of the present invention, still fall within the scope of protection of the technical solution of the present invention.

Claims

1. A method for preparing a carbon-coated lanthanum cobalt oxide heterojunction nanocatalyst, characterized in that: The following steps are involved: S1, mixing terephthalic acid and N,N-dimethylformamide to obtain a mixed solution; S2, mixing the mixed solution obtained in step S1, lanthanum salt and cobalt salt, and performing a solvothermal reaction to obtain a bimetallic organic framework precursor; the molar ratio of the lanthanum salt to the cobalt salt is 6-9:1-4; S3. Under air atmosphere, calcining the bimetallic organic framework precursor obtained in step (2) to obtain a carbon-coated lanthanum cobalt oxide heterojunction nanocatalyst.

2. The method for preparing the carbon-coated lanthanum cobalt oxide heterojunction nanocatalyst according to claim 1, characterized in that: The molar ratio of terephthalic acid to lanthanum salt is 5-15:

8.

3. The method for preparing the carbon-coated lanthanum cobalt oxide heterojunction nanocatalyst according to claim 2, characterized in that: In step S2, the temperature of the dissolution heat reaction is 100°C to 150°C, and the time of the dissolution heat reaction is 18h to 30h.

4. The method for preparing the carbon-coated lanthanum cobalt oxide heterojunction nanocatalyst according to claim 3, characterized in that: In step S3, the calcination temperature is 700°C to 900°C, the calcination time is 1h to 3h, and the heating rate during the calcination process is 3°C / min to 8°C / min.

5. The method for preparing the carbon-coated lanthanum cobalt oxide heterojunction nanocatalyst according to any one of claims 1 to 4, characterized in that: In step S1, the ratio of terephthalic acid to N,N-dimethylformamide is 0.831 g to 2.492 g: 40 mL, and the mixing is performed under stirring at a speed of 400 rpm to 600 rpm.

6. The method for preparing the carbon-coated lanthanum cobalt oxide heterojunction nanocatalyst according to any one of claims 1 to 4, characterized in that: In step S2, the lanthanum salt is lanthanum nitrate, the cobalt salt is cobalt nitrate hexahydrate, the mixing is carried out under stirring conditions, the stirring speed is 300rpm~500rpm, and the stirring time is 20min~40min; the bimetallic organic framework precursor also includes the following treatments before use: centrifuging, washing, and drying the bimetallic organic framework precursor; the washing is carried out using N,N-dimethylformamide and methanol, the centrifugal speed is 6000rpm~8000rpm, the centrifugal time is 5min~7min, the drying is carried out under vacuum conditions, the drying temperature is 50℃~80℃, and the drying time is 10h~14h; In step S3, the following treatments are further performed after the calcination: the calcined product is washed, centrifuged, and dried; the washing is performed 2 to 3 times with water or ethanol, the centrifugal speed is 6000 rpm to 8000 rpm, the centrifugal time is 5 min to 7 min, the drying is performed under vacuum conditions, the drying temperature is 50° C. to 80° C., and the drying time is 10 h to 14 h.

7. A carbon-coated lanthanum cobalt oxide heterojunction nanocatalyst prepared by the method for preparing a carbon-coated lanthanum cobalt oxide heterojunction nanocatalyst as claimed in any one of claims 1 to 6.

8. Use of the carbon-coated lanthanum cobalt oxide heterojunction nanocatalyst as claimed in claim 7 in treating organic pollutants.

9. The use according to claim 8, characterized in that: The following steps are involved: The carbon-coated lanthanum cobalt oxide heterojunction nanocatalyst and water containing organic pollutants are mixed, and persulfate is added to carry out a degradation reaction to achieve the degradation of organic pollutants in the water; the ratio of the carbon-coated lanthanum cobalt oxide heterojunction nanocatalyst to the water containing organic pollutants is 0.02g-0.15g:1L.

10. The use according to claim 9, characterized in that: The amount of persulfate added is 0.3mmol to 1.5mmol per liter of water containing organic pollutants, the persulfate is potassium hydrogen persulfate, the organic pollutants in the water containing organic pollutants include at least one of antibiotics and dyes, the antibiotic is at least one of carbamazepine, tetracycline hydrochloride and ciprofloxacin, the dye is at least one of rose red B and methylene blue, the concentration of organic pollutants in the water containing organic pollutants is ≤20mg / L, and the degradation reaction time is ≥5min.

Citation Information

Patent Citations

  • Preparation method of carbon-coated cerium oxide-cobalt heterojunction oxygen evolution electrocatalyst

    CN116876018A

  • MOFs-derived cobalt-based porous carbon material catalyst for catalytic decomposition of ozone and preparation method of MOFs-derived cobalt-based porous carbon material catalyst

    CN117582994A

  • Preparation method and application of Co3O4 / CuO C catalyst

    CN118079920A

  • Porous semiconductor metal oxide complex nanofibers including nanoparticle catalyst functionalized by nano-catalyst included within metal-organic framework, gas sensor and member using the same, and method of manufacturing the same

    US20170003272A1

  • Catalyst for water splitting

    US20220097027A1

Cited By

  • Co and La double-metal co-doped Ti3AlC2 composite material as well as preparation method and application thereof

    CN121467068A

  • Cobalt / lanthanum hydroxide heterojunction loaded porous carbon nanofiber electrocatalyst and preparation method thereof

    CN121484091A