Method for preparing micron-sized spherical nickel powder from mixed nickel source
Through liquid phase reduction method without the assistance of hard template, using mixed nickel source aqueous solution and surfactant, micron-sized spherical nickel powder with uniform particle size and good morphology is prepared, which solves the problem of particle size and morphology in the existing technology. Problems that are difficult to control have been solved, and low-cost, efficient industrial production has been achieved.
Patent Information
- Application Number
- CN202411159886.4
- Authority / Receiving Office
- CN · China
- Patent Type
- Applications(China)
- Current Assignee / Owner
- Filing Date
- 2024-08-22
- Publication Date
- 2024-10-15
- Estimated Expiration
- 2044-08-22
AI Technical Summary
In the existing technology, the particle size and morphology of fine nickel powder are difficult to control, burrs or roughness are easily formed on the particle surface during the reaction process, the reaction rate is difficult to control, and the cost is high, making it difficult to achieve industrial production.
Using the liquid phase reduction method without the assistance of a hard template, prepare a mixed nickel source aqueous solution, add the stabilizer nickel sulfate hexahydrate and a surfactant, and use a peristaltic pump dripping method to prepare micron-sized spherical nickel powder at normal pressure and low temperature. The steps Simple and low equipment requirements.
The preparation of micron-sized spherical nickel powder with a particle size of 1 μm-4 μm has been achieved. The particle size and morphology have significant advantages, solving the problems of unstable reaction rate and high cost, and is suitable for large-scale industrial production.
Smart Images

Figure CN118768563A_ABST
Abstract
Description
Technical Field
[0001] The invention relates to the technical field of nickel powder preparation, in particular to a method for preparing micron-sized spherical nickel powder by mixing nickel sources. Background Art
[0002] Fine nickel powder has great surface effect and volume effect, and shows many special properties in magnetism, internal pressure, thermal resistance, light absorption, chemical activity, etc. As a new material, it has broad application prospects in catalysts, power electrode materials, multilayer ceramic capacitors, conductive fibers, cemented carbide materials, absorption materials, etc., and has become one of the hot spots for the development of new functional materials at home and abroad; in addition, compared with ultrafine nickel powder, fine nickel powder is more conducive to achieving the effect of good coating and uniform coating in the process of preparing silver-coated nickel for conductive slurry technology by chemical plating. However, in the current production process, fine powder has problems such as difficult to control particle size and morphology, too fast reduction rate during the reaction, easy formation of burrs or rough surface on the particle surface, easy agglomeration when adding special reagents to reduce the reaction rate, high technical requirements and high costs, so it is difficult to achieve industrial production.
[0003] In the prior art, a nickel salt is often used as a reaction nickel source, and the reductant selection requires a variety of reductants to be mixed and used, and the operation is relatively complicated. And in the liquid phase reduction system, special reagents are required to provide mild conditions to promote the generation of nickel particle crystals and slowly grow into micron particles, but the standard potential of nickel ions is lower than that of precious metals, and conventional weak reductants cannot be reduced, so it is necessary to use strong reductants such as hydrazine hydrate and potassium borohydride for reduction synthesis, and strong reductants will also increase the reaction rate in the process of promoting nickel ion reduction, resulting in the reaction rate of micron-sized nickel powder particles cannot be controlled, and the phenomenon is severe. Therefore, for the production of micron-sized nickel powder, it is still necessary to have simple operation, a relatively mild reaction process, low equipment requirements and a controllable morphology preparation method. Therefore, it is of great significance to explore the industrial production of micron-sized nickel powder products with high purity, dispersion and uniform particle size distribution and spherical structure. Summary of the invention
[0004] Purpose of the invention: The present invention proposes a method for preparing micron-sized spherical nickel powder by mixing nickel sources, the purpose of which is to solve the problems existing in the prior art.
[0005] Technical solution: The present invention proposes a method for preparing micron-sized spherical nickel powder by mixing nickel sources, using a liquid phase reduction method, without the assistance of a hard template, to prepare micron-sized spherical nickel powder with a particle size of 1 μm-4 μm; the method comprises the following steps:
[0006] Step 1, preparing a mixed nickel source aqueous solution, using nickel chloride hexahydrate as the main nickel source, supplemented with nickel sulfate hexahydrate as a stabilizer, mixing with deionized water at a molar ratio of (1-4):1, and stirring with ultrasonic to dissolve evenly to obtain solution A;
[0007] Step 2: prepare a sodium hydroxide aqueous solution, mix sodium hydroxide and deionized water, stir and dissolve evenly, and obtain solution B;
[0008] Step 3, adding a surfactant to solution A, and subjecting the solution to ultrasonic stirring to mix the solution uniformly, to obtain solution C;
[0009] Step 4: Preheat solution C in a water bath, pump solution B into solution C using a peristaltic pump, and stir evenly to obtain solution D;
[0010] Step 5, adding a reducing agent to solution D, stirring to mix evenly, heating in a water bath for reaction, ultrasonic treatment and cooling to room temperature to obtain product E;
[0011] Step 6: After solid-liquid separation, the product E is washed with water, washed with alcohol and vacuum dried to obtain micron-sized spherical nickel powder.
[0012] Furthermore, the nickel ion concentration of solution A in step 1 is 0.035 mol / L-0.8 mol / L; and the concentration of solution B in step 2 is 0.15-0.95 mol / L.
[0013] Furthermore, in step three, the surfactant is polyvinyl pyrrolidone.
[0014] Furthermore, in the step three, the mass ratio of the added amount of the surfactant to the nickel source is 1:(2.5-2.8).
[0015] Furthermore, in step 4, the preheating temperature of the water bath is 80-90°C.
[0016] Furthermore, in the step 5, the reducing agent is hydrazine hydrate.
[0017] Furthermore, the concentration of the reducing agent in step five is 0.38-1.44 mol / L.
[0018] Furthermore, in step 5, the temperature of the heating reaction is 70-90° C., and the heating reaction time is 2-4 hours.
[0019] Furthermore, the heating reaction in step 5 is carried out in a water bath.
[0020] Furthermore, in step six, the vacuum drying temperature is 60° C., and the vacuum drying time is 12 h.
[0021] Beneficial effects:
[0022] 1. Compared with the prior art, this method prepares micron-sized spherical nickel powder by separately preparing a mixed nickel salt solution and a reducing solution and adopting a peristaltic pump dropwise addition method at normal pressure and a relatively low temperature. It has low equipment requirements, simple operation steps and strong operability.
[0023] 2. Compared with the existing technology, this method ensures the single nickel source NiCl 2 6H 2 O as the main nickel source, by adding stabilizer NiSO 4 6H 2 O, which increases the concentration of nickel ions in the nickel source aqueous solution and increases the output, while assisting NiCl 2 6H 2 O achieves a stable reaction, overcoming the existing use of NiCl 2 6H 2 O The problem of unstable reaction rate and high energy consumption in preparing nickel powder with a single nickel source.
[0024] 3. Compared with the prior art, this method, by adding stabilizer NiSO 4 6H 2 The micron-sized spherical nickel powder prepared by mixing the mixed nickel source aqueous solution with the addition ratio of (1-4): 1 has significant advantages in nickel powder particle size, nickel powder morphology, etc., and solves the problem of uncontrollable reaction in the prior art. In addition, the steps are closely linked, and the raw material ratio is properly arranged, which not only maintains good performance but also ensures the production efficiency of the reaction product, and meets the needs of large-scale industrial production in the fields of conductive slurries, battery materials, magnetic materials, wave absorbing and special coatings. BRIEF DESCRIPTION OF THE DRAWINGS
[0025] Figure 1 This is the SEM image of the spherical micron nickel powder prepared in Example 1 (*20000);
[0026] Figure 2 This is the SEM image (*4000) of the spherical micron nickel powder prepared in Example 1;
[0027] Figure 3 This is the SEM image of the spherical micron nickel powder prepared in Example 2 (*10000);
[0028] Figure 4 The SEM image of the spherical micron nickel powder prepared in Example 2 (*2000);
[0029] Figure 5 This is the SEM image of the spherical micron nickel powder prepared in Example 3 (*20000);
[0030] Figure 6 This is the SEM image (*4000) of the spherical micron nickel powder prepared in Example 3;
[0031] Figure 7 This is the SEM image of the spherical micron nickel powder prepared in Comparative Example 1 (*20000);
[0032] Figure 8 This is the SEM image of the spherical micron nickel powder prepared in Comparative Example 1 (*4000). DETAILED DESCRIPTION
[0033] In order to make the technical means, creative features, objectives and effects of the present invention easy to understand, the technical solutions in the embodiments of the present invention will be clearly and completely described below in conjunction with the drawings in the embodiments of the present invention. Obviously, the described embodiments are only part of the embodiments of the present invention, not all of them. Based on the embodiments of the present invention, all other embodiments obtained by ordinary technicians in this field without creative work are within the scope of protection of the present invention.
[0034] Example 1
[0035] This embodiment adopts a liquid phase reduction method to prepare micron-sized spherical nickel powder with a particle size of 1-3 μm without the assistance of a hard template, comprising the following steps:
[0036] Step 1: 0.08 mol NiCl 2 6H 2 O and 0.02mol NiSO 4 6H 2 O (addition ratio is 4:1) is dissolved in 125g deionized water, ultrasonically mixed, and then 7.5g PVP is added and ultrasonically stirred to obtain solution A; 0.15mol NaOH is dissolved in 125g deionized water and uniformly mixed to obtain solution B;
[0037] Step 2: preheat solution A in a water bath at 80°C, pump solution B into solution A at a pumping speed of 40 ml / min using a peristaltic pump after reaching the preheating temperature, stir with a stirring paddle for 3 h, then add 0.26 mol of 80% hydrazine hydrate and stir evenly, heat at 80°C for 1 h, sonicate for 30 min after the reaction is completed, and cool to room temperature (25°C);
[0038] Step 3: Pour off the supernatant, wash the crude product with water until the conductivity drops below 5 μs / cm, wash it twice with anhydrous ethanol, and dry it in a vacuum drying oven at 60°C for 12 hours to obtain micron-sized spherical nickel powder with a particle size of 1-3 μm.
[0039] Example 2
[0040] This embodiment adopts a liquid phase reduction method to prepare micron-sized spherical nickel powder with a particle size of 1-4 μm without the assistance of a hard template, comprising the following steps:
[0041] Step 1: 0.14 mol NiCl 2 6H 2 O and 0.06mol NiSO 4 6H 2 O (addition ratio is 2.3:1) is dissolved in 250g water and uniformly mixed by ultrasonic, then 6.8g PVP is added and uniformly stirred by ultrasonic to obtain solution A; 0.12mol NaOH is dissolved in 250g water and uniformly mixed to obtain solution B;
[0042] Step 2: preheat solution A in a 90°C water bath, pump solution B into solution A using a peristaltic pump at a pumping speed of 40 ml / min after reaching the preheating temperature, stir with a stirring paddle for 1.5 h, then add 0.28 mol of 80% hydrazine hydrate and stir evenly, heat at 90°C for 3 h, sonicate for 30 min after the reaction is completed, and cool to room temperature (25°C);
[0043] Step 3: Pour off the supernatant, wash the crude product with water until the conductivity drops below 5 μs / cm, wash it twice with anhydrous ethanol, and dry it in a vacuum drying oven at 60°C for 12 hours to obtain micron-sized spherical nickel powder with a particle size of 1-4 μm.
[0044] Example 3
[0045] This embodiment adopts a liquid phase reduction method to prepare micron-sized spherical nickel powder with a particle size of 1.5-2 μm without the assistance of a hard template, comprising the following steps:
[0046] Step 1: 0.2 mol NiCl 2 6H 2 O and 0.2 mol NiSO 4 6H 2 O (addition ratio is 1:1) is dissolved in 500g water and uniformly mixed by ultrasonic, then 8.8g PVP is added and uniformly stirred by ultrasonic to obtain solution A; 0.6mol NaOH is dissolved in 500g water and uniformly mixed to obtain solution B;
[0047] Step 2: preheat solution A in a water bath at 80°C, pump solution B into solution A at a pumping speed of 40 ml / min using a peristaltic pump after reaching the preheating temperature, stir for 3 hours using a stirring paddle, then add 0.78 mol of 80% hydrazine hydrate and stir evenly, heat at 90°C for 3 hours, sonicate for 30 minutes after the reaction is completed, and cool to room temperature (25°C);
[0048] Step 3: Pour off the supernatant, wash the crude product with water until the conductivity drops below 5 μs / cm, wash it twice with anhydrous ethanol, and dry it in a vacuum drying oven at 60°C for 12 hours to obtain micron-sized spherical nickel powder with a particle size of 1.5-2 μm.
[0049] Comparative Example 1
[0050] This embodiment adopts a liquid phase reduction method to prepare micron-sized spherical nickel powder with a particle size of 1.5-2 μm without the assistance of a hard template, comprising the following steps:
[0051] Step 1: 0.4 mol NiCl 2 6H 2 O was dissolved in 500 g of water and uniformly mixed by ultrasonication, and then 5 g of PVP was added and uniformly stirred by ultrasonication to obtain solution A; 0.3 mol of NaOH was dissolved in 500 g of water and uniformly mixed to obtain solution B;
[0052] Step 2: preheat solution A in a water bath at 80°C, pump solution B into solution A at a pumping speed of 40 ml / min using a peristaltic pump after reaching the preheating temperature, stir the mixture for 3 h using a stirring paddle, then add 0.5 mol of 80% hydrazine hydrate and stir evenly, heat at 90°C for 30 min, react until overflowing, sonicate for 30 min, and cool to room temperature (25°C);
[0053] Step 3: Pour off the supernatant, wash the crude product with water until the conductivity drops below 5 μs / cm, wash it twice with anhydrous ethanol, and dry it in a vacuum drying oven at 60°C for 12 hours to obtain micron-sized spherical nickel powder with a particle size of about 1.5-2 μm.
[0054] The nickel sources in Examples 1-3 are all NiCl 2 6H 2 O is the main nickel source, NiSO 4 6H 2 O is a stabilizer, and the two are mixed in a ratio of (1-4): 1 to prepare a mixed nickel source aqueous solution with a nickel ion concentration of 0.8 mol / L, and micron-sized spherical nickel powder is prepared by mixing the nickel source aqueous solution. Figures 1 to 6 It can be seen that the addition of stabilizer NiSO 4 6H 2O, and NiCl 2 6H 2 O and NiSO 4 6H 2 O addition ratio was controlled at (1-4):1 to obtain a mixed nickel source aqueous solution. During the experiment, NiSO 4 6H 2 O, compared with the addition of other stabilizers, NiSO 4 6H 2 O not only provides additional Ni 2+ , and in SO 4 2- Adjust the reaction rate to be stable and controllable. 4 6H 2 O assisted stabilization, the prepared spherical micron nickel particles have an average particle size of 1-4 μm, and have a complete spherical structure, a smooth particle surface, a controllable particle size and a narrow distribution, high purity and a large specific surface area; Comparative Example 1 is relative to Examples 1-3, only a single nickel source NiCl 2 6H 2 O prepared a nickel source aqueous solution with a nickel ion concentration of 0.8 mol / L. Specifically, no stabilizer was added to the nickel source aqueous solution prepared in Comparative Example 1, resulting in the experimental process relying only on NiCl 2 6H 2 O aqueous solution, the reaction rate is unstable and Figure 7 , Figure 8 It can be seen that the prepared spherical micron nickel particles have incomplete spherical structures and are even adhered to each other. The particle surface is not smooth, the particle size is difficult to control, the distribution range is large, the purity is low, and the specific surface area is small.
[0055] In general, the method of the present invention improves the existing method of using NiCl 2 6H 2 The method of preparing nickel powder with a single nickel source is unstable, the particle size of the prepared nickel powder and the morphology of the nickel powder are uncontrollable, and the stabilizer NiSO is added 4 6H 2 O, and the mixed nickel source aqueous solution obtained by adding (1-4): 1 has significant advantages in nickel powder particle size, nickel powder morphology, etc. This method adds a stabilizer NiSO 4 6H 2 O, while ensuring that NiCl 2 6H 2O as the main nickel source, not only the nickel ion concentration is increased, the output is improved, but also the reaction system is stabilized, effectively solving the problem of unstable reaction rate in the traditional single nickel source preparation. Moreover, the steps are closely linked, and the raw material ratio is properly arranged, which not only maintains good performance, but also ensures the production efficiency of the reaction product, meeting the needs of large-scale industrial production.
[0056] The above are only embodiments of the present application and are not intended to limit the present application. For those skilled in the art, the present application may have various changes and variations. Any modification, equivalent replacement, improvement, etc. made within the spirit and principle of the present application should be included within the scope of the claims of the present application.
Claims
1. A method for preparing micron-sized spherical nickel powder by mixing nickel sources, characterized in that: A micron-sized spherical nickel powder with a particle size of 1 μm to 4 μm is prepared by a liquid phase reduction method without the assistance of a hard template. The method comprises the following steps: Step 1, preparing a mixed nickel source aqueous solution, using nickel chloride hexahydrate as the main nickel source, supplemented with nickel sulfate hexahydrate as a stabilizer, mixing with deionized water at a molar ratio of (1-4):1, and stirring with ultrasonic to dissolve evenly to obtain solution A; Step 2: prepare a sodium hydroxide aqueous solution, mix sodium hydroxide and deionized water, stir and dissolve evenly, and obtain solution B; Step 3, adding a surfactant to solution A, and subjecting the solution to ultrasonic stirring to mix the solution uniformly, to obtain solution C; Step 4: Preheat solution C in a water bath, pump solution B into solution C using a peristaltic pump, and stir evenly to obtain solution D; Step 5, adding a reducing agent to solution D, stirring to mix evenly, heating in a water bath for reaction, ultrasonic treatment and cooling to room temperature to obtain product E; Step 6: After solid-liquid separation, the product E is washed with water, washed with alcohol and vacuum dried to obtain micron-sized spherical nickel powder.
2. The method for preparing micron-sized spherical nickel powder by mixing nickel sources according to claim 1, characterized in that: The nickel ion concentration in solution A in step 1 is 0.035 mol / L-0.8 mol / L; the concentration of solution B in step 2 is 0.15-0.95 mol / L.
3. The method for preparing micron-sized spherical nickel powder by mixing nickel sources according to claim 1, characterized in that: The surfactant in step three is polyvinyl pyrrolidone.
4. The method for preparing micron-sized spherical nickel powder by mixing nickel sources according to claim 1, characterized in that: The mass ratio of the added amount of the surfactant to the nickel source in the step three is 1:(2.5-2.8).
5. The method for preparing micron-sized spherical nickel powder by mixing nickel sources according to claim 1, characterized in that: The preheating temperature of the water bath in step 4 is 80-90°C.
6. The method for preparing micron-sized spherical nickel powder by mixing nickel sources according to claim 1, characterized in that: In the step 5, the reducing agent is hydrazine hydrate.
7. The method for preparing micron-sized spherical nickel powder by mixing nickel sources according to claim 1, characterized in that: The concentration of the reducing agent in step 5 is 0.38-1.44 mol / L.
8. The method for preparing micron-sized spherical nickel powder by mixing nickel sources according to claim 1, characterized in that: The temperature of the heating reaction in step 5 is 70-90° C., and the heating reaction time is 2-4 hours.
9. The method for preparing micron-sized spherical nickel powder by mixing nickel sources according to claim 1, characterized in that: The heating reaction in step 5 is carried out by water bath heating reaction.
10. The method for preparing micron-sized spherical nickel powder by mixing nickel sources according to claim 1, characterized in that: The vacuum drying temperature in step 6 is 60° C. and the vacuum drying time is 12 h.
Citation Information
Patent Citations
Method for preparing spherical submicron nickel powder with controllable particle size
CN102554259A
Method of preparing micron-sized spherical high-purity nickel powder
CN102699348A
Method for synthesizing superfine single crystal nickel powder by solvothermal method
CN110947979A
Production of fine nickel powder
JP1993051610A
Method for manufacturing nano-scale nickel powders bywet reducing process