Iron-based amorphous nanocrystalline soft magnetic material and preparation method and application thereof
By using iron-based amorphous nanocrystalline soft magnetic materials in photovoltaic inverters, fine nanocrystals are formed through smelting, quick quenching, annealing and laser-induced processing, and coating modified particles are added to the magnetic core to solve the existing problems. There is a problem in technology with large differences in material strength and magnetic permeability. It achieves stable magnetic permeability and inductance change rates at high and low frequencies, which is suitable for industrial applications.
Patent Information
- Application Number
- CN202410750288.8
- Authority / Receiving Office
- CN · China
- Patent Type
- Applications(China)
- Current Assignee / Owner
- Filing Date
- 2024-06-12
- Publication Date
- 2024-10-15
AI Technical Summary
The FeSi-based alloy materials used in existing photovoltaic inverters have problems such as low mechanical strength, large difference in high-frequency and low-frequency magnetic permeability, large inductance change rate under high saturation magnetic field strength, and easy aging, making it difficult to meet practical application requirements.
The method for preparing iron-based amorphous nanocrystalline soft magnetic materials includes melting Fe-Co-Si-Al material in a protective atmosphere, rapid quenching, annealing and pulse laser induction treatment to form refined iron-based nanocrystals. , and add coated modified Fe-Co-Si-Al particles and silicone resin to the magnetic core to improve the mechanical strength and magnetic permeability of the magnetic core.
It achieves high bending strength of the magnetic core, high magnetic permeability and small difference under high and low frequencies, small inductance change rate under high saturation magnetic field intensity, long-lasting and stable performance, and is suitable for use in photovoltaic inverters.
Smart Images

Figure BDA0004887671060000081
Abstract
Description
Technical Field
[0001] The invention relates to the technical field of soft magnetic materials, and in particular to an iron-based amorphous nanocrystalline soft magnetic material and a preparation method and application thereof. Background Art
[0002] Photovoltaic power generation system is a power generation system that directly converts solar radiation energy into electrical energy by utilizing the photovoltaic effect of photovoltaic cells. It is mainly composed of three parts: solar panels, controllers and inverters. Photovoltaic inverters can convert the variable direct current generated by solar panels into alternating current of commercial power frequency. The conversion efficiency and reliability will directly affect the overall performance of the photovoltaic power generation system. At present, most photovoltaic inverters use FeSi-based soft magnetic materials made of FeSi-based alloy materials through resin impregnation process. Although it has a high saturation magnetization intensity (150Am 2 / kg), but there are problems such as low mechanical strength, large difference in magnetic permeability at high and low frequencies, large rate of inductance change at high saturation magnetic field strength, and easy aging, which make it difficult to fully meet the requirements of practical applications.
[0003] Therefore, it is of great significance to develop a soft magnetic material with high mechanical strength, high magnetic permeability and small difference at high and low frequencies, small inductance change rate at high saturation magnetic field intensity, and long-lasting and stable performance.
[0004] The above statements merely provide background information related to the present invention and do not necessarily constitute prior art. Summary of the invention
[0005] The purpose of the present invention is to provide an iron-based amorphous nanocrystalline soft magnetic material and a preparation method and application thereof.
[0006] The technical solution adopted by the present invention is:
[0007] A method for preparing an iron-based amorphous nanocrystalline soft magnetic material comprises the following steps:
[0008] 1) placing the Fe-Co-Si-Al material in a protective atmosphere for smelting to obtain a melt;
[0009] 2) adding the melt into a vacuum single-roller spinning quenching machine for rapid quenching to obtain a Fe-Co-Si-Al amorphous strip;
[0010] 3) The Fe-Co-Si-Al amorphous strip is placed in a protective atmosphere at a temperature of 520°C to 570°C for annealing, and then the temperature is lowered to 0°C to 5°C, and then both sides of the strip are laser-induced treated with a pulsed laser to obtain an iron-based amorphous nanocrystalline soft magnetic material.
[0011] Preferably, the Fe-Co-Si-Al material in step 1) comprises the following components in weight percentage:
[0012] Fe: 65.5%~75.5%;
[0013] Co: 20%-27%;
[0014] Si: 3% to 5%;
[0015] Al: 1.5% to 2.5%.
[0016] Preferably, the smelting in step 1) is carried out at a temperature of 1550° C. to 1650° C., the number of smelting is 3 to 5 times, and the time of a single smelting is 30s to 60s.
[0017] Preferably, the protective atmosphere in step 1) is an argon atmosphere or a nitrogen atmosphere.
[0018] Preferably, the rapid quenching treatment in step 2) is carried out under the condition that the rotation speed of the cooling roller of the vacuum single-roller spinning quenching machine is 20m / s to 30m / s.
[0019] Preferably, in step 2), the thickness of the Fe—Co—Si—Al amorphous strip is 30 μm to 60 μm.
[0020] Preferably, the protective atmosphere in step 3) is an argon atmosphere or a nitrogen atmosphere.
[0021] Preferably, the annealing treatment time in step 3) is 10 min to 20 min.
[0022] Preferably, in step 3), the frequency of the pulse laser is 50 Hz to 100 Hz, the pulse width is 10 ms to 30 ms, and the spot diameter is 10 mm to 20 mm.
[0023] Preferably, the operation of the laser induced treatment in step 3) is: using a pulsed laser to scan the strip surface line by line at a scanning speed of 15 mm / s to 35 mm / s.
[0024] An iron-based amorphous nanocrystalline soft magnetic material is made by the above-mentioned preparation method.
[0025] A magnetic core comprises iron-based amorphous nanocrystalline soft magnetic particles, coated modified Fe-Co-Si-Al particles and silicone resin in a weight ratio of 1:0.5-1.5:0.03-0.08; the iron-based amorphous nanocrystalline soft magnetic particles are made by crushing the above-mentioned iron-based amorphous nanocrystalline soft magnetic material; the coated modified Fe-Co-Si-Al particles are composed of a Fe-Co-Si-Al core, a Si-Al composite oxide layer and an Al layer from the inside to the outside.
[0026] Preferably, the particle size of the iron-based amorphous nanocrystalline soft magnetic particles is 20 μm to 60 μm.
[0027] Preferably, the coated modified Fe-Co-Si-Al particles are prepared by a preparation method comprising the following steps:
[0028] a) smelting the Fe-Co-Si-Al material, and then performing ultra-high pressure water atomization to obtain Fe-Co-Si-Al powder with a particle size of 3 μm to 50 μm;
[0029] b) air-classifying the Fe-Co-Si-Al powder, mixing it with a high-temperature resistant oxide powder having a particle size of 0.1 μm to 1 μm, treating it at 400° C. to 600° C. in an atmosphere containing water vapor, and then sieving out the high-temperature resistant oxide powder to obtain Fe-Co-Si-Al particles containing a Si-Al composite oxide layer;
[0030] c) placing the Fe-Co-Si-Al particles containing the Si-Al composite oxide layer in a reducing atmosphere for annealing to form an Al layer on the surface of the Si-Al composite oxide layer, thereby obtaining coated and modified Fe-Co-Si-Al particles.
[0031] Preferably, the Fe-Co-Si-Al material in step a) comprises the following components in weight percentage:
[0032] Fe: 65.5%~75.5%;
[0033] Co: 20%-27%;
[0034] Si: 3% to 5%;
[0035] Al: 1.5% to 2.5%.
[0036] Preferably, the amount of the high temperature resistant oxide powder added in step b) is 5% to 25% of the weight of the Fe-Co-Si-Al powder.
[0037] Preferably, the high temperature resistant oxide powder in step b) is at least one of silicon oxide powder and aluminum oxide powder. The high temperature resistant oxide powder is distributed among the Fe-Co-Si-Al powders, which can effectively prevent the Fe-Co-Si-Al powders from sticking and agglomerating during the oxidation treatment.
[0038] Preferably, in step b), the particle size of the Fe-Co-Si-Al powder after airflow classification is 3 μm to 27 μm.
[0039] Preferably, the water vapor-containing atmosphere in step b) consists of water vapor and at least one of air, nitrogen and argon.
[0040] Preferably, the volume percentage of water vapor in the water vapor-containing atmosphere in step b) is 70% to 90%.
[0041] Preferably, the treatment time in step b) is 1 h to 5 h.
[0042] Preferably, the reducing atmosphere in step c) is an atmosphere containing hydrogen.
[0043] Preferably, the annealing in step c) is carried out at 600° C. to 700° C., and the annealing time is 1 h to 3 h.
[0044] A method for preparing the magnetic core as described above comprises the following steps:
[0045] The iron-based amorphous nanocrystalline soft magnetic particles, coated modified Fe-Co-Si-Al particles and silicone resin are mixed, pressed into shape, and then sintered in a protective atmosphere to obtain a magnetic core.
[0046] Preferably, the silicone resin is at least one of silicone resin KR-282 produced by Shin-Etsu Chemical Co., Ltd., silicone resin KR-242A produced by Shin-Etsu Chemical Co., Ltd., and silicone resin KR-271 produced by Shin-Etsu Chemical Co., Ltd.
[0047] Preferably, the pressing pressure is 25 tons / cm 2 ~30 tons / cm 2 .
[0048] Preferably, the protective atmosphere is an argon atmosphere or a nitrogen atmosphere.
[0049] Preferably, the sintering is carried out at a temperature of 550° C. to 650° C., and the sintering time is 0.5 h to 1.5 h.
[0050] A photovoltaic inverter comprises the magnetic core.
[0051] A photovoltaic power generation system comprises the photovoltaic inverter.
[0052] Principle of the present invention:
[0053] 1) The present invention rapidly converts the melt obtained by smelting the Fe-Co-Si-Al material into an Fe-Co-Si-Al amorphous strip by a single-roll spinning method, and then forms iron-based nanocrystals of different sizes in the Fe-Co-Si-Al amorphous strip by annealing, and then converts the iron-based nanocrystals of different sizes in the Fe-Co-Si-Al amorphous strip into iron-based nanocrystals of uniform size by laser induced treatment (the laser can rapidly heat up the area irradiated by the strip, and the operating temperature of 0°C to 5°C during the irradiation interval of the pulsed laser can rapidly cool down the area. The stress caused by the operation of "rapid heating + rapid cooling" can convert the large-sized iron-based nanocrystals in the area into smaller and more uniform iron-based nanocrystals, and finally achieve the effect of grain refinement). The iron-based amorphous nanocrystal soft magnetic particles made of the iron-based amorphous nanocrystal soft magnetic material are used in the magnetic core to effectively improve the mechanical strength, magnetic permeability and other properties of the magnetic core;
[0054] 2) The present invention adds coated and modified Fe-Co-Si-Al particles (from the inside to the outside, Fe-Co-Si-Al core, Si-Al composite oxide layer and Al layer) into the magnetic core, and utilizes the Si-Al composite oxide layer to improve the insulation performance of the magnetic core material, thereby reducing the eddy current loss between the particles, and utilizes the Al oxide film formed between the metal particles during the pressing and molding of the magnetic core material by the Al layer to achieve the bonding of the metal particles, thereby avoiding the use of the traditional resin impregnation process, so that the prepared magnetic core has no aging problem and can be used at the KHz level, and finally the magnetic core can have the advantages of high magnetic permeability and small difference at high and low frequencies, small inductance change rate at high saturation magnetic field strength, and long-lasting and stable performance.
[0055] The beneficial effects of the present invention are as follows: the magnetic core made of the iron-based amorphous nanocrystalline soft magnetic material of the present invention has the advantages of high bending strength, high and small difference in magnetic permeability at high and low frequencies, small inductance change rate at high saturation magnetic field strength, and long-lasting and stable performance. It can be used as a magnetic core in a photovoltaic inverter and is suitable for large-scale industrial production applications. DETAILED DESCRIPTION
[0056] The present invention will be further explained and illustrated below in conjunction with specific embodiments.
[0057] Embodiment 1:
[0058] An iron-based amorphous nanocrystalline soft magnetic material, the preparation method of which is as follows:
[0059] 1) Fe-Co-Si-Al material (composition: 75.5wt% Fe, 20wt% Co, 3wt% Si and 1.5wt% Al) is added into an electric arc furnace, and filled with nitrogen for protection, and then smelted 4 times at a temperature of 1570° C., with a single smelting time of 50s to obtain a melt;
[0060] 2) adding the melt into a vacuum single-roller spinning quenching strip spinning machine, adjusting the rotation speed (linear speed) of the cooling roll to 20 m / s for rapid quenching to obtain a Fe-Co-Si-Al amorphous strip (thickness of 45 μm to 60 μm);
[0061] 3) The Fe-Co-Si-Al amorphous strip is placed in a nitrogen atmosphere at a temperature of 530°C for annealing for 20 minutes, and then cooled to 0°C. A pulse laser is used to scan the upper and lower surfaces of the strip line by line at a scanning speed of 20 mm / s. The frequency of the pulse laser is 50 Hz, the pulse width is 20 ms, and the spot diameter is 15 mm, thereby obtaining an iron-based amorphous nanocrystalline soft magnetic material.
[0062] A magnetic core, the preparation method of which is as follows:
[0063] 1) crushing the above-mentioned iron-based amorphous nanocrystalline soft magnetic material to obtain iron-based amorphous nanocrystalline soft magnetic particles (particle size is 40 μm to 60 μm);
[0064] 2) adding Fe-Co-Si-Al material (composition: 75.5wt% Fe, 20wt% Co, 3wt% Si and 1.5wt% Al) into a high frequency furnace for smelting, and then performing ultra-high pressure water atomization to obtain Fe-Co-Si-Al powder with a particle size of 3μm to 50μm; performing air flow classification on the Fe-Co-Si-Al powder, and then taking Fe-Co-Si-Al powder with a particle size of 3μm to 27μm and silicon oxide powder with a particle size of 0.1μm to 1μm according to The Fe-Co-Si-Al particles were mixed uniformly at a weight ratio of 1:0.25, and then placed in an argon-water vapor mixed atmosphere (the volume ratio of argon to water vapor is 3:7) for treatment at 400°C for 5 hours, and then the silicon oxide powder was sieved out to obtain Fe-Co-Si-Al particles containing a Si-Al composite oxide layer; the Fe-Co-Si-Al particles containing a Si-Al composite oxide layer were placed in a hydrogen atmosphere for annealing at 700°C for 1 hour to form an Al layer on the surface of the Si-Al composite oxide layer, and coated and modified Fe-Co-Si-Al particles were obtained;
[0065] 3) The iron-based amorphous nanocrystalline soft magnetic particles, the coated modified Fe-Co-Si-Al particles and the silicone resin (Silicone resin KR-282 of Shin-Etsu Chemical Co., Ltd.) were mixed uniformly in a weight ratio of 1:1:0.05, and then heated under a pressure of 25 tons / cm 2It is pressed into shape under the conditions of and then sintered at 600℃ in an argon atmosphere for 1h to obtain a magnetic core.
[0066] Embodiment 2:
[0067] An iron-based amorphous nanocrystalline soft magnetic material, the preparation method of which is as follows:
[0068] 1) Fe-Co-Si-Al material (composition: 70.5wt% Fe, 23wt% Co, 4.5wt% Si and 2wt% Al) was added into an electric arc furnace, and nitrogen was filled into the furnace for protection, and then smelted 4 times at a temperature of 1590° C., with a single smelting time of 40 seconds to obtain a melt;
[0069] 2) adding the melt into a vacuum single-roller spinning quenching strip spinning machine, adjusting the rotation speed (linear speed) of the cooling roll to 23 m / s for rapid quenching treatment, and obtaining a Fe-Co-Si-Al amorphous strip (thickness of 40 μm to 55 μm);
[0070] 3) The Fe-Co-Si-Al amorphous strip is placed in a nitrogen atmosphere at a temperature of 550°C for annealing for 20 minutes, and then cooled to 0°C. A pulse laser is used to scan the upper and lower surfaces of the strip line by line at a scanning speed of 20 mm / s. The frequency of the pulse laser is 50 Hz, the pulse width is 20 ms, and the spot diameter is 15 mm, thereby obtaining an iron-based amorphous nanocrystalline soft magnetic material.
[0071] A magnetic core, the preparation method of which is as follows:
[0072] 1) crushing the above-mentioned iron-based amorphous nanocrystalline soft magnetic material to obtain iron-based amorphous nanocrystalline soft magnetic particles (particle size is 35 μm to 55 μm);
[0073] 2) adding Fe-Co-Si-Al material (composition: 70.5wt% Fe, 23wt% Co, 4.5wt% Si and 2wt% Al) into a high frequency furnace for smelting, and then performing ultra-high pressure water atomization to obtain Fe-Co-Si-Al powder with a particle size of 3μm to 50μm; performing air flow classification on the Fe-Co-Si-Al powder, and then taking Fe-Co-Si-Al powder with a particle size of 3μm to 27μm and silicon oxide powder with a particle size of 0.1μm to 1μm according to The mixture is mixed uniformly in a weight ratio of 1:0.15, and then placed in an air-water vapor mixed atmosphere (the volume ratio of air to water vapor is 2:8) for treatment at 500° C. for 3 hours, and then the silicon oxide powder is sieved out to obtain Fe-Co-Si-Al particles containing a Si-Al composite oxide layer; the Fe-Co-Si-Al particles containing a Si-Al composite oxide layer are placed in a hydrogen atmosphere at 650° C. for annealing for 2 hours to form an Al layer on the surface of the Si-Al composite oxide layer, and thus coated and modified Fe-Co-Si-Al particles are obtained;
[0074] 3) The iron-based amorphous nanocrystalline soft magnetic particles, the coated modified Fe-Co-Si-Al particles and the silicone resin (Silicon resin KR-282 of Shin-Etsu Chemical Co., Ltd.) were mixed uniformly in a weight ratio of 1:0.8:0.06, and then heated under a pressure of 25 tons / cm 2 It is pressed into shape under the conditions of and then sintered at 600℃ in an argon atmosphere for 0.5h to obtain a magnetic core.
[0075] Embodiment 3:
[0076] An iron-based amorphous nanocrystalline soft magnetic material, the preparation method of which is as follows:
[0077] 1) Fe-Co-Si-Al material (composition: 65.5wt% Fe, 27wt% Co, 5wt% Si and 2.5wt% Al) was added into an electric arc furnace, and nitrogen was filled into the furnace for protection, and then smelted three times at a temperature of 1640° C., with a single smelting time of 60 s to obtain a melt;
[0078] 2) adding the melt into a vacuum single-roller spinning quenching strip spinning machine, adjusting the rotation speed (linear speed) of the cooling roll to 30 m / s for rapid quenching to obtain a Fe-Co-Si-Al amorphous strip (thickness of 30 μm to 40 μm);
[0079] 3) The Fe-Co-Si-Al amorphous strip was annealed in a nitrogen atmosphere at 560°C for 10 minutes, and then cooled to 5°C. A pulsed laser was used to scan the upper and lower surfaces of the strip line by line at a scanning speed of 30 mm / s. The frequency of the pulsed laser was 50 Hz, the pulse width was 15 ms, and the spot diameter was 20 mm, thereby obtaining an iron-based amorphous nanocrystalline soft magnetic material.
[0080] A magnetic core, the preparation method of which is as follows:
[0081] 1) crushing the above-mentioned iron-based amorphous nanocrystalline soft magnetic material to obtain iron-based amorphous nanocrystalline soft magnetic particles (particle size is 25 μm to 40 μm);
[0082] 2) adding Fe-Co-Si-Al material (composition: 65.5wt% Fe, 27wt% Co, 5wt% Si and 2.5wt% Al) into a high frequency furnace for smelting, and then performing ultra-high pressure water atomization to obtain Fe-Co-Si-Al powder with a particle size of 3μm to 50μm; performing air flow classification on the Fe-Co-Si-Al powder, and then taking Fe-Co-Si-Al powder with a particle size of 3μm to 27μm and alumina powder with a particle size of 0.1μm to 1μm according to The Fe-Co-Si-Al particles were uniformly mixed at a weight ratio of 1:0.05, and then placed in a nitrogen-water vapor mixed atmosphere (the volume ratio of nitrogen to water vapor is 1:9) for treatment at 400°C for 1 hour, and then the aluminum oxide powder was sieved out to obtain Fe-Co-Si-Al particles containing a Si-Al composite oxide layer; the Fe-Co-Si-Al particles containing a Si-Al composite oxide layer were annealed at 600°C for 3 hours in a hydrogen atmosphere to form an Al layer on the surface of the Si-Al composite oxide layer, and coated and modified Fe-Co-Si-Al particles were obtained;
[0083] 3) The iron-based amorphous nanocrystalline soft magnetic particles, the coated modified Fe-Co-Si-Al particles and the silicone resin (Silicone resin KR-282 of Shin-Etsu Chemical Co., Ltd.) were mixed uniformly in a weight ratio of 1:1.3:0.08, and then heated under a pressure of 25 tons / cm 2 It is pressed into shape under the conditions of and then sintered at 650℃ in an argon atmosphere for 0.5h to obtain the magnetic core.
[0084] Embodiment 4:
[0085] An iron-based amorphous nanocrystalline soft magnetic material, the preparation method of which is as follows:
[0086] 1) Fe-Co-Si-Al material (composition: 72wt% Fe, 22wt% Co, 4wt% Si and 2wt% Al) is added into an electric arc furnace, and filled with nitrogen for protection, and then smelted 4 times at a temperature of 1600° C., with a single smelting time of 45 seconds to obtain a melt;
[0087] 2) adding the melt into a vacuum single-roller spinning quenching strip spinning machine, adjusting the rotation speed (linear speed) of the cooling roll to 25 m / s for rapid quenching to obtain a Fe-Co-Si-Al amorphous strip (thickness of 40 μm to 50 μm);
[0088] 3) The Fe-Co-Si-Al amorphous strip was annealed in a nitrogen atmosphere at a temperature of 550°C for 15 minutes, and then cooled to 0°C. A pulsed laser was used to scan the upper and lower surfaces of the strip line by line at a scanning speed of 25 mm / s. The frequency of the pulsed laser was 50 Hz, the pulse width was 20 ms, and the spot diameter was 15 mm, thereby obtaining an iron-based amorphous nanocrystalline soft magnetic material.
[0089] A magnetic core, the preparation method of which is as follows:
[0090] 1) crushing the above-mentioned iron-based amorphous nanocrystalline soft magnetic material to obtain iron-based amorphous nanocrystalline soft magnetic particles (particle size is 35 μm to 50 μm);
[0091] 2) adding Fe-Co-Si-Al material (composition: 72wt% Fe, 22wt% Co, 4wt% Si and 2wt% Al) into a high frequency furnace for smelting, and then performing ultra-high pressure water atomization to obtain Fe-Co-Si-Al powder with a particle size of 3μm to 50μm; performing air flow classification on the Fe-Co-Si-Al powder, and then taking Fe-Co-Si-Al powder with a particle size of 3μm to 27μm and silicon oxide powder with a particle size of 0.1μm to 1μm according to weight The Fe-Co-Si-Al particles are uniformly mixed in a volume ratio of 1:0.15, and then placed in an argon-water vapor mixed atmosphere (the volume ratio of argon to water vapor is 2:8) at 550°C for 3 hours, and then the silicon oxide powder is sieved out to obtain Fe-Co-Si-Al particles containing a Si-Al composite oxide layer; the Fe-Co-Si-Al particles containing a Si-Al composite oxide layer are placed in a hydrogen atmosphere at 650°C for annealing for 2 hours to form an Al layer on the surface of the Si-Al composite oxide layer, and thus coated and modified Fe-Co-Si-Al particles are obtained;
[0092] 3) The iron-based amorphous nanocrystalline soft magnetic particles, the coated modified Fe-Co-Si-Al particles and the silicone resin (Silicone resin KR-282 of Shin-Etsu Chemical Co., Ltd.) were mixed uniformly in a weight ratio of 1:1:0.06, and then heated under a pressure of 25 tons / cm 2 It is pressed into shape under the conditions of and then sintered at 600℃ in an argon atmosphere for 1h to obtain a magnetic core.
[0093] Comparative Example 1: (Fe-Co-Si-Al particles without coating modification)
[0094] A magnetic core, the preparation method of which is as follows:
[0095] The iron-based amorphous nanocrystalline soft magnetic particles (same as in Example 4) and silicone resin (Silicone resin KR-282 produced by Shin-Etsu Chemical Co., Ltd.) were mixed uniformly in a weight ratio of 1:0.03 and then heated under a pressure of 25 tons / cm 2It is pressed into shape under the conditions of and then sintered at 600℃ in an argon atmosphere for 1h to obtain a magnetic core.
[0096] Comparative Example 2: (without iron-based amorphous nanocrystalline soft magnetic particles)
[0097] A magnetic core, the preparation method of which is as follows:
[0098] The coated modified Fe-Co-Si-Al particles (same as in Example 4) and silicone resin (Silicon resin KR-282 from Shin-Etsu Chemical Co., Ltd.) were mixed uniformly at a weight ratio of 1:0.03 and then heated under a pressure of 25 tons / cm 2 It is pressed into shape under the conditions of and then sintered at 600℃ in an argon atmosphere for 1h to obtain a magnetic core.
[0099] Comparative Example 3: (Laser induced treatment was carried out at room temperature)
[0100] An iron-based amorphous nanocrystalline soft magnetic material is exactly the same as Example 4 except that the temperature of the laser induced treatment is replaced from "0°C" to "room temperature (25°C±5°C)" during preparation.
[0101] A magnetic core, the preparation method of which is as follows:
[0102] 1) crushing the above-mentioned iron-based amorphous nanocrystalline soft magnetic material to obtain iron-based amorphous nanocrystalline soft magnetic particles (particle size is 35 μm to 50 μm);
[0103] 2) The iron-based amorphous nanocrystalline soft magnetic particles, the coated modified Fe-Co-Si-Al particles (same as in Example 4) and the silicone resin (Silicon resin KR-282 of Shin-Etsu Chemical Co., Ltd.) were mixed uniformly in a weight ratio of 1:1:0.06, and then heated under a pressure of 25 tons / cm 2 It is pressed into shape under the conditions of and then sintered at 600℃ in an argon atmosphere for 1h to obtain a magnetic core.
[0104] Comparative Example 4: (without laser induction treatment)
[0105] An iron-based amorphous nanocrystalline soft magnetic material is completely the same as Example 4 except that no laser induced treatment is performed during preparation.
[0106] A magnetic core, the preparation method of which is as follows:
[0107] 1) crushing the above-mentioned iron-based amorphous nanocrystalline soft magnetic material to obtain iron-based amorphous nanocrystalline soft magnetic particles (particle size is 35 μm to 50 μm);
[0108] 2) The iron-based amorphous nanocrystalline soft magnetic particles, the coated modified Fe-Co-Si-Al particles (same as in Example 4) and the silicone resin (Silicon resin KR-282 of Shin-Etsu Chemical Co., Ltd.) were mixed uniformly in a weight ratio of 1:1:0.06, and then heated under a pressure of 25 tons / cm 2 It is pressed into shape under the conditions of and then sintered at 600℃ in an argon atmosphere for 1h to obtain a magnetic core.
[0109] Performance Testing:
[0110] The performance test results of the magnetic cores of Examples 1 to 4 and Comparative Examples 1 to 4 are shown in the following table:
[0111] Table 1 Performance test results of the magnetic cores of Examples 1 to 4 and Comparative Examples 1 to 4
[0112]
[0113] Note:
[0114] Bending strength: The size of the test specimen is 35mm×4mm×3mm. It is tested on a universal testing machine with a test span of 30mm and a displacement loading rate of 0.5mm / min.
[0115] Magnetic permeability and inductance drop rate: The test sample is ring-shaped, with an outer diameter of 20mm, an inner diameter of 12mm, a height of 2mm, and a winding number of N=13Ts turns. The effective magnetic permeability μ of the magnetic ring sample is tested using a 3260B LCR tester. e (The test frequencies are 10KHz, 50KHz and 100KHz respectively), and the decrease rate of inductance under the equivalent magnetic field strength of DC field H of 100Oe relative to H of 0Oe is tested.
[0116] From Table 1, we can see that:
[0117] 1) The magnetic cores of Examples 1 to 4 have high bending strength, high and small differences in magnetic permeability at high and low frequencies, small inductance change rate at high saturation magnetic field strength, and long-lasting and stable performance, and are suitable for use as magnetic cores in photovoltaic inverters;
[0118] 2) The bending strength, high frequency and low frequency magnetic permeability of the magnetic core of Comparative Example 1 (without adding the coated modified Fe-Co-Si-Al particles) and the magnetic core of Comparative Example 2 (without adding the iron-based amorphous nanocrystalline soft magnetic particles) are significantly lower than those of the magnetic core of Example 4, and the difference in magnetic permeability at high frequency and low frequency is greater, the inductance change rate at high saturation magnetic field strength is greater, and the performance stability is much worse, indicating that the coated modified Fe-Co-Si-Al particles and the iron-based amorphous nanocrystalline soft magnetic particles work synergistically and are indispensable;
[0119] 3) The bending strength, high frequency and low frequency magnetic permeability of the magnetic core of Comparative Example 3 (the iron-based amorphous nanocrystalline soft magnetic material was laser-induced at room temperature during preparation) were significantly lower than those of the magnetic core of Example 4, and the difference in magnetic permeability at high frequency and low frequency was greater, the inductance change rate at high saturation magnetic field strength was greater, and the performance stability was much worse, indicating that the laser-induced treatment needs to be carried out at a lower temperature (0°C to 5°C) to achieve a good effect;
[0120] 4) The bending strength and magnetic permeability at high and low frequencies of the magnetic core of Comparative Example 4 (the iron-based amorphous nanocrystalline soft magnetic material was not subjected to laser induced treatment during preparation) are significantly lower than those of the magnetic core of Example 4, and the difference in magnetic permeability at high and low frequencies is greater, the rate of change of inductance at high saturation magnetic field strength is greater, and the performance stability is much worse, indicating that laser induced treatment is crucial for refining the grains in iron-based amorphous nanocrystalline soft magnetic materials.
[0121] The above embodiments are preferred implementation modes of the present invention, but the implementation modes of the present invention are not limited to the above embodiments. Any other changes, modifications, substitutions, combinations, and simplifications that do not deviate from the spirit and principles of the present invention should be equivalent replacement methods and are included in the protection scope of the present invention.
Claims
1. A method for preparing an iron-based amorphous nanocrystalline soft magnetic material, characterized in that: The following steps are involved: 1) placing the Fe-Co-Si-Al material in a protective atmosphere for smelting to obtain a melt; 2) adding the melt into a vacuum single-roller spinning quenching machine for rapid quenching to obtain a Fe-Co-Si-Al amorphous strip; 3) The Fe-Co-Si-Al amorphous strip is placed in a protective atmosphere at a temperature of 520°C to 570°C for annealing, and then the temperature is lowered to 0°C to 5°C, and then both sides of the strip are laser-induced treated with a pulsed laser to obtain an iron-based amorphous nanocrystalline soft magnetic material.
2. The preparation method according to claim 1, characterized in that: Step 1) The Fe-Co-Si-Al material comprises the following components in weight percentage: Fe: 65.5%~75.5%; Co: 20%-27%; Si: 3% to 5%; Al:1.5%~2.5%。 3. The preparation method according to claim 1 or 2, characterized in that: Step 1) The smelting is carried out at a temperature of 1550° C. to 1650° C., the number of smelting is 3 to 5 times, and the time of a single smelting is 30s to 60s.
4. The preparation method according to claim 1, characterized in that: Step 2) The rapid quenching treatment is carried out under the condition that the rotation speed of the cooling roller of the vacuum single-roller spinning quenching machine is 20m / s to 30m / s; Step 2) The thickness of the Fe-Co-Si-Al amorphous strip is 30μm to 60μm.
5. The preparation method according to claim 1, characterized in that: Step 3) The annealing treatment time is 10 min to 20 min.
6. The preparation method according to claim 1 or 5, characterized in that: Step 3) The frequency of the pulse laser is 50Hz~100Hz, the pulse width is 10ms~30ms, and the spot diameter is 10mm~20mm; Step 3) The operation of the laser induced treatment is: use a pulse laser to scan the surface of the strip line by line at a scanning speed of 15mm / s~35mm / s.
7. An iron-based amorphous nanocrystalline soft magnetic material, characterized in that: Prepared by the preparation method according to any one of claims 1 to 6.
8. A magnetic core, characterized in that: The composition includes iron-based amorphous nanocrystalline soft magnetic particles, coated modified Fe-Co-Si-Al particles and silicone resin in a weight ratio of 1:0.5 to 1.5:0.03 to 0.08; the iron-based amorphous nanocrystalline soft magnetic particles are made by crushing the iron-based amorphous nanocrystalline soft magnetic material according to claim 7; the coated modified Fe-Co-Si-Al particles are composed of a Fe-Co-Si-Al core, a Si-Al composite oxide layer and an Al layer from the inside to the outside.
9. A photovoltaic inverter, characterized in that: The magnetic core comprising the magnetic core as claimed in claim 8.
10. A photovoltaic power generation system, characterized in that: A photovoltaic inverter comprising the method of claim 9.
Citation Information
Patent Citations
Laser inducement nano-surface preparation method for iron based amorphous nanocrystalline soft magnetic material
CN101509053A
Iron-based nanocrystalline soft magnetic alloy with high saturation magnetic induction and low cost
CN102304669A
Amorphous nanocrystalline high-entropy soft magnetic alloy and preparation method thereof
CN108396262A
Iron-based amorphous-nanocrystalline magnetically soft alloy and strip and preparation method thereof
CN116313356A
Iron-cobalt magnetic core and preparation method and application thereof
CN116825468A