Synthesis method and application of low-temperature poison-resistant catalyst for treating nitrogen oxides
Through the hydrothermal reaction of sec-butanol, methylglycol, water, manganese salt, cobalt salt and cyclohexamethylenetetramine, a MnCo2O4 catalyst with a flower-like structure of hollow microspheres was prepared, which solved the problem of low-temperature problems of existing catalysts. The problem of insufficient denitrification efficiency and toxicity resistance on high-concentration NOx emission sources has been achieved, and efficient low-temperature denitrification and stability improvement have been achieved.
Patent Information
- Application Number
- CN202310349699.1
- Authority / Receiving Office
- CN · China
- Patent Type
- Applications(China)
- Current Assignee / Owner
- Filing Date
- 2023-04-04
- Publication Date
- 2024-10-15
- Estimated Expiration
- Not applicable · inactive patent
AI Technical Summary
Existing catalysts have risks of ash blocking and poisoning under high dusty flue gas conditions. They are also sensitive to SO2 at low temperatures and have poor N2 selectivity at high temperatures. They are difficult to adapt to the denitrification needs of low-temperature and high-concentration NOx emission sources.
A MnCo2O4 spinel catalyst with a hollow microsphere flower-like structure was prepared using a hydrothermal reaction method of sec-butanol, methylglycol, water, manganese salt, cobalt salt and cyclohexamethylenetetramine. The reaction and hydrothermal reaction form a through-hole shell and cavity structure, which improves the low-temperature activity and resistance to poisoning of the catalyst.
It achieves more than 90% denitrification efficiency at high concentrations of NOx (above 8000ppm) under conditions below 100°C. It has high anti-poisoning properties and stability, and is suitable for low-temperature denitrification treatment of high concentrations of nitrogen oxides.
Smart Images

Figure BDA0004161032410000101 
Figure HDA0004161032420000011 
Figure HDA0004161032420000021
Abstract
Description
Technical Field
[0001] The invention relates to a method for synthesizing a catalyst for treating nitrogen oxides, in particular to a method for synthesizing a low-temperature, poison-resistant catalyst for treating high-concentration nitrogen oxides, and belongs to the technical field of materials and environmental protection. Background Art
[0002] NOx emitted from stationary sources such as coal-fired power plants and industrial boilers x It is generally considered to be the main source of regional air pollution and air acidification in my country. Excessive NO x It will lead to a series of serious environmental problems, such as acid rain, photochemical smog, ozone depletion and greenhouse effect. x Despite the governance, the total emissions are still high and further efforts are needed to reduce emissions.
[0003] Selective catalytic reduction (SCR) of NH3 is currently the most widely used technology for denitrification in industry. Catalysts are the core of this technology. Catalysts of different types and functions have been developed and applied to different fields. Among many commercial catalysts, mixed metal oxides mainly composed of V have been widely used. However, although vanadium-based catalysts have high efficiency in denitrification at high temperatures (300-400°C), this technology still has some shortcomings that need to be improved, such as a narrow reaction window, a strong ability to convert SO2 into SO3 at high temperatures, and the toxicity of vanadium that can cause damage to the environment and human body.
[0004] Chinese patent application publication No. CN102755898A adds surfactants, sizing agents and lubricants when preparing vanadium-tungsten-titanium denitration catalysts, forms secondary microstructures and reasonable pore size distribution through secondary drying and calcination, and prepares SCR denitration catalysts suitable for high dust-containing flue gas conditions, reducing the risk of ash plugging and poisoning of honeycomb catalysts under high dust-containing flue gas conditions. The added metal oxides also further improve the anti-poisoning ability of the catalyst, improve the adaptability of the denitration catalyst under high dust-containing flue gas conditions, and achieve a breakthrough in denitration catalyst technology under high dust-containing flue gas conditions. However, this method is complex and not suitable for industrial production. More importantly, the flue gas temperature generated by some industries is relatively low (100-200°C), which is difficult to match the optimal active temperature window of such catalysts, and heating the flue gas will cause great energy consumption.
[0005] At present, manganese-based catalysts have received extensive attention and research due to their excellent low-temperature activity and environmentally friendly properties. For example, Chinese patent application publication No. CN110721677A discloses a nano manganese-based catalyst, the composition of which is: A x Mn y O z / SiO2, where A is at least one of K, Fe, Co, Ni, Cu, Zn, Ce, Zr, Bi, Sr, Mg and La; x is the atomic ratio of A, x∈[0,2]; y is the atomic ratio of Mn, y∈[1,3]; z is the atomic ratio of oxygen, which is the number of oxygen atoms that balance A and Mn. The catalyst has good activity, high temperature tolerance and catalytic life in the catalytic combustion of VOCs, and has low preparation cost. However, the catalyst still has some disadvantages, such as being sensitive to SO2 at low temperatures and poor N2 selectivity at high temperatures.
[0006] Therefore, it is very necessary to develop catalysts with low price and high low-temperature activity. Summary of the invention
[0007] One object of the present application is to provide a method for synthesizing a catalyst for treating nitrogen oxides. The catalyst prepared by this method has a hollow microsphere structure. The catalyst has a high nitrogen oxide removal rate at low temperatures, has high anti-poisoning properties, high stability and service life, and can efficiently treat high-concentration nitrogen oxides.
[0008] Another object of the present application is to provide a method for synthesizing a catalyst for treating nitrogen oxides. The method is simple, the raw materials are inexpensive, the morphology and uniformity of the catalyst can be controlled, and it has good economic, environmental and social benefits.
[0009] Another object of the present invention is to provide a catalyst for treating nitrogen oxides. x Under the conditions of concentration, the denitrification effect can be above 90%.
[0010] In the present application, a method for synthesizing a catalyst for treating nitrogen oxides comprises:
[0011] The mixed solution is obtained by mixing sec-butyl alcohol, methyl glycol, water, manganese salt, cobalt salt and cyclohexamethylenetetramine, and then subjected to a preliminary reaction; the precursor solution obtained after the preliminary reaction is subjected to a hydrothermal reaction to obtain a hydrothermal product; and the hydrothermal product is dried and calcined to obtain a catalyst.
[0012] The catalyst prepared in the present application is a MnCo2O4 spinel structure, and its morphology is a hollow microsphere flower-like structure, its shell has through holes, and the interior is a cavity, and the size is in the micrometer level. In the process of low-temperature treatment of nitrogen oxides, it has good catalytic performance.
[0013] The catalyst prepared in the present application is used in a low-temperature treatment system for high-concentration nitrogen oxide denitrification, and has a good denitrification effect at a higher NOx concentration (above 8000 ppm) and a lower reaction temperature (for example, a denitrification efficiency of more than 90% can be achieved at 75°C, and a denitrification efficiency of 98% can be achieved at 100°C). BRIEF DESCRIPTION OF THE DRAWINGS
[0014] Figure 1 This is a scanning electron microscope image of the hollow microsphere flower-shaped manganese-cobalt spinel catalyst in Example 1 at low magnification.
[0015] Figure 2 This is a scanning electron microscope image of the hollow microsphere flower-shaped manganese-cobalt spinel catalyst in Example 1 at a high magnification.
[0016] Figure 3 These are the XRD diagrams of the hollow microsphere flower-shaped manganese-cobalt spinel catalysts of Example 1, Example 2, and Example 3.
[0017] Figure 4 This is the SEM image of the catalyst prepared in Comparative Example 2.
[0018] Figure 5 The graph is a graph showing the change in nitrogen oxide conversion rate over time of the catalysts prepared in Example 1 and Comparative Example 1 in the anti-sulfur experiment.
[0019] Figure 6 The graph is a graph showing the change in nitrogen oxide conversion rate with temperature for the catalysts prepared in Example 1 and Comparative Example 1 in an alkali resistance test. DETAILED DESCRIPTION
[0020] The following is a further detailed description of a catalyst for treating nitrogen oxides and a preparation method of the present invention. The scope of protection of this application is not limited, and its scope of protection is defined by the claims. Certain disclosed specific details provide a comprehensive understanding of each disclosed embodiment. However, those skilled in the relevant art know that the embodiment can be implemented without using one or more of these specific details and using other materials, etc.
[0021] Unless the context requires otherwise, in the specification and claims, the terms "include" and "comprising" should be construed as having an open-ended, inclusive meaning, that is, "including, but not limited to".
[0022] The "embodiment", "one embodiment", "another embodiment" or "certain embodiments" mentioned in the specification means that the specific features, structures or characteristics described in connection with the embodiment are included in at least one embodiment. Therefore, "embodiment", "one embodiment", "another embodiment" or "certain embodiments" do not necessarily all refer to the same embodiment. Moreover, specific features, structures or characteristics may be combined in any manner in one or more embodiments. Each feature disclosed in the specification may be replaced by any alternative feature that can provide the same, equal or similar purpose. Therefore, unless otherwise specified, the disclosed features are only general examples of equal or similar features.
[0023] The present invention will be further described below in conjunction with specific examples. It should be understood that these examples are intended only to illustrate the present invention and are not intended to limit the scope of the present invention. The experimental methods in the following examples without specifying specific conditions are usually performed under normal conditions or according to the conditions recommended by the manufacturer. Unless otherwise stated, all percentages, ratios, proportions, or parts are by weight.
[0024] The units of weight-volume percentage in the present invention are well known to those skilled in the art, for example, refer to the weight of the solute in 100 ml of solution.
[0025] In the present invention, the concentration unit "M" of a solution represents mol / L.
[0026] Nitrogen oxides refer to compounds composed of only two elements, nitrogen and oxygen, including a variety of compounds, such as nitrous oxide (N2O), nitric oxide (NO), nitrogen dioxide (NO2), nitrogen trioxide (N2O3), nitrogen tetroxide (N2O4) and nitrogen pentoxide (N2O5). Therefore, the mixture of several gases in the environment is often called smoke (gas), mainly nitric oxide and nitrogen dioxide, with nitrogen dioxide as the main component. Nitrogen oxides are toxic to varying degrees.
[0027] Unless otherwise defined, all professional and scientific terms used herein have the same meanings as those familiar to those skilled in the art. In addition, any methods and materials similar or equivalent to those described herein can be applied to the methods of the present invention. The preferred implementation methods and materials described herein are for demonstration purposes only.
[0028] This application mainly removes nitrogen oxides at low temperature. Usually, nitrogen oxides contain more water at low temperature and the activity of the catalyst is low. For the low-temperature removal of nitrogen oxides system, a catalyst with low price and high low-temperature activity is developed.
[0029] In the present application, a method for synthesizing a catalyst for treating nitrogen oxides comprises:
[0030] (1) mixing sec-butyl alcohol, methyl glycol, water, manganese salt, cobalt salt and hexamethylenetetramine to obtain a mixed solution, and performing a pre-reaction;
[0031] (2) subjecting the precursor solution obtained after the preliminary reaction to a hydrothermal reaction to obtain a hydrothermal product;
[0032] (3) Drying and calcining the hydrothermal product to obtain a catalyst.
[0033] In the present application, sec-butyl alcohol, methyl glycol, cyclohexamethylenetetramine and manganese cobalt solution are first subjected to a pre-reaction and then a hydrothermal reaction process. In the pre-reaction system of the present application, the liquid tension in the solution is suitable for the nucleation of the hollow microsphere flower-shaped catalyst. Therefore, the morphology of the catalyst can be controlled, and the prepared catalyst has a larger specific surface area, which is more conducive to the low-temperature denitration performance of the reactant.
[0034] In certain embodiments, the reaction temperature of the pre-reaction is controlled at 80°C to 90°C.
[0035] In certain embodiments, the reaction temperature of the pre-reaction is controlled at 80°C, 82°C, 85°C, 88°C or 90°C for condensation reflux.
[0036] In the preparation method system, the metal cations of manganese and cobalt can react, nucleate and grow in a controllable manner during the pre-reaction process. Specifically, the condensation reflux at a certain temperature (such as 80°C to 90°C) can ensure the stability of the rate of metal cations during the reaction process, so that the nucleation and growth processes are kept in a relatively stable and mild state, which can ensure the uniformity of the size and integrity of the morphology of the hollow microsphere flower-like structure formed.
[0037] In certain embodiments, the pre-reaction time is 2 h to 4 h, such as 2 h, 2.5 h, 3 h, 3.5 h or 4 h.
[0038] In certain embodiments, sec-butyl alcohol, methyl glycol and water are first mixed to obtain a viscous solution; manganese salt and cobalt salt are added to the viscous solution, and then cyclohexamethylenetetramine is added.
[0039] After sec-butanol is used as a solvent, methyl glycol is used as a surfactant and water to form a mixed solution, after the solution system is stabilized, Mn and Co metal salt precursors are added. In this solution system, metal cations can further react rapidly to form nuclei, and after a large number of nuclei are formed, they combine with hexamethylenetetramine to self-assemble to form a hollow microsphere flower-like structure.
[0040] In certain embodiments, the molar ratio of Mn element to Co element in the manganese salt and the cobalt salt is 1:(0.8-1.2)
[0041] Preferably, the molar ratio of Mn element to Co element in the manganese salt and the cobalt salt is 1:1.
[0042] The manganese salt may be a soluble salt containing manganese, for example, at least one of manganese sulfate, manganese nitrate and manganese acetate.
[0043] The cobalt salt may be a soluble salt containing cobalt, for example, at least one of cobalt sulfate, cobalt nitrate and cobalt acetate.
[0044] In certain embodiments, the volume ratio of sec-butyl alcohol, methyl glycol, and water is 1:(1.8-2.5):(3.5-4.5).
[0045] Preferably, the volume ratio of sec-butyl alcohol, methyl glycol and water is 1:2:4.
[0046] The volume mass ratio of sec-butyl alcohol to hexamethylenetetramine is: 1:(0.05-0.2) (ml / g).
[0047] In this embodiment, the mass ratio of hexamethylenetetramine to the Mn element is 1:(0.4-7).
[0048] Preferably, the mass ratio of hexamethylenetetramine to the Mn element is 1:(0.2-2).
[0049] In certain embodiments, the temperature of the hydrothermal reaction is 100°C to 220°C.
[0050] Preferably, the temperature of the hydrothermal reaction is 100°C to 180°C.
[0051] In certain embodiments, the temperature of the hydrothermal reaction is 100°C, 120°C, 130°C, 140°C, 150°C, 155°C, 160°C, 170°C, or 180°C, etc.
[0052] Preferably, the hydrothermal reaction time is 6 h to 24 h.
[0053] More preferably, the hydrothermal reaction time is 10 h to 18 h, for example 10 h, 11 h, 12 h, 13 h, 14 h, 15 h, 16 h or 18 h.
[0054] In certain embodiments, during the hydrothermal process, the pre-reacted solution is heated to the hydrothermal reaction temperature at a rate of 1° C. / min to 5° C. / min.
[0055] Controlling the heating rate in the hydrothermal reaction can better control the growth rate of the hollow microsphere flower-like structure, keeping it in a uniform growth state. It can also maintain the uniformity and integrity of the morphology, thereby further improving the low-temperature catalytic effect and anti-poisoning ability of the catalyst.
[0056] In certain embodiments, the calcination temperature in step (3) is 350°C to 500°C, for example, 350°C, 360°C, 380°C, 400°C, 425°C, 450°C, 475°C or 500°C.
[0057] The calcination time in step (3) is 2 h to 6 h, for example 2 h, 2.5 h, 3 h, 3.5 h, 4 h, 4.5 h, 5 h, 5.5 h or 6 h.
[0058] In certain embodiments, between step (2) and step (3), the method further comprises the steps of washing and drying the hydrothermal product.
[0059] Preferably, the washing includes water washing and alcohol washing.
[0060] The water washing is usually washing the hydrothermal product with distilled water. The solvent used in the alcohol washing can be an alcohol solvent such as anhydrous ethanol.
[0061] The water washing process can clean the metal ions and organic solvents that have not reacted completely.
[0062] The product after alcohol washing is convenient to dry, and can also reduce the damage to the catalyst morphology caused by surface tension caused by evaporation using only water washing during the drying process.
[0063] In some cases, the drying is vacuum drying, and the drying temperature is 60°C to 80°C, such as 60°C, 65°C, 70°C, 75°C or 80°C.
[0064] The drying time is 15 h to 20 h, for example 15 h, 16 h, 17 h, 18 h, 19 h or 20 h.
[0065] On the other hand, the catalyst for treating nitrogen oxides of the present application is a manganese-cobalt composite metal oxide with a spinel structure, and the manganese-cobalt composite metal oxide is in a hollow microsphere structure.
[0066] The hollow microsphere structure comprises a shell layer with through holes and a cavity located in the shell layer.
[0067] In the catalyst of the present invention, the physical structure of the manganese-cobalt composite metal oxide is a MnCo2O4 spinel structure, and the morphology is a hollow microsphere flower-like structure, the shell layer of which has through holes and the interior is a cavity with a size of micrometer level.
[0068] This structure is beneficial to the gas mass transfer process and protects the active sites of the inner layer. The catalyst has excellent low-temperature activity (for example, it can still achieve a denitrification efficiency of more than 90% at 75°C and a denitrification efficiency of 98% at 100°C), anti-poisoning properties, high stability and service life.
[0069] In certain embodiments, the catalyst is a catalyst with cobalt-rich surface. Cobalt species are enriched on the surface, which is beneficial to improving the catalytic performance of the catalyst.
[0070] Preferably, the manganese-cobalt composite metal oxide has a hollow spherical flower-like morphology. The spherical flower-like structure means that the manganese-cobalt composite oxide is spherical as a whole, with a cavity inside, and the shell is arranged like petals and has through holes. For example, the petals are arranged in a structure similar to that of a hydrangea.
[0071] The catalyst having the above structure can be prepared by any method. The method for preparing the catalyst provided in the present application can not only obtain the catalyst having the above structure, but also has a simple preparation method, low raw material price, adjustable catalyst morphology and uniformity, and has good economic, environmental and social benefits.
[0072] In certain embodiments, the particle size of the manganese-cobalt composite metal oxide is in the range of 1 um to 3 um, and the particle size distribution is relatively uniform.
[0073] Preferably, the shell layer has a thickness of 100 nm to 300 nm, for example, 100 nm, 150 nm, 200 nm, 250 nm or 300 nm.
[0074] In another aspect, the catalyst is used in a reaction for treating nitrogen oxides.
[0075] The method for removing nitrogen oxides comprises: the nitrogen oxides react under the action of the above catalyst at a temperature of 70 to 100° C. to convert the nitrogen oxides into nitrogen.
[0076] During the reaction process of treating nitrogen oxides, a reducing agent, such as ammonia, is introduced.
[0077] For example, the catalyst is used in the NH3-SCR system, where nitrogen oxides react with NH3 to reduce them to N2.
[0078] Generally, the water content in flue gas or exhaust gas containing nitrogen oxides at a temperature below 100°C is relatively high. High water content, alkalinity or sulfur-containing substances in the system will affect the catalytic performance or life of the nitrogen oxide removal catalyst.
[0079] The catalyst prepared in the present application is used in a low-temperature denitrification system for treating high-concentration nitrogen oxides. It has a good denitrification effect at a higher NOx concentration (above 8000 ppm) and a lower reaction temperature (for example, a denitrification efficiency of more than 90% can be achieved at 75°C, and a denitrification efficiency of 98% can be achieved at 100°C). It also has high anti-poisoning properties, stability and service life, and can be used for low-temperature denitrification control of high-concentration nitrogen oxide emission sources.
[0080] The catalyst for treating nitrogen oxides, its preparation method and its catalytic effect of the present invention are further described below with reference to specific examples.
[0081] Example 1
[0082] The preparation method of the catalyst comprises the following steps:
[0083] a) 10 ml of sec-butyl alcohol was slowly added to 20 ml of methyl glycol, and after stirring evenly, 40 ml of ultrapure water was added. The mixed solution was vigorously stirred for 2 h to finally obtain a homogeneous viscous solution without stratification.
[0084] b) Add 2.4 g of manganese acetate tetrahydrate and 2.5 g of cobalt acetate tetrahydrate to the transparent solution obtained in step a), and continue stirring for 2 h. After the precursor is completely dissolved, add 0.5 g of cyclohexamethylenetetramine, and condense and reflux at 85° C. for 3 h.
[0085] c) The solution obtained in step b) was transferred to a 100 ml reactor, heated at a heating rate of 2°C / min, and finally subjected to hydrothermal reaction at 140°C for 16 hours. After the reaction, the temperature was cooled to room temperature, and the product was collected, washed with water and alcohol for several times, and vacuum dried at 80°C for 15 hours. Finally, the product was calcined at 500°C for 4 hours at a heating rate of 1°C / min to obtain a spinel structure hollow microsphere catalyst A.
[0086] The hollow microsphere catalyst A prepared in this example was subjected to X-ray powder diffraction (XRD) analysis and scanning electron microscope (SEM) analysis. Figure 3 The XRD pattern shows that the catalyst is a manganese-cobalt composite metal oxide with a spinel structure of MnCo2O4. The scanning electron microscope analysis of catalyst A at different magnifications shows that Figure 1 and Figure 2 The manganese-cobalt composite metal oxide has a hollow microsphere flower-like morphology; the hollow microsphere structure includes a shell layer with through holes and a cavity located in the shell layer, and the shell layer is arranged like a petal and has through holes. The particle size of the manganese-cobalt composite metal oxide is in the range of 1um to 3um, and the thickness of the shell layer is about 100nm.
[0087] The catalyst obtained in this example adopts Brunauer–Emmett–Teller (BET specific surface area test method) to measure its specific surface area. The results show that the catalyst has a large specific surface area (226m 2 g -1 ), providing more active sites, which is beneficial to improving the denitrification efficiency.
[0088] Example 2
[0089] The preparation method of the catalyst comprises the following steps:
[0090] a) 10 ml of sec-butyl alcohol was slowly added to 20 ml of methyl glycol, and after stirring evenly, 40 ml of ultrapure water was added. The mixed solution was vigorously stirred for 2 h to finally obtain a homogeneous viscous solution without stratification.
[0091] b) Add 2.5 g of manganese nitrate tetrahydrate and 2.9 g of cobalt nitrate hexahydrate to the transparent solution obtained in step a), and continue stirring for 2 h. After the precursor is completely dissolved, add 1 g of cyclohexamethylenetetramine, and condense and reflux at 85° C. for 3 h.
[0092] c) The solution obtained in step b) was transferred to a 100 ml reactor, heated at a heating rate of 2°C / min, and finally subjected to hydrothermal reaction at 140°C for 16 hours. After the reaction, the temperature was cooled to room temperature, and the product was collected. After being washed with water and alcohol for several times, the product was vacuum dried at 80°C for 15 hours, and finally calcined at 500°C for 4 hours at a heating rate of 1°C / min to obtain a spinel structure hollow microsphere catalyst B.
[0093] Catalyst B prepared in this embodiment is a manganese-cobalt composite metal oxide including a spinel structure, and the manganese-cobalt composite metal oxide is a hollow microsphere structure; the hollow microsphere structure includes a shell layer with through holes and a cavity located in the shell layer, and the shell layer is arranged like petals and has through holes.
[0094] Example 3
[0095] The preparation method of the catalyst comprises the following steps:
[0096] a) 10 ml of sec-butyl alcohol was slowly added to 20 ml of methyl glycol, and after stirring evenly, 40 ml of ultrapure water was added. The mixed solution was vigorously stirred for 2 h to finally obtain a homogeneous viscous solution without stratification.
[0097] b) Add 1.5 g of manganese sulfate and 1.6 g of cobalt sulfate to the transparent solution obtained in step a), and continue stirring for 2 h. After the precursor is completely dissolved, add 2 g of cyclohexamethylenetetramine, and condense and reflux at 85° C. for 3 h.
[0098] c) The solution obtained in step b) was transferred to a 100 ml reactor, heated at a heating rate of 1°C / min, and finally subjected to hydrothermal reaction at 170°C for 18 hours. After the reaction, the temperature was lowered at a cooling rate of 5°C / min. The product was collected at room temperature, washed with water and alcohol for several times, and then vacuum dried at 60°C for 15 hours. Finally, the product was calcined at 400°C for 5 hours to obtain a spinel structured hollow microsphere catalyst C.
[0099] The catalyst C prepared in this embodiment includes a manganese-cobalt composite metal oxide with a spinel structure, and the manganese-cobalt composite metal oxide is in a hollow microsphere structure; the hollow microsphere structure includes a shell layer with through holes and a cavity located in the shell layer, and the shell layer is arranged like petals and has through holes.
[0100] Example 4
[0101] The difference from Example 1 is that the temperature of the hydrothermal reaction is 220° C. The obtained catalyst is recorded as catalyst D.
[0102] Example 5
[0103] The difference from Example 1 is that the hydrothermal reaction time is 6 hours. The obtained catalyst is recorded as catalyst E.
[0104] Example 6
[0105] The difference from Example 1 is that the hydrothermal reaction time is 24 hours. The obtained catalyst is recorded as catalyst F.
[0106] Comparative Example 1
[0107] This comparative example adopts a traditional method to prepare granular manganese-cobalt composite metal oxide, and the preparation method is as follows:
[0108] a) 2.4 g of manganese acetate tetrahydrate and 2.5 g of cobalt acetate tetrahydrate were added to 50 ml of ultrapure water and stirred for 2 h to obtain a homogeneous transparent solution.
[0109] b) Add 4 g of ammonium carbonate to 20 ml of ultrapure water and stir until completely dissolved.
[0110] c) Slowly add the solution obtained in step b) dropwise to the solution in step a) with continuous stirring, and stir for 2 hours after the addition is completed.
[0111] d) The precipitated product was collected, washed with water and alcohol for several times, and then vacuum dried at 60° C. for 15 h. Finally, the product was calcined at 400° C. for 5 h. The obtained catalyst was recorded as catalyst M1.
[0112] Comparative Example 2
[0113] The difference between this comparative example and Example 1 is that sec-butyl alcohol and methyl glycol are not added, but are replaced by ethanol equal to the total mass of the two. The obtained catalyst is recorded as catalyst M2.
[0114] The SEM image of the catalyst obtained in this comparative example is shown in Figure 4 Its morphology is solid spherical. The reason may be that the change of solvent leads to the failure of forming the flower-like morphology of hollow microspheres.
[0115] Comparative Example 3
[0116] The difference between this comparative example and Example 1 is that sec-butyl alcohol and methyl glycol are not added, but propylene glycol is used in an amount equal to the total mass of the two. The obtained catalyst is recorded as catalyst M3.
[0117] Comparative Example 4
[0118] The difference between this comparative example and Example 1 is that the condensation reflux step in step b) is not performed, and the mixed solution is directly transferred to a reactor for hydrothermal reaction. The obtained catalyst is recorded as catalyst M4.
[0119] Effect test:
[0120] Experimental Example 1
[0121] The catalysts prepared in Examples 1-6 and Comparative Documents 1-3 were evaluated, and the test conditions for denitration performance were as follows: reaction temperature 75°C, gas flow rate 100mL / min, NO concentration 8000ppm, NH3 concentration 8000ppm, O2 concentration 8% in the gas; N2 was used as the balance gas, and the space velocity was 32000h -1 The catalyst denitrification efficiency is shown in Table 1.
[0122] Table 1
[0123]
[0124] By comparing Example 1 with Example 4, it can be seen that the hydrothermal temperature will affect the product performance. A higher hydrothermal temperature will lead to a decrease in the low-temperature denitrification performance.
[0125] By comparing Example 1 with Comparative Example 1, it can be seen that the low-temperature denitration activity of the granular catalyst prepared by the traditional co-precipitation method is much lower than that of the hollow microsphere flower-shaped catalyst prepared in this example.
[0126] By comparing Example 1 with Comparative Examples 2-3, it can be seen that the choice of solvent plays a very important role in forming the flower-like morphology of hollow microspheres and the special spinel structure. The combined effect of the above morphology and crystal structure improves the comprehensive performance of the catalyst. Comparative Examples 2-3 use ethanol or glycerol as solvent, and the denitration efficiency of the obtained catalyst is greatly reduced compared with Example 1.
[0127] By comparing Example 1 with Comparative Example 4, it can be seen that failure to perform condensation reflux will result in reduced low-temperature denitration performance of the catalyst.
[0128] Experimental Example 2
[0129] The anti-poisoning test process is as follows: by simulating the poisoning process of sulfur dioxide and alkali metals on the catalyst in the actual flue gas environment, the resistance of the catalyst is examined respectively. In the anti-sulfur and anti-alkali metal test, glass flue gas with a high pollutant concentration is used as the experimental simulated flue gas:
[0130] The experimental conditions of the sulfur resistance and simultaneous water resistance and sulfur resistance experiments are as follows: reaction temperature 150°C, the content of each substance in the gas: 8000ppm NO, 8000ppm NH3, 8vol% O2, and 200ppm SO2, or the content of each substance in the gas: 8000ppm NO, 8000ppm NH3, 8vol% O2, 200ppm SO2 and 10vol% H2O, high-purity N2 as carrier gas. The curves of nitrogen oxide conversion rate change over time of catalyst A and catalyst M are shown in Figure 5 As can be seen from the figure, when the system contains sulfur, or sulfur and water, the low-temperature catalytic activity of catalyst A is increased by 16% compared with catalyst M1.
[0131] The experimental conditions of the alkali resistance experiment are as follows: at different temperatures, the content of each substance in the gas: 8000ppm NO, 8000ppm NH3, 8vol% O2, and 10vol% H2O; high-purity N2 is used as the carrier gas.
[0132] Catalyst A prepared in Example 1 and Catalyst M1 prepared in Comparative Example 1 were impregnated with a mixed solution containing sodium nitrate, potassium nitrate, calcium nitrate and magnesium nitrate, and then calcined, so that Catalyst A and Catalyst M1 contained about 4 wt% of alkali metal and alkaline earth metal (1 wt% each of the mass of Na2O, K2O, CaO and MgO). Catalyst A and Catalyst M1 loaded with alkali metal and alkaline earth metal were used to catalyze the above-mentioned gas system to remove NO.
[0133] The curves of nitrogen oxide conversion rate of catalyst A and catalyst M1 as a function of temperature are shown in Figure 6 As can be seen from the figure, the low-temperature catalytic activity of catalyst A at 150°C is improved by 88.5% compared with catalyst M1.
[0134] The applicant declares that the present invention illustrates the detailed method of the present invention through the above-mentioned embodiments, but the present invention is not limited to the above-mentioned detailed method, that is, it does not mean that the present invention must rely on the above-mentioned detailed method to be implemented. Those skilled in the art should understand that any improvement of the present invention, equivalent replacement of various raw materials of the product of the present invention, addition of auxiliary components, selection of specific methods, etc., all fall within the protection scope and disclosure scope of the present invention.
Claims
1. A method for synthesizing a catalyst for treating nitrogen oxides, include: (1) mixing sec-butyl alcohol, methyl glycol, water, manganese salt, cobalt salt and hexamethylenetetramine to obtain a mixed solution, and performing a pre-reaction; (2) subjecting the precursor solution obtained after the preliminary reaction to a hydrothermal reaction to obtain a hydrothermal product; (3) drying and calcining the hydrothermal product to obtain a catalyst; Preferably, in step (1), sec-butyl alcohol, methyl glycol and water are first mixed to obtain a viscous solution; Manganese salt and cobalt salt are added to the viscous solution, and then cyclohexamethylenetetramine is added.
2. The synthesis method according to claim 1, It is characterized in that The reaction temperature of the pre-reaction is controlled at 80°C to 90°C; Preferably, the reaction temperature of the pre-reaction is controlled at 80°C, 82°C, 85°C, 88°C or 90°C for condensation reflux; More preferably, the pre-reaction time is 2 h to 4 h, for example 2 h, 2.5 h, 3 h, 3.5 h or 4 h.
3. The synthesis method according to claim 1, It is characterized in that The volume ratio of sec-butanol, methyl glycol and water is 1:(1.8-2.5):(3.5-4.5); preferably, the volume ratio of sec-butanol, methyl glycol and water is 1:2:
4.
4. The synthesis method according to any one of claims 1 to 3, It is characterized in that The volume mass ratio of sec-butyl alcohol and cyclohexamethylenetetramine is: 1: (0.05-0.2) (ml / g); Preferably, the molar ratio of Mn element to Co element in the manganese salt and the cobalt salt is 1:(0.8-1.2); More preferably, the mass ratio of hexamethylenetetramine to the Mn element is 1:(0.4-7).
5. The synthesis method according to any one of claims 1 to 3, It is characterized in that The temperature of the hydrothermal reaction is 100°C to 220°C; Preferably, the temperature of the hydrothermal reaction is 100°C to 180°C; More preferably, the hydrothermal reaction time is 6 h to 24 h.
6. The synthesis method according to claim 5, It is characterized in that During the hydrothermal process, the pre-reacted solution is heated to the hydrothermal reaction temperature at a rate of 1°C / min to 5°C / min.
7. The synthesis method according to any one of claims 1 to 6, It is characterized in that The calcination temperature in step (3) is 350° C. to 500° C. Preferably, the calcination temperature is 350°C, 360°C, 380°C, 400°C, 425°C, 450°C, 475°C or 500°C; More preferably, the calcination time is 2 h to 6 h.
8. A catalyst for treating nitrogen oxides, the catalyst being a spinel-structured manganese-cobalt composite metal oxide, the manganese-cobalt composite metal oxide being a hollow microsphere structure, The hollow microsphere structure comprises a shell layer having through holes and a cavity located in the shell layer; Preferably, the particle size of the manganese-cobalt composite metal oxide is in the range of 1um to 3um; More preferably, the thickness of the shell layer is 100 nm to 300 nm.
9. Use of the catalyst according to claim 8 in a reaction for treating nitrogen oxides.
10. The use according to claim 9, It is characterized in that Nitrogen oxides react under the action of a catalyst at a temperature of 70 to 100°C to convert the nitrogen oxides into nitrogen.
Citation Information
Patent Citations
Micro spherical hollow structure nickel-based hydrogenation catalyst as well as preparation method thereof
CN103962140A
MnyCoOx hybrid nanorod catalyst and preparation method and application thereof
CN113262800A