Preparation method of carbon-containing hydrodemetallization catalyst

By using carbon-modified flake pseudo-boehmite and rolling ball forming technology in catalyst preparation, an alumina carrier with a high porous structure is formed, and Ni-Mo is used as the active component, which solves the problems of reduced catalyst activity and metal deposition poisoning. problem, achieving high catalytic activity and stability while improving hydrodemetallization efficiency.

CN118767933AActive Publication Date: 2024-10-15CHINA PETROLEUM & CHEMICAL CORP +1
View PDF 7 Cites 0 Cited by

Patent Information

Application Number
CN202310356868.4
Authority / Receiving Office
CN · China
Patent Type
Applications(China)
Current Assignee / Owner
Filing Date
2023-04-06
Publication Date
2024-10-15
Estimated Expiration
2043-04-06

AI Technical Summary

Technical Problem

Existing catalysts have problems with activity decline and metal deposition poisoning in the hydrotreating of heavy and residual oils, and the pore structure of conventional alumina carriers is not suitable for the diffusion of macromolecular reactants, resulting in insufficient catalyst activity stability and demetallization capabilities.

Method used

Carbon-modified flaky pseudo-boehmite is prepared by hydrothermal treatment of aluminum nitrate after roasting with an aqueous solution of propylene oxide and polyhydric alcohol. Combined with the rolling ball molding and impregnation steps, an alumina carrier with a high porous structure is formed, and Ni -Mo is the active component, and a hydrodemetallization catalyst with high catalytic activity and anti-fouling ability is prepared.

Benefits of technology

The highly catalytically active site pore structure matching of the catalyst is achieved, the reactant diffusion capacity and the catalyst's resistance to metal deposition are improved, and the activity stability and demetallization efficiency of the catalyst are ensured.

✦ Generated by Eureka AI based on patent content.

Smart Images

  • Figure CN118767933A_ABST
    Figure CN118767933A_ABST
Patent Text Reader

Abstract

The invention discloses a preparation method of a carbon-containing hydrodemetallization catalyst, which comprises the following steps: (1) roasting, crushing and screening aluminum nitrate, mixing the screened material with an aqueous solution containing epoxypropane and polyol, carrying out hydrothermal treatment, and filtering, washing and drying the treated material to obtain carbon-modified flaky pseudo-boehmite P1; (2) mixing pseudo-boehmite P1 and pseudo-boehmite P2 to obtain a mixed material H0, and carrying out rolling ball molding to obtain an alumina carrier precursor S0; (3) mixing S0 with the carbon modified sheet prepared in the step (1), continuously rolling and forming, and drying and roasting the formed material to obtain an alumina carrier; and (4) impregnating the carrier with the active component impregnation liquid, drying, and roasting to obtain the hydrodemetallization catalyst. The hydrodemetallization catalyst prepared by the method has the advantages of large high catalytic activity site pore channel, strong metal impurity capacity and carbon deposition resistance, and high demetallization activity and high activity stability in the residual oil hydrotreating process.
Need to check novelty before this filing date? Find Prior Art

Description

Technical Field

[0001] The invention belongs to the field of catalyst preparation, and specifically relates to a method for preparing a carbon-containing hydrodemetallization catalyst. Background Art

[0002] As crude oil becomes heavier and inferior, oil refining companies are faced with a large number of heavy and residual oil processing and utilization problems. Heavy and residual oil molecules have complex three-dimensional structures. During the catalytic hydrogenation process, heavy oil macromolecules are adsorbed and deposited on the surface or pores of the catalyst, increasing the diffusion resistance in the reaction and causing the apparent activity of the catalyst to decrease. At the same time, heavy and residual oils contain more coke precursors, which will generate coke and deposit in the pores under certain conditions, causing the active center of the catalyst to be poisoned. Therefore, catalysts with larger pore volume and larger pore diameter have strong metal and carbon storage capacity, which can slow down the deactivation of the catalyst and extend the operation cycle of the catalyst.

[0003] Alumina is a commonly used catalyst carrier in the petrochemical industry. It has been the most widely used and largest amount of catalytic carrier due to its good mechanical stability, easy control of specific surface area and pore structure, and low price and availability. However, the pores of conventional alumina carriers are relatively small. In order to meet the needs of heavy and residual oil hydroprocessing, the "pore expansion" method is usually used to improve the pore structure of alumina carriers. On the other hand, during the roasting process, the active metal components easily react with the alumina carrier to form a strong MO-Al bond, causing the active components to form a spinel phase and lose activity, or making the active components unable to be completely sulfided, thereby reducing the activity of the catalyst.

[0004] CN201510191156.7 discloses a heavy oil hydrogenation catalyst and a preparation method thereof. The catalyst comprises an alumina carrier composed of flaky polycrystalline γ-alumina and a hydrogenation active metal. The preparation method of the catalyst is as follows: adding a binder and an extrusion aid to the flaky γ-polycrystalline alumina raw powder, kneading, molding, drying and calcining to obtain an alumina carrier, and loading the active metal on the obtained alumina carrier by a conventional method. The preparation method of the flaky polycrystalline γ-alumina comprises the following steps: (1) mixing an inorganic aluminum salt, a low-carbon alcohol and / or water, and a low-carbon alkylene oxide uniformly to form a gel, and then aging the gel; (2) soaking the gel obtained in step (1) with a low-carbon alcohol, and then drying and calcining; (3) immersing the material obtained in step (2) in ammonia water for closed hydrothermal treatment, solid-liquid separation, and drying to obtain flaky γ-polycrystalline alumina raw powder. This invention adjusts the pore structure of the carrier by adding flaky polycrystalline γ-alumina into the alumina carrier, but the preparation process of flaky polycrystalline γ-alumina is relatively complicated.

[0005] CN104646008A discloses a catalyst for demetallization of inferior heavy oil by hydrodesulfurization and a preparation method thereof. The catalyst uses alumina as a carrier, and group VIII and VIB elements, especially Ni-Mo, as active components. The catalyst has a pore volume of 0.61-0.70 mL / g and a specific surface area of ​​155-200 m 2 / g, and the average pore diameter is 13.0-18.0nm. The preparation method of the catalyst is to treat the carrier particles after forming and calcining with an acid solution with continuously increasing concentration. Although this method can make the average pore diameter of the final catalyst gradually increase along the radial direction of the catalyst particles from the center to the outer surface, this treatment method is difficult to form larger pores on the carrier surface.

[0006] CN105582947A discloses a method for preparing a carbon-containing residue hydrodemetallization catalyst, which comprises the following contents: (1) preparing at least two polyol and / or monosaccharide aqueous solutions of different concentrations, and spraying them on an alumina carrier in order of concentration from high to low, so that the concentration of the polyol and / or monosaccharide forms a gradient distribution from low to high from the outside to the inside on the carrier; (2) subjecting the impregnated alumina carrier to hydrothermal carbonization treatment and drying treatment in a sealed container; (3) using an impregnation solution containing an active metal component to impregnate the carrier of step (2), placing the impregnated wet material in a pressure-resistant container, and introducing ammonia gas for step-by-step treatment; (4) drying the material treated in step (3), and then subjecting it to an oxygen-free high-temperature treatment to obtain a catalyst product. This method improves the activity of the catalyst by regulating the strong interaction between the active metal and the carrier through carbon, but the pore structure of the catalyst is not conducive to the diffusion of macromolecular reactants into the catalyst. Summary of the invention

[0007] In view of the deficiencies in the prior art, the present invention provides a method for preparing a carbon-containing hydrodemetallization catalyst. The hydrodemetallization catalyst prepared by the method has large pores at high catalytic activity sites, strong metal impurity tolerance and carbon deposition resistance, and has high demetallization activity and high activity stability during the residual oil hydroprocessing process.

[0008] The preparation method of the carbon-containing hydrodemetallization catalyst of the present invention comprises the following contents: (1) calcining aluminum nitrate, crushing and screening the calcined material, mixing the screened material with an aqueous solution containing propylene oxide and a polyol, and then performing a hydrothermal treatment. The treated material is filtered, washed, and dried to obtain carbon-modified flaky pseudo-boehmite P1; (2) mixing the carbon-modified flaky pseudo-boehmite P1 and the pseudo-boehmite P2 to obtain a mixed material H0, and then rolling the mixed material into a ball to obtain an alumina carrier precursor S0; (3) mixing the alumina carrier precursor S0 prepared in step (2) with the carbon-modified flaky pseudo-boehmite P1, and continuing to roll the spherical balls to form the shaped materials, and drying and calcining the formed materials to obtain an alumina carrier; (4) The carrier of step (3) is impregnated with the active component impregnation solution, dried and calcined to obtain a hydrodemetallization catalyst.

[0009] In the method of the present invention, the aluminum nitrate in step (1) is calcined at a temperature of 450-650° C., for a time of 4-8 hours, and the crushed particle size is greater than 100 mesh.

[0010] In the method of the present invention, the concentration of propylene oxide solution in the aqueous solution containing propylene oxide and polyols in step (1) is 2.5wt%-12wt%, preferably 4wt%-8wt%, and the mass ratio of the mixed solution to the powder material is 3:1-10:1, preferably 4:1-8:1.

[0011] In the method of the present invention, the polyol described in step (1) is one or a mixture of xylitol, sorbitol, mannitol, and arabitol, and the concentration of the polyol in the aqueous solution containing propylene oxide and the polyol is 10wt%-20wt%.

[0012] In the method of the present invention, the sealed hydrothermal treatment in step (1) is carried out in a sealed container, preferably an autoclave, the hydrothermal treatment temperature is 110-180°C, preferably 120-160°C, the treatment time is 4-8 hours, and the pressure in the sealed container during the hydrothermal treatment is autogenous pressure. After the treatment, the material is filtered, washed, and dried, the drying temperature is generally 80-160°C, and the drying time is 4-8 hours.

[0013] In the method of the present invention, the pseudo-boehmite P2 particles described in step (2) are generally in granular form and may be a commercially available product or pseudo-boehmite prepared by methods such as acid precipitation, alkali precipitation, alcohol aluminum hydrolysis, etc., preferably pseudo-boehmite having a pore size greater than 10 nm.

[0014] In the method of the present invention, the mass ratio of the carbon-modified flaky pseudo-boehmite P1 to the pseudo-boehmite P2 in step (2) is 1:4-2:3. The ball forming is carried out in a turntable forming machine, and the rotating operating conditions of the turntable forming machine are: the inclination angle of the turntable is 40-70º, the rotation speed of the turntable is 10-30rpm; the forming time of the material in the turntable is 10-120min. The radius of the alumina carrier precursor S0 is 0.4r-0.8r, r is the radius of the alumina carrier. During the ball forming process, an aqueous solution containing a gelling agent is sprayed into the material; the aqueous solution containing a gelling agent is one or a mixture of aqueous solutions of nitric acid, phosphoric acid, oxalic acid, and acetic acid, and the mass concentration of the solution is 1%-3%, preferably an aqueous solution of acetic acid.

[0015] In the method of the present invention, the ball forming in step (3) is carried out in a turntable forming machine, and the rotating operating conditions of the turntable forming machine are: the inclination angle of the turntable is 40-70°, the rotation speed of the turntable is 10-30rpm; the forming time of the material in the turntable is 10-120min. During the ball forming process, an aqueous solution containing a peptizing agent is sprayed into the material; the aqueous solution containing a peptizing agent is one or a mixture of aqueous solutions of nitric acid, phosphoric acid, oxalic acid, and acetic acid, and the mass concentration of the solution is 1%-3%, preferably an aqueous solution of acetic acid.

[0016] In the method of the present invention, the drying temperature in step (3) is 60°C-180°C, the drying time is 1-8 hours, preferably 2-6 hours, the calcination is carried out under the protection of an inert atmosphere, preferably under a nitrogen atmosphere, the temperature is 350-800°C, preferably 550-750°C, and the calcination time is 2-6 hours.

[0017] In the method of the present invention, the active component impregnation solution in step (4) is a solution containing a metal of Group VIB and a metal of Group VIII. The metal of Group VIB is Mo or W, preferably Mo, the metal of Group VIII is Ni or Co, preferably Ni, the content of the metal of Group VIB is 5.5-12.5 g / 100 mL in terms of oxide, and the content of the metal of Group VIII is 0.5-4.5 g / 100 mL in terms of oxide. The active component impregnation solution can be an ammonia solution, an aqueous solution or a phosphoric acid solution of the metal of Group VIB and the metal of Group VIII, preferably a phosphoric acid solution containing the metal of Group VIB and the metal of Group VIII; the drying and calcining conditions are well known to those skilled in the art, generally: a drying temperature of 100-160°C, a drying time of 6-10 hours; the calcination is carried out in an inert atmosphere, preferably nitrogen, the calcination temperature is 400-550°C, and the calcination time is 2-6 hours.

[0018] The carbon-containing hydrodemetallization catalyst prepared by the method of the present invention has a carbon content of 1%-5% by weight of the catalyst, a molybdenum oxide content of 5%-10%, a nickel oxide content of 1.3%-3%, and the rest being an aluminum oxide carrier.

[0019] The specific surface area of ​​the carbon-containing hydrodemetallization catalyst prepared by the method of the present invention is 160-280m 2 / g, the pore volume is 0.8-1.0mL / g, the content of pores with a diameter of 10-20nm accounts for 35%-55% of the mesopore volume, the content of pores with a diameter of 50-100nm accounts for 12.5%-25% of the total pore volume, and the content of pores with a diameter greater than 100nm accounts for 10%-20% of the total pore volume.

[0020] The invention discloses an application of the carbon-containing hydrodemetallization catalyst prepared by the method of the invention in a residual oil hydrotreating process.

[0021] Compared with the prior art, the present invention has the following advantages: (1) The present invention places the aluminum oxide compound obtained by roasting aluminum nitrate in a mixed solution of propylene oxide and polyols for hydrothermal treatment to prepare carbon-modified flaky pseudo-boehmite. During the hydrothermal treatment, the aluminum oxide compound undergoes a rehydration reaction in a weakly alkaline solution to form flaky pseudo-boehmite. The preparation process of the flaky pseudo-boehmite is simple, and the acid-base neutralization gelation process in the conventional technology is omitted. During the hydration reaction, the polyol in the solution is uniformly adsorbed on the aluminum oxide compound through the hydrogen bonding between the hydroxyl groups, and the carbon-modified flaky pseudo-boehmite is generated in one step. The polyol makes the structure of the formed carbon-modified flaky pseudo-boehmite more regular and uniform in shape. The pseudo-boehmite flaky grains are accumulated to form a large number of 50-150nm pore structures. The pore structure is solid and not easy to collapse. Using the pseudo-boehmite as a raw material can effectively ensure the macropore content of the later alumina carrier.

[0022] (2) When the alumina carrier is formed, the content of carbon-modified flaky pseudo-boehmite in the mixed material is adjusted so that the pores of the carrier obtained in the end are distributed in a core-shell structure, that is, the shell layer has a larger pore size, a wider pore size, and a higher macropore content, while the core layer is inferior. Since the flaky pseudo-boehmite is carbon-modified, the active metal components in the macropores formed by the accumulation of flaky alumina particles in the final hydrodemetallization catalyst react appropriately with the carrier, and the active metal oxides in this area are easier to sulfidize, and the hydrodemetallization activity is high. At the same time, the high catalytic activity sites of the catalyst are well matched with the pore structure, which is conducive to the diffusion of reactants and the catalyst has a strong ability to resist metal deposition, so that the catalyst has good activity stability. BRIEF DESCRIPTION OF THE DRAWINGS

[0023] FIG. 1 is a SEM image of the carbon-modified flaky pseudo-boehmite P1-1 prepared in Example 1.

[0024] Figure 2 is a SEM image of material P1-6 prepared in Comparative Example 3. Implementation

[0025] The technical scheme and technical effect of the present invention are further described below in conjunction with the embodiments, but are not limited to the following embodiments. In the present invention, wt% represents mass fraction.

[0026] BET method: N2 physical adsorption-desorption was used to characterize the pore structure of the carriers of the embodiment and the comparative example. The specific operation was as follows: The pore structure of the sample was characterized by using an ASAP-2420 N2 physical adsorption-desorption instrument. A small amount of sample was vacuum treated at 300°C for 3-4 hours, and finally the product was placed under liquid nitrogen low temperature (-200°C) for nitrogen adsorption-desorption test. The specific surface area was obtained according to the BET equation, and the pore volume and the distribution rate of pore diameters below 30nm were obtained according to the BJH model.

[0027] Scanning electron microscopy was used to characterize the microstructure of the alumina carrier. The specific operation was as follows: a JSM-7500F scanning electron microscope was used to characterize the microstructure of the carrier, with an accelerating voltage of 5 KV, an accelerating current of 20 µA, and a working distance of 8 mm.

[0028] X-ray diffraction (XRD) analysis was performed on a D / max-2500 fully automatic rotating target X-ray diffractometer produced by Rigaku Corporation, Japan, using a Cu target, Kα radiation source, graphite monochromator, tube voltage of 40 kV, and tube current of 80 mA.

[0029] Mercury intrusion method: A mercury intrusion instrument was used to characterize the pore diameter distribution of the carriers of the embodiment and the comparative example. The specific operation is as follows: The pore distribution of the sample was characterized using the American Micromeritics AutoPore 9500 fully automatic mercury intrusion instrument. After the sample was dried, it was weighed and loaded into the dilatometer, and degassed for 30 minutes under the vacuum conditions given by the instrument, and then loaded with mercury. The dilatometer was then placed in an autoclave and vented. Then, a pressure increase and pressure reduction test was performed. The mercury contact angle was 130°, and the mercury interfacial tension was 0.485N.cm -1 The distribution rate of pores with a diameter of more than 100 nm is measured by mercury intrusion porosimetry.

[0030] The most probable pore size determination: Take the material pore size as the horizontal coordinate and the rate of change of pore volume with pore size as the vertical coordinate to obtain the pore size differential distribution curve. The peak value in the curve is the most probable pore size.

[0031] The GB / T 34099-2017 standard method was used to determine the Ni and V contents in oil products.

[0032] V+Ni removal rate % = (metal V+Ni content of crude oil - metal V+Ni content of product) / metal V+Ni content of crude oil × 100%.

[0033] Relative demetallization rate: Determine the demetallization rate of a certain catalyst, define its relative demetallization rate as 100%, and the impurity removal rate of other catalysts / defined catalyst impurity removal rate × 100% is the relative deimpurity removal rate. Example 1

[0034] (1) Weigh an appropriate amount of aluminum nitrate and place it in a crucible and calcine it at 500℃ for 5.5 hours. The particles were crushed and sieved to obtain particles with a mesh size of 200 or larger. 100 g of the sieved particles were weighed, and 610 g of a mixed solution having a propylene oxide concentration of 5.5 wt% and a xylitol concentration of 15 wt% was added. The mixture was stirred magnetically for 30 minutes, and then the mixture was transferred to an autoclave and sealed and heated at 145°C for 5.3 hours. After cooling, the solid material was filtered, washed, and dried at 120°C for 4 hours to obtain carbon-modified flaky pseudo-boehmite P1-1. The microstructure of the sample was observed to be flaky grain accumulation by scanning electron microscopy. The scanning electron microscopy image is shown in FIG.Figure 1 .

[0035] (2) Weigh 100 g of the carbon-modified pseudo-boehmite P1-1 prepared in step (1) and 235 The mixture was placed in a turntable forming machine and mixed evenly with pseudo-boehmite P2 (prepared by aluminum sulfate-sodium aluminate method, with a maximum pore size of 15 nm). The inclination angle of the turntable was adjusted to 45° and the rotation speed of the turntable was 17 rpm. An acetic acid aqueous solution with a mass concentration of 1% was sprayed onto the material in the turntable through a sprayer. After mixing and contacting, the material was formed in the turntable for 50 minutes to obtain an alumina carrier precursor S0. (3) The carbon-modified flaky pseudo-boehmite P1-1 prepared in step (1) and the alumina carrier precursor S0 prepared in step (2) are placed in a turntable molding machine and mixed thoroughly. The inclination angle of the turntable is adjusted to 35° and the rotation speed of the turntable is 10 rpm. An acetic acid aqueous solution with a mass concentration of 1.3% is sprayed onto the materials in the turntable through a sprayer. After mixed contact, the materials are molded in the turntable for 60 minutes. The obtained materials are dried at 120° C. for 4 hours and calcined at 700° C. in a nitrogen atmosphere for 4 hours to obtain a carbon-containing alumina carrier.

[0036] (4) Weigh 50 g of the carbon-containing alumina carrier prepared in step (3), and impregnate the carrier with a Mo-Ni-P impregnation solution having a molybdenum oxide concentration of 8.5 g / 100 mL and a nickel oxide concentration of 2.3 g / 100 mL by an equal volume impregnation method. The impregnated material is dried at 120° C. for 6 h, and calcined at 500° C. in a nitrogen atmosphere for 4 h to obtain the hydrodemetallization catalyst Cat-1 of the present invention. The catalyst properties are shown in Table 1. Example 2

[0037] Same as Example 1, except that the calcination temperature of aluminum nitrate in step (1) is 600°C and the calcination time is 6 hours. The concentration of propylene oxide in the mixed solution is 6.7wt%, xylitol is replaced by sorbitol, the polyol concentration is 17.5wt%, the solution dosage is 560g, the hydrothermal treatment temperature is 135°C, and the treatment time is 6.5 hours. In step (2), the amount of pseudo-boehmite P2 added is 186g, and the rolling time is 70min. In step (3), the rolling time is 40min, and the hydrodemetallization catalyst Cat-2 of the present invention is obtained. The catalyst properties are shown in Table 1. Example 3

[0038] Same as Example 1, except that the calcination temperature of aluminum nitrate in step (1) is 650°C and the calcination time is 4 hours. The concentration of propylene oxide in the mixed solution is 4.3wt%, xylitol is replaced by mannitol, the concentration of polyol is 12.5wt%, the amount of solution is 750g, the hydrothermal treatment temperature is 155°C, and the treatment time is 4.5 hours. In step (2), the amount of pseudo-boehmite P2 added is 300g, and the rolling time is 60min. In step (3), the rolling time is 50min, and the hydrodemetallization catalyst Cat-3 of the present invention is obtained. The catalyst properties are shown in Table 1. Example 4

[0039] Same as Example 1, except that the calcination temperature of aluminum nitrate in step (1) is 450°C and the calcination time is 7 hours. The concentration of propylene oxide in the mixed solution is 7.8wt%, xylitol is replaced by arabitol, the polyol concentration is 19wt%, the solution dosage is 440g, the hydrothermal treatment temperature is 125°C, and the treatment time is 7.5 hours. In step (2), the amount of pseudo-boehmite P2 added is 168g, and the rolling time is 80min. In step (3), the rolling time is 30min, and the hydrodemetallization catalyst Cat-4 of the present invention is obtained. The catalyst properties are shown in Table 1.

[0040] Comparative Example 1 The same method as in Example 1 was used, except that the propylene oxide in the mixed solution of step (1) was replaced by the same amount of ethylene oxide. After the hydrothermal treatment, no lamellar grains were observed in the microstructure of the material P1-5. A comparative hydrodemetallization catalyst Cat-5 was prepared. The catalyst properties are shown in Table 1.

[0041] Comparative Example 2 The same as Example 1, except that the aluminum nitrate in step (1) is replaced by aluminum sulfate, and the solid material particles are dissolved after hydrothermal treatment, and the product is not separated.

[0042] Comparative Example 3 The same as Example 1, except that the aluminum nitrate in step (1) was replaced by aluminum chloride. No lamellar grains were observed in the microstructure of the material P1-6 after hydrothermal treatment. A comparative hydrodemetallization catalyst Cat-6 was prepared. The catalyst properties are shown in Table 1.

[0043] Comparative Example 4 The same as Example 1, except that in step (1), no polyol was added to the mixed solution. Instead, the polyol was loaded onto the alumina carrier by impregnation to prepare a comparative hydrodemetallization catalyst Cat-7 with the same carbon content. The catalyst properties are shown in Table 1.

[0044] Table 1 Catalyst properties Example 1 Example 2 Example 3 Example 4 Comparative Example 1 Comparative Example 3 Comparative Example 4 catalyst Cat-1 Cat-2 Cat-3 Cat-4 Cat-5 Cat-6 Cat-7 <![CDATA[Specific surface area, m 2 / g]]> 196 182 213 171 183 189 200 Pore ​​volume, mL / g 0.91 0.89 0.92 0.88 0.79 0.81 0.91 <![CDATA[MoO3 content, wt%]]> 8.3 8.4 8.5 8.2 8.3 8.3 8.3 Ni content, wt% 2.3 2.4 2.5 2.4 2.2 2.3 2.4 C content, wt% 3.2 3.8 2.6 4.3 3.1 3.5 3.2 10-20nm pore content, v% 43.6 45.7 41.5 49.3 49.9 47.7 43.9 50-100nm pore content, v% 17.6 19.3 16.2 22.7 6.2 5.1 16.8 Pore ​​content greater than 100nm, v% 16.1 13.9 14.8 11.6 3.2 2.7 16.5 It can be seen from the data in Table 1 that the hydrodemetallization catalyst prepared by the present invention has a relatively high content of pores of 50-100 nm and larger than 100 nm.

[0045] The catalytic performance of the hydrodemetallization catalysts (Cat-1-Cat-7) prepared in the above examples and comparative examples was evaluated by the following method: Using a certain residual oil as raw material, the metal (Ni+V) content in the raw oil is 171μg / g. The catalytic performance of the hydrodemetallization catalyst Cat-1-Cat-7 was evaluated on a 200mL small evaluation device. The reaction conditions are as follows: reaction temperature 385℃, pressure 14.0MPa, liquid hourly volume space velocity 0.65h -1 The volume ratio of hydrogen to oil was 850. The content of each impurity in the generated oil was determined after 500 hours and 5000 hours of reaction. The metal removal rate of the comparative catalyst Cat-5 at 500 hours of reaction was taken as 100%, and the relative removal rates of impurities of other catalysts were calculated. The evaluation results are shown in Table 2.

[0046] Table 2 Comparison of catalyst hydrogenation performance Catalyst No. Cat-1 Cat-2 Cat-3 Cat-4 Cat-5 Cat-6 Cat-7 500 hours relative demetallization (V+Ni) rate, % 137 135 140 131 100 97 129 5000 hours relative demetallization (V+Ni) rate, % 136 130 135 126 89 81 111 It can be seen from the data in Table 2 that when the reaction time is 500 hours, the catalyst prepared by the method of the present invention has a higher hydrodemetallization activity than the comparative catalyst. When the reaction time is 5000 hours, the catalyst prepared by the method of the present invention still has a higher hydrodemetallization activity than the comparative catalyst, which indicates that the hydrodemetallization catalyst prepared by the method of the present invention has a higher demetallization activity and better activity stability.

Claims

1. A method for preparing a carbon-containing hydrodemetallization catalyst, Features The method comprises the following contents: (1) calcining aluminum nitrate, crushing and screening the calcined material, mixing the screened material with an aqueous solution containing propylene oxide and a polyol, and then subjecting the material to hydrothermal treatment. After treatment, the material is filtered, washed and dried to obtain carbon-modified flaky pseudo-boehmite P1; (2) mixing the carbon-modified flaky pseudo-boehmite P1 with the pseudo-boehmite P2 to obtain a mixed material H0, and subjecting the mixed material to ball rolling to obtain an alumina carrier precursor S0; (3) mixing the alumina carrier precursor S0 obtained in step (2) with the carbon-modified flaky pseudo-boehmite P1, and continuing to ball rolling to obtain the formed material, drying and calcining to obtain an alumina carrier; (4) impregnating the carrier in step (3) with an active component impregnation solution, drying and calcining, and obtaining a hydrogenation demetallization catalyst.

2. The method according to claim 1, Features: The aluminum nitrate in step (1) is calcined at a temperature of 450-650° C. for a time of 4-8 hours, and the crushed particle size is greater than 100 mesh.

3. The method according to claim 1, Features: In the aqueous solution containing propylene oxide and polyols in step (1), the concentration of propylene oxide is 2.5wt%-12wt%, preferably 4wt%-8wt%; the mass ratio of the solution to the powder material is 3:1-10:1, preferably 4:1-8:

1.

4. The method according to claim 1, Features: The polyol described in step (1) is one or more of xylitol, sorbitol, mannitol, and arabitol. In the aqueous solution containing propylene oxide and the polyol, the concentration of the polyol is 10wt%-20wt%.

5. The method according to claim 1, Features: The sealed hydrothermal treatment in step (1) is carried out in a sealed container at a temperature of 110-180°C, preferably 120-160°C, for 4-8 hours. The pressure in the sealed container during the hydrothermal treatment is autogenous pressure.

6. The method according to claim 1, Features: The pseudo-boehmite P2 particles described in step (2) are in granular form and are commercially available products or homemade by acid precipitation, alkali precipitation, or alcohol aluminum hydrolysis. The pseudo-boehmite with a pore size greater than 10 nm is preferred.

7. The method according to claim 1, Features: The mass ratio of the carbon-modified flaky pseudo-boehmite P1 to the pseudo-boehmite P2 in step (2) is 1:4-2:3; the ball forming is carried out in a turntable forming machine, and the rotation operating conditions of the turntable forming machine are: the inclination angle of the turntable is 40-70º, the rotation speed of the turntable is 10-30rpm; the forming time of the material in the turntable is 10-120min; the radius of the alumina carrier precursor S0 is 0.4r-0.8r, where r is the radius of the alumina carrier.

8. The method according to claim 1, Features: The ball forming in step (3) is carried out in a turntable forming machine, and the rotation operating conditions of the turntable forming machine are: the inclination angle of the turntable is 40-70°, the rotation speed of the turntable is 10-30 rpm; the forming time of the material in the turntable is 10-120 min; during the ball forming process, an aqueous solution containing a glue solvent is sprayed into the material; the aqueous solution containing a glue solvent is one or a mixture of aqueous solutions of nitric acid, phosphoric acid, oxalic acid, and acetic acid, and the mass percentage concentration of the solution is 1%-3%.

9. The method according to claim 1, Features: The drying temperature in step (3) is 60°C-180°C, and the drying time is 1-8 hours; the calcination is carried out in an inert atmosphere, at a temperature of 350-800°C, and the calcination time is 2-6 hours.

10. The method according to claim 1, Features: The active component impregnation solution in step (4) is a solution containing a Group VIB metal and a Group VIII metal; the Group VIB metal is Mo or W, preferably Mo, the Group VIII metal is Ni or Co, preferably Ni, the Group VIB metal content is 5.5-12.5 g / 100 mL in terms of oxide, and the Group VIII metal content is 0.5-4.5 g / 100 mL in terms of oxide; the active component impregnation solution is an ammonia solution, an aqueous solution or a phosphoric acid solution of the Group VIB metal and the Group VIII metal; the drying temperature is 100-160°C, and the drying time is 6-10 hours; the calcination is carried out in an inert atmosphere, the calcination temperature is 400-550°C, and the calcination time is 2-6 hours.

11. A carbon-containing hydrodemetallization catalyst prepared according to any one of claims 1 to 10, Features: Based on the weight of the catalyst, the carbon content is 1%-5%, the molybdenum oxide content is 5%-10%, the nickel oxide content is 1.3%-3%, and the rest is an alumina carrier.

12. A carbon-containing hydrodemetallization catalyst prepared according to any one of claims 1 to 10, Features: The specific surface area of ​​the catalyst is 160-280m 2 / g, the pore volume is 0.8-1.0mL / g, the content of pores with a diameter of 10-20nm accounts for 35%-55% of the mesopore volume, the content of pores with a diameter of 50-100nm accounts for 12.5%-25% of the total pore volume, and the content of pores with a diameter greater than 100nm accounts for 10%-20% of the total pore volume.

13. Use of the carbon-containing hydrodemetallization catalyst prepared according to the method of any one of claims 1 to 10 in a residual oil hydrotreating process.

Citation Information

Patent Citations

  • Flaky polycrystal gamma-aluminum oxide and preparation method thereof

    CN104556162A

  • High-dispersion particle catalyst applied to synthesis of hydrogen peroxide as well as preparation method and application thereof

    CN107008492A

  • Preparation method of carbon-containing hydrodemetallization catalyst

    CN110935464A

  • Preparation method of high-activity hydrodemetallization catalyst

    CN110935469A

  • Catalyst for preparing styrene through gas phase dehydration of alpha-phenethyl alcohol

    CN113274996A