A method for preparing nickel element

Through hydrolysis neutralization, heating, ammonia washing and water washing treatment under nitrogen protection, combined with the reduction treatment of hydrazine hydrate, the problem of loss of nickel elements and purity in the preparation of nickel element as raw material nickel is solved. High yield and high purity nickel element preparation is achieved.

CN118768580BActive Publication Date: 2024-11-15RES INST OF PHYSICAL & CHEM ENG OF NUCLEAR IND
View PDF 5 Cites 0 Cited by

Patent Information

Application Number
CN202411260227.X
Authority / Receiving Office
CN · China
Patent Type
Patents(China)
Current Assignee / Owner
Filing Date
2024-09-10
Publication Date
2024-11-15
Estimated Expiration
2044-09-10

AI Technical Summary

Technical Problem

It is difficult for the prior art to efficiently prepare high-yield nickel element with tetrafluorophosphine as raw material, and there are problems of nickel element loss and product purity not meeting standards during the preparation of nickel-62 element.

Method used

Ammonia water is used for hydrolysis and neutralization reaction, and heat, ammonia and water washing are carried out under nitrogen protection conditions. Combined with the reduction treatment of hydrazine hydrate, nickel element is gradually obtained to ensure the recovery of nickel ions and product purity.

Benefits of technology

The output rate of nickel element is improved, the product purity reaches more than 97%, meeting the use requirements of nickel batteries and reducing the loss of nickel elements.

✦ Generated by Eureka AI based on patent content.

Smart Images

  • Figure CN118768580B_ABST
    Figure CN118768580B_ABST
Patent Text Reader

Abstract

The present invention provides a method for preparing a nickel single substance, which belongs to the technical field of preparing a nickel single substance. The method solves the technical problem of preparing a qualified and high-yield nickel single substance product using tetrakis(trifluorophosphine)nickel as a raw material. The method comprises: providing ammonia water; adding tetrakis(trifluorophosphine)nickel to the ammonia water, and performing a hydrolysis neutralization reaction and a heating process under the condition of nitrogen protection to obtain a first nickel solid and a reaction liquid; adding hydrazine hydrate to the reaction liquid for reduction treatment to obtain a second nickel solid; adding ammonia water to the first nickel solid and the second nickel solid, and performing ammonia washing treatment under the condition of nitrogen protection to obtain a third nickel solid and ammonia washing liquid; adding hydrazine hydrate to the ammonia washing liquid for reduction treatment to obtain a fourth nickel solid; adding ultrapure water to the third nickel solid and the fourth nickel solid for water washing treatment, and drying to obtain a nickel single substance. The method for preparing a nickel single substance provided by the present invention has a high yield of qualified products, and the product purity can meet the use requirements of nickel batteries.
Need to check novelty before this filing date? Find Prior Art

Description

Technical Field

[0001] The invention relates to the technical field of nickel element preparation, in particular to a method for preparing nickel element. Background Art

[0002] Nickel-63 is the preferred material for making radioisotope batteries. It is usually obtained by irradiating the stable isotope nickel-62 in a nuclear reactor. In order to obtain nickel-62, the enriched nickel-62 tetrakis(trifluorophosphine) needs to be converted. In order to meet the requirements of nickel-62 irradiation, the nickel-62 content to be prepared should not be less than 99%. At the same time, in order to achieve the requirements of high conversion rate, the loss of nickel-62 isotope should be reduced as much as possible.

[0003] In order to meet the above needs, it is necessary to use nickel tetrakis(trifluorophosphine) as a raw material to prepare qualified and high-yield nickel. According to the existing technology, the method of obtaining nickel by heating and decomposing nickel tetrakis(trifluorophosphine) can only achieve an output rate of about 20%; the nickel prepared by hydrolysis and neutralization must undergo ammonia washing and other treatment processes to reduce the phosphorus content in the product to ensure that the product purity meets the standard, but according to the current preparation process, the output rate can only reach about 70%, which is far from meeting the use requirements; the method of preparing high-yield nickel using nickel tetrakis(trifluorophosphine) as a raw material is still in a blank stage. Summary of the invention

[0004] The invention provides a method for preparing nickel single substance, which solves the technical problem of preparing a qualified nickel single substance product with high yield by using nickel tetrakis(trifluorophosphine) as a raw material.

[0005] In order to solve the above technical problems, the technical solution of the present invention is as follows:

[0006] A method for preparing nickel element, comprising:

[0007] Provide ammonia;

[0008] Adding tetrakis(trifluorophosphine)nickel into the ammonia water, and subjecting the mixture to a hydrolysis and neutralization reaction and a heating process under nitrogen protection to obtain a first nickel solid and a reaction liquid;

[0009] Adding hydrazine hydrate to the reaction solution for reduction treatment to obtain a second nickel solid;

[0010] Adding ammonia water to the first nickel solid and the second nickel solid, and performing ammonia washing treatment under nitrogen protection to obtain a third nickel solid and ammonia washing solution;

[0011] Adding hydrazine hydrate to the ammonia wash solution for reduction treatment to obtain a fourth nickel solid;

[0012] The third nickel solid and the fourth nickel solid are added with ultrapure water for washing, and then dried to obtain nickel element.

[0013] Optionally, tetrakis(trifluorophosphine)nickel is added to the ammonia water, and subjected to a hydrolysis neutralization reaction and a heating process under nitrogen protection to obtain a first nickel solid and a reaction liquid, comprising:

[0014] Pour the ammonia water into a reaction kettle, adjust the internal temperature of the reaction kettle to a first preset temperature, and introduce nitrogen for a first preset time;

[0015] Adding tetrakis(trifluorophosphine)nickel into the reaction kettle to react with the ammonia water to form a suspension;

[0016] The pH value of the suspension is detected, and when the pH value reaches a first preset value, nitrogen is introduced for a first preset time and heating is performed, and when the pH value reaches a second preset value, heating is stopped to obtain a first nickel solid and a reaction liquid.

[0017] Optionally, the reaction solution is added with hydrazine hydrate for reduction treatment to obtain a second nickel solid, comprising:

[0018] Adding ultrapure water to dilute the reaction solution to obtain a diluted solution;

[0019] The diluent is added to hydrazine hydrate, and after being fully mixed, a heating treatment is performed at a second preset temperature and for a second preset time to obtain a second nickel solid.

[0020] Optionally, adding ammonia water to the first nickel solid and the second nickel solid, and performing ammonia washing treatment under nitrogen protection to obtain a third nickel solid and ammonia washing solution, comprising:

[0021] placing the first nickel solid and the second nickel solid in the reactor, adding ammonia water, and introducing nitrogen gas into the reactor for a third preset time;

[0022] The internal temperature of the reactor is adjusted to a third preset temperature and maintained for a fourth preset time to obtain a third nickel solid and an ammonia washing solution.

[0023] Optionally, the ammonia wash solution is added with hydrazine hydrate for reduction treatment to obtain a fourth nickel solid, comprising:

[0024] The ammonia wash solution is added to hydrazine hydrate, and after being fully mixed, a heating treatment is performed at a second preset temperature and for a second preset time to obtain a fourth nickel solid.

[0025] Optionally, the third nickel solid and the fourth nickel solid are added with ultrapure water for washing, and then dried to obtain a nickel single substance, comprising:

[0026] The third nickel solid and the fourth nickel solid are placed in the reactor, and ultrapure water is added for stirring;

[0027] The inner temperature of the reactor is heated to a fourth preset temperature and maintained for a fifth preset time, and then cooled to room temperature to obtain nickel solid;

[0028] The nickel solid is dried at a fifth preset temperature to obtain nickel element.

[0029] Optionally, the mass fraction of the hydrazine hydrate is 80%.

[0030] Optionally, 80% hydrazine hydrate is added to the diluent at a ratio of 3 to 4 times the amount of tetrakis(trifluorophosphine)nickel added.

[0031] Optionally, the ammonia wash solution is added with 80% hydrazine hydrate at a ratio of 1.0 to 1.1 times the amount of tetrakis(trifluorophosphine)nickel added.

[0032] Optionally, pouring the ammonia water into a reactor, adjusting the internal temperature of the reactor to a first preset temperature, and introducing nitrogen for a first preset time period, comprises:

[0033] The ammonia water was poured into the reaction kettle, the internal temperature of the reaction kettle was adjusted to -25°C to -15°C, and nitrogen was introduced for 3 to 5 minutes.

[0034] Optionally, the pH value of the suspension is detected, and when the pH value reaches a first preset value, nitrogen is introduced for a first preset time and heated, and when the pH value reaches a second preset value, the heating is stopped to obtain a first nickel solid and a reaction liquid, comprising:

[0035] The pH value of the suspension is detected. When the pH value reaches 10.5 to 11.0, nitrogen is introduced for 3 to 5 minutes and heating is performed. When the pH value reaches 6.5 to 7.0, heating is stopped to obtain a first nickel solid and a reaction solution.

[0036] Optionally, adding hydrazine hydrate to the diluent, fully mixing, and then heating for a second preset time at a second preset temperature to obtain a second nickel solid, comprising:

[0037] The diluted solution is added with hydrazine hydrate, and after being fully mixed, a heating treatment is performed at 140° C. to 160° C. for 1.5 h to 2.5 h to obtain a second nickel solid.

[0038] Optionally, placing the first nickel solid and the second nickel solid in the reactor, adding ammonia water, and introducing nitrogen gas for a third preset time into the reactor comprises:

[0039] The first nickel solid and the second nickel solid are placed in the reactor, ammonia water is added, and nitrogen is introduced into the reactor for 1 to 2 minutes.

[0040] Optionally, adjusting the internal temperature of the reactor to a third preset temperature and maintaining it for a fourth preset time to obtain a third nickel solid and an ammonia wash solution comprises:

[0041] The internal temperature of the reactor is adjusted to 80° C. to 90° C. and maintained for 1 h to 1.5 h to obtain a third nickel solid and an ammonia washing solution.

[0042] Optionally, adding the ammonia wash to hydrazine hydrate, fully mixing, and then heating for a second preset time at a second preset temperature to obtain a fourth nickel solid, comprising:

[0043] The ammonia wash solution is added to hydrazine hydrate, and after being fully mixed, a heating treatment is performed at 140° C. to 160° C. for 1.5 h to 2.5 h to obtain a fourth nickel solid.

[0044] Optionally, heating the inner temperature of the reactor to a fourth preset temperature and maintaining it for a fifth preset time, and cooling it to room temperature to obtain nickel solid, comprising:

[0045] The inner temperature of the reactor is heated to 90° C. to 100° C. and maintained for 1 to 1.5 hours, and then cooled to room temperature to obtain nickel solid.

[0046] Optionally, drying the nickel solid at a fifth preset temperature to obtain a nickel single substance comprises:

[0047] The nickel solid is dried at 150° C. to 200° C. to obtain nickel element.

[0048] Optionally, placing the third nickel solid and the fourth nickel solid in the reactor, adding ultrapure water and stirring, comprises:

[0049] The third nickel solid and the fourth nickel solid are placed in the reactor, and ultrapure water is added to perform water washing treatment at least three times.

[0050] The beneficial effects of the above technical solution of the present invention are:

[0051] The above embodiment of the present invention provides ammonia water; adds tetrakis(trifluorophosphine) nickel to the ammonia water, and undergoes a hydrolysis neutralization reaction and a heating process under nitrogen protection to obtain a first nickel solid and a reaction liquid; adds hydrazine hydrate to the reaction liquid for reduction treatment to obtain a second nickel solid; adds the first nickel solid and the second nickel solid to ammonia water, and performs ammonia washing treatment under nitrogen protection to obtain a third nickel solid and ammonia washing liquid; adds hydrazine hydrate to the ammonia washing liquid for reduction treatment to obtain a fourth nickel solid; adds ultrapure water to the third nickel solid and the fourth nickel solid for washing treatment, and obtains nickel element after drying. The method for preparing a nickel element by nitrogen protection synthesis reaction and simultaneous reduction of nickel ions provided by the present invention has a high yield of qualified products, and the product purity can meet the use requirements of nickel batteries. BRIEF DESCRIPTION OF THE DRAWINGS

[0052] Figure 1 1 is a schematic flow chart of a method for preparing a single substance of nickel according to an embodiment of the present invention;

[0053] Figure 2 1 is a process flow chart of a method for preparing a single substance of nickel according to an embodiment of the present invention;

[0054] Figure 3 Schematic diagram of a nitrogen-protected hydrolysis neutralization device according to an embodiment of the present invention;

[0055] Figure 4 is a schematic diagram of a nitrogen protection heating device according to an embodiment of the present invention;

[0056] Figure 5 is a schematic diagram of an ammonia washing device according to an embodiment of the present invention;

[0057] Figure 6 is a schematic diagram of a water washing device according to an embodiment of the present invention;

[0058] Figure 7 Schematic diagram of X-ray diffraction test results of the nickel single substance product of Example 1 of the present invention;

[0059] Figure 8 It is a schematic diagram of the X-ray diffraction test results of the nickel single substance product of Example 2 of the present invention. DETAILED DESCRIPTION

[0060] Embodiments of the present invention are described in detail below. Examples of the embodiments are shown in the accompanying drawings. The embodiments described below with reference to the accompanying drawings are exemplary and are intended to be used to explain the present invention, but should not be construed as limiting the present invention.

[0061] like Figure 1 and Figure 2 As shown, the present invention provides a method for preparing a single substance of nickel, comprising:

[0062] Step 11, providing aqueous ammonia;

[0063] Step 12, adding tetrakis(trifluorophosphine)nickel into aqueous ammonia, and subjecting the mixture to a hydrolysis and neutralization reaction and a heating process under nitrogen protection to obtain a first nickel solid and a reaction liquid;

[0064] Step 13, adding hydrazine hydrate to the reaction solution for reduction treatment to obtain a second nickel solid;

[0065] Step 14, adding ammonia water to the first nickel solid and the second nickel solid, and performing ammonia washing treatment under nitrogen protection to obtain a third nickel solid and ammonia washing solution;

[0066] Step 15, adding hydrazine hydrate to the ammonia wash solution for reduction treatment to obtain a fourth nickel solid;

[0067] Step 16, adding ultrapure water to the third nickel solid and the fourth nickel solid for washing, and drying to obtain nickel element.

[0068] The method for preparing nickel element provided by this embodiment of the present invention, which uses nickel tetrakis (trifluorophosphine) and ammonia water as raw materials, adopts nitrogen protection reaction, and simultaneously reduces nickel ions, aims to improve the reaction yield on the basis of ensuring the purity of nickel element, and prepares a qualified product with high yield. The method eliminates the conditions for the oxidation of nickel element to nickel ions by adding nitrogen protection in the hydrolysis neutralization process, the heating process, and the ammonia washing process, and effectively reduces the loss of nickel products. At the same time, nickel ions, hexaammine nickel and tetraammine nickel complex ions will exist in the heated reaction solution and the ammonia washing solution. If these ions are not recovered, the reaction yield will be seriously affected; especially in the process of preparing nickel-62 element, the reduction in yield will cause economic losses. The invention utilizes the oxidizing property of nickel ions and reduces them through reducing substances. Meanwhile, considering the purity requirement of the product, a strong reducing agent hydrazine hydrate without introducing impurity elements is used for reduction. In the process of preparing nickel element through liquid phase reaction, the invention adopts a method of nitrogen protection hydrolysis neutralization, heating and ammonia washing process, and a method of reducing nickel ions in reaction liquid and ammonia washing liquid, so that the loss of nickel element can be effectively reduced on the basis of ensuring the purity of the product, so that the reaction yield reaches more than 97%, thereby improving the reaction yield.

[0069] In some embodiments of the present invention, step 12 includes:

[0070] Step 121, pouring ammonia water into the reactor, adjusting the internal temperature of the reactor to a first preset temperature and introducing nitrogen for a first preset time;

[0071] Step 122, adding tetrakis(trifluorophosphine)nickel into a reaction kettle to react with aqueous ammonia to form a suspension;

[0072] Step 123, detecting the pH value of the suspension, introducing nitrogen for a first preset time and heating when the pH value reaches a first preset value, and stopping heating when the pH value reaches a second preset value to obtain a first nickel solid and a reaction liquid.

[0073] In this embodiment, the reaction process of preparing nickel element by reacting tetrakis(trifluorophosphine)nickel with ammonia water includes hydrolysis of tetrakis(trifluorophosphine)nickel and neutralization of the acidic hydrolysis product with alkali. The specific reaction process is as follows:

[0074] Ni(PF3)4+12H2O⇋Ni+4H3PO3+12HF

[0075] H3PO3+3NH3.H2O = (NH4)3PO3+3H2O

[0076] HF+NH3.H2O = NH4F+H2O

[0077] There are many side reactions in this process. The most important side reaction is the oxidation of nickel. Nickel is an electropositive metal, and the electrode potential of its oxidation reaction is -0.250V. Ni→Ni 2+ (aq)+2e- (E θ =-0.250V). Nickel can be corroded by ammonia water, because ammonia can form stable complex ions with nickel ions, which reduces the standard electrode potential between nickel ions and nickel element, making nickel more easily oxidized. Therefore, in the presence of ammonia water, nickel is easily oxidized by oxygen in the air to form nickel ions. The generation of nickel ions will cause nickel element loss and affect the yield. At the same time, nickel ions will combine with phosphite and hydroxide in the solution to form insoluble solid nickel phosphite and nickel hydroxide, which will be mixed in the nickel element and affect the purity of the product. Therefore, it is necessary to avoid the oxidation reaction of nickel element as much as possible during the reaction. Ammonia water participates in the neutralization reaction as a neutralizer and cannot be removed. The introduction of the oxidant-oxygen can only be avoided as much as possible in the reaction system. The present invention adopts a nitrogen protection method to isolate the reaction system from the oxygen environment.

[0078] The small metal nickel particles generated after the neutralization reaction are mixed in the reaction solution to form a suspension system. The heating process can promote the aggregation of small metal nickel particles to form larger metal particles that precipitate from the solution; it is also beneficial to promote the complete hydrolysis of tetrakis(trifluorophosphine)nickel and improve the conversion rate of nickel. The ammonia dissolved in the reaction solution and the ammonia complexed with nickel ions will be released during the heating process, causing the pH value of the reaction system to continue to decrease. However, in the initial stage of heating, the alkalinity of the solution is still very strong, and there is a large amount of ammonia in the system, so nitrogen protection is also required during the heating process. The specific operation process is as follows:

[0079] like Figure 3As shown, a certain amount of ammonia water is weighed in a 1L polytetrafluoroethylene reactor, and the reactor is placed in a low-temperature tank and cooled to -30~-20°C. The internal temperature is controlled at -25~-15°C. After reaching the temperature, nitrogen is introduced for 3~5 minutes, and then the nitrogen outlet valve is closed. A certain amount of tetrakis(trifluorophosphine)nickel is slowly added while stirring. After the raw materials are added, the reaction is continued for a period of time, and the pH value of the reaction system is detected. The reaction is stopped when the pH value reaches 10.5~11.0.

[0080] like Figure 4 As shown, nitrogen was introduced into the reaction system for 3-5 minutes, and then the nitrogen outlet valve was closed. The reaction system was heated and the pH value change was detected. When the pH value reached 6.5-7.0, the heating was stopped.

[0081] In some embodiments of the present invention, step 13 includes:

[0082] Step 131, adding ultrapure water to dilute the reaction solution to obtain a diluted solution;

[0083] Step 132, adding hydrazine hydrate to the diluent, fully mixing, and then performing a heating treatment at a second preset temperature and for a second preset time to obtain a second nickel solid.

[0084] In this embodiment, after cooling from the heating process, nickel solids are deposited at the bottom of the reactor, and the nickel solids are filtered out. The upper solution contains oxidized nickel ions, and it is calculated that such nickel ions account for 10-20% of the total input of nickel element. If such nickel ions are not reduced, a large amount of nickel element will be lost, reducing the yield. Nickel ions are oxidizing and can be reduced by a reducing agent. Hydrazine hydrate is used as a reducing agent to recover nickel from the reaction solution by chemical reduction under liquid phase conditions. The reaction principle is as follows:

[0085]

[0086] The advantage of hydrazine hydrate reduction is that no other impurity elements are introduced during the reduction process, which will not affect the purity of the product. The specific operation process is as follows:

[0087] Add a certain amount of ultrapure water to the reaction solution for dilution, then add 80% hydrazine hydrate at a ratio of 3 to 4 times the amount of tetrakis(trifluorophosphine)nickel added, stir for 3 to 5 minutes, pour into a hydrothermal synthesis reactor with a polytetrafluoroethylene liner, put into a blast drying oven, and heat at 140 to 160°C for 1.5 to 2.5 hours. After cooling, take out the recovered second nickel solid and mix it with the first nickel solid obtained during the heating process.

[0088] In some embodiments of the present invention, step 14 includes:

[0089] Step 141, placing the first nickel solid and the second nickel solid in a reactor, adding ammonia water and introducing nitrogen gas into the reactor for a third preset time;

[0090] Step 142, adjusting the internal temperature of the reactor to a third preset temperature and maintaining it for a fourth preset time to obtain a third nickel solid and an ammonia washing solution.

[0091] In this embodiment, ammonia washing is to remove impurities such as nickel phosphate, nickel carbonate, nickel hydroxide, etc. mixed in the nickel solid to ensure the purity of the product. The principle is that nickel ions are very easy to complex with ammonia water, so in the presence of ammonia water, the ionization equilibrium of the sparingly soluble nickel salt can be promoted to move forward, and finally a nickel ion complex is formed and dissolved. For example:

[0092] Ni(OH)2⇋Ni 2+ +2OH -

[0093] Ni(OH)2+4NH3.H2O⇋[Ni(NH3)4] 2+ +2OH - +4H2O

[0094] or:

[0095] Ni(OH)2+6NH3.H2O⇋[Ni(NH3)6] 2+ +2OH - +6H2O

[0096] In order to reduce the oxidation of nickel during the ammonia washing process, nitrogen protection is used in this process. The specific operation process is as follows:

[0097] like Figure 5 As shown, the first nickel solid and the second nickel solid are added to the reactor, and 120-150 ml of ammonia water is added. First, nitrogen is introduced for 1-2 minutes to fill the reactor with nitrogen. Stirring is started, the internal temperature is controlled at 80-90°C and heated for 1-1.5 hours, heating and stirring are stopped, and cooling is performed to room temperature. The ammonia washing process is repeated twice to obtain the third nickel solid and ammonia washing solution.

[0098] In some embodiments of the present invention, step 15 includes:

[0099] The ammonia washing solution is added to hydrazine hydrate, and after being fully mixed, a heating treatment is performed at a second preset temperature and for a second preset time to obtain a fourth nickel solid.

[0100] In this embodiment, since the ammonia wash solution contains a certain amount of nickel ion complex, the nickel ion is 5-10% of the added amount, these nickel elements need to be recovered to ensure the yield. To ensure the purity of the product, the ammonia wash solution is still reduced with hydrazine hydrate, and the principle is as follows:

[0101] 2[Ni(NH3)4] 2+ + N2H4+4OH - →2Ni↓ +N2↑+4H2O+8NH3↑

[0102] or:

[0103] 2[Ni(NH3)6] 2+ + N2H4+4OH - →2Ni↓ +N2↑+4H2O+12NH3↑

[0104] The specific operation process is: after weighing the two ammonia washing solutions, pour them into the hydrothermal synthesis reactor, add 80% hydrazine hydrate at a ratio of 1.0~1.1 times the amount of tetrakis(trifluorophosphine)nickel, and place it in a drying oven and heat it at 140~160℃ for 1.5~2.5h to obtain the fourth nickel solid.

[0105] In some embodiments of the present invention, step 16 includes:

[0106] Step 161, placing the third nickel solid and the fourth nickel solid in a reaction kettle, adding ultrapure water and stirring;

[0107] Step 162, heating the inner temperature of the reactor to a fourth preset temperature and maintaining it for a fifth preset time, and cooling it to room temperature to obtain nickel solid;

[0108] Step 163, drying the nickel solid at a fifth preset temperature to obtain nickel element.

[0109] In this embodiment, if Figure 6 As shown, the soluble salts attached to the solid surface are removed by water washing. The purpose of drying is to remove free water in the product and reduce the water content of the metal nickel product; in addition, drying can also remove some low-boiling point substances attached to the surface of the nickel solid. The specific operation process is: the fourth nickel solid obtained by reducing the ammonia wash solution is mixed with the third nickel solid and added to the reactor, 200~300ml of ultrapure water is added, stirring is turned on, the internal temperature is controlled at 90~100℃ for a period of time, and then cooled to room temperature, the water wash solution is poured out, and the water washing operation is repeated 3~4 times. After washing, the water-containing nickel single substance solid is placed in a polytetrafluoroethylene tray, placed in a drying oven at 150~200℃ for drying to obtain nickel single substance.

[0110] Example 1

[0111] Weigh 204.25 g of ammonia water in a reactor, cool the reactor to -20°C, control the internal temperature at -15°C, introduce nitrogen for 3 min, and then slowly add 33.32 g of nickel tetrakis(trifluorophosphine) under stirring conditions. Add the materials for a total of 3 h. After the raw materials are added, continue for 1 h. Stop the reaction when the pH reaches 10.80.

[0112] Rinse the sticky materials on the pipeline and kettle cover with ultrapure water into the reactor, place the reactor in an electric heating jacket, pass nitrogen for 4 minutes, close the nitrogen outlet valve, control the external temperature at 120℃ and heat, and stop heating when the pH value reaches 6.50.

[0113] After cooling, the solid and liquid are separated, and the nickel solid sinks to the bottom of the kettle. The nickel solid is filtered out, and about 700 ml of the solution is diluted with 200 ml of ultrapure water, and 103.14 g of hydrazine hydrate is added and stirred for 5 minutes. The solution is poured into three 500 ml hydrothermal kettles, placed in a drying oven, and heated at 150 ° C for 2 hours. After cooling, the recovered nickel solid is taken out and mixed with the nickel solid obtained in the heating process.

[0114] Add nickel solid to the reactor and add 150 ml of ammonia water. Pass nitrogen for 2 minutes to fill the reactor with nitrogen. Turn on stirring and control the internal temperature at 80-90℃ for 1.5 hours. Stop heating and stirring and cool to room temperature. Repeat the ammonia washing process twice.

[0115] Combine the two ammonia washes and add them into a hydrothermal reactor. Add 35.28 g of hydrazine hydrate, stir for 3 minutes, then put it into a drying oven and heat at 150°C for 2 hours.

[0116] The nickel element obtained by reducing the ammonia washing solution was mixed with the original solid and added to the reactor, 300 ml of ultrapure water was added, stirring was started, the internal temperature was controlled at 90-100°C for heating for 1 hour, and then cooled to room temperature, the washing liquid was poured out, and the washing operation was repeated 4 times. The water-containing nickel element was placed in a drying oven at 200°C for 3 hours to obtain 4.668 g of nickel element solid, with a yield of 97.3%.

[0117] Example 2

[0118] Weigh 204.06 g of ammonia water in a reactor, cool the reactor to -30°C, control the internal temperature at -25°C, introduce nitrogen for 3 minutes, and then slowly add 33.10 g of nickel tetrakis(trifluorophosphine) under stirring conditions. The addition time is 3 hours in total. After the addition of the raw materials is completed, continue for 1 hour. Stop the reaction when the pH value reaches 10.84.

[0119] Rinse the sticky materials on the pipeline and kettle cover with ultrapure water into the reactor, place the reactor in an electric heating jacket, pass nitrogen for 5 minutes, close the nitrogen outlet valve, control the external temperature at 120℃ and heat, and stop heating when the pH value reaches 6.75.

[0120] After cooling, the solid and liquid are separated, and the nickel solid sinks to the bottom of the kettle. The nickel solid is filtered out, and about 800 ml of the solution is diluted with 200 ml of ultrapure water, and 132.73 g of hydrazine hydrate is added and stirred for 5 min. The solution is poured into three 500 ml hydrothermal synthesis reactors, placed in a drying oven, and heated at 150 ° C for 2 h. After cooling, the recovered nickel solid is taken out and mixed with the nickel solid obtained in the heating process.

[0121] Add nickel solid to the reactor and add 150ml of ammonia water. Pass nitrogen for 2 minutes to fill the reactor with nitrogen. Turn on stirring and control the internal temperature at 80~90℃ for 1 hour. Stop heating and stirring and cool to room temperature. Repeat the ammonia washing process twice.

[0122] Combine the two ammonia washes and add them into a hydrothermal kettle. Add 35.30 g of hydrazine hydrate, stir for 3 minutes, then put into a drying oven and heat at 150°C for 2 hours.

[0123] The nickel element obtained by reducing the ammonia washing solution was mixed with the original solid and added to the reactor, 250 ml of ultrapure water was added, stirring was started, the internal temperature was controlled at 90-100 ° C for 1 hour, and then cooled to room temperature, the washing liquid was poured out, and the washing operation was repeated 4 times. The water-containing nickel element was placed in a drying oven at 200 ° C for 3 hours to obtain 4.726 g of nickel element, with a yield of 99.2%.

[0124] X-ray diffraction (XRD) was performed on the samples in the above two embodiments. Figure 7 and Figure 8 As shown, the diffraction line of the spectrum measured by nickel single substance is strong, and the spectra of the two samples are both at 2θ=44.5 o , 51.8 o and 76.4 o There are cross-sectional peaks, and the diffraction peaks are sharp, symmetrical, and free of impurity peaks, proving that the sample is pure phase and free of impurity crystals, with a crystallinity of ≥99% and a cubic phase structure.

[0125] According to the national standard, the nickel samples in the two embodiments were tested for 16 impurity elements, of which carbon and sulfur were tested by high-frequency induction furnace combustion infrared absorption method, and the remaining 14 elements were tested by inductively coupled plasma optical emission spectrometer (ICP-OES). The content of the nickel sample was obtained by subtracting the content of the 16 impurity elements from 100%, and the test results are shown in Tables 1 and 2.

[0126] Table 1 Detection results of nickel elemental product content in Example 1

[0127] project Test results / % Cobalt (Co) 0.012 Copper (Cu) <0.01 Silicon (Si) 0.012 Manganese (Mn) <0.01 Magnesium (Mg) <0.01 Phosphorus (P) 0.48 Iron (Fe) 0.012 Lead (Pb) <0.02 Bismuth (Bi) <0.02 Arsenic (As) <0.02 Antimony (Sb) <0.02 Zinc (Zn) <0.01 Cadmium (Cd) <0.01 Tin (Sn) <0.02 Carbon (C) 0.14 Sulfur (S) 0.0022 total <0.8082 Nickel (Ni) >99.1918

[0128] Table 2 Detection results of nickel elemental product content in Example 2

[0129] project Test results / % Cobalt (Co) 0.012 Copper (Cu) <0.01 Silicon (Si) <0.01 Manganese (Mn) <0.01 Magnesium (Mg) <0.01 Phosphorus (P) 0.63 Iron (Fe) <0.01 Lead (Pb) <0.02 Bismuth (Bi) <0.02 Arsenic (As) <0.02 Antimony (Sb) <0.02 Zinc (Zn) <0.01 Cadmium (Cd) <0.01 Tin (Sn) <0.02 Carbon (C) 0.16 Sulfur (S) 0.0034 total <0.9754 Nickel (Ni) >99.0246

[0130] The samples in the above two embodiments were tested by high-frequency induction furnace combustion infrared absorption method and inductively coupled plasma emission spectrometer. The sum of 16 impurity elements was <1%, and the nickel metal content was >99%, which can meet the requirements for nickel battery use.

[0131] In the description of this specification, the description with reference to the terms "one embodiment", "some embodiments", "example", "specific implementation", or "some implementations" means that the specific features, structures, materials or characteristics described in conjunction with the embodiment or example are included in at least one embodiment or example of the present invention. In this specification, the schematic expressions of the above terms do not necessarily refer to the same embodiment or example.

[0132] Although the embodiments of the present invention have been shown and described above, it is to be understood that the above embodiments are exemplary and are not to be construed as limitations of the present invention. A person skilled in the art may change, modify, replace and vary the above embodiments within the scope of the present invention.

Claims

1. A method for preparing a nickel element, characterized in that: include: Provide ammonia; Adding tetrakis(trifluorophosphine)nickel into the ammonia water, and subjecting the mixture to a hydrolysis and neutralization reaction and a heating process under nitrogen protection to obtain a first nickel solid and a reaction liquid; Adding hydrazine hydrate to the reaction solution for reduction treatment to obtain a second nickel solid; Adding ammonia water to the first nickel solid and the second nickel solid, and performing ammonia washing treatment under nitrogen protection to obtain a third nickel solid and ammonia washing solution; Adding hydrazine hydrate to the ammonia wash solution for reduction treatment to obtain a fourth nickel solid; The third nickel solid and the fourth nickel solid are added with ultrapure water for washing, and then dried to obtain nickel element.

2. The method for preparing nickel simple substance according to claim 1, characterized in that: Tetrakis(trifluorophosphine)nickel is added to the ammonia water, and subjected to a hydrolysis neutralization reaction and a heating process under nitrogen protection to obtain a first nickel solid and a reaction liquid, including: Pour the ammonia water into a reaction kettle, adjust the internal temperature of the reaction kettle to a first preset temperature, and introduce nitrogen for a first preset time; Adding tetrakis(trifluorophosphine)nickel into the reaction kettle to react with the ammonia water to form a suspension; The pH value of the suspension is detected, and when the pH value reaches a first preset value, nitrogen is introduced for a first preset time and heating is performed, and when the pH value reaches a second preset value, heating is stopped to obtain a first nickel solid and a reaction liquid.

3. The method for preparing nickel simple substance according to claim 2, characterized in that: The reaction solution is added with hydrazine hydrate for reduction treatment to obtain a second nickel solid, comprising: Adding ultrapure water to dilute the reaction solution to obtain a diluted solution; The diluent is added to hydrazine hydrate, and after being fully mixed, a heating treatment is performed at a second preset temperature and for a second preset time to obtain a second nickel solid.

4. The method for preparing a nickel single substance according to claim 3, characterized in that: The first nickel solid and the second nickel solid are added with ammonia water, and washed with ammonia under nitrogen protection to obtain a third nickel solid and an ammonia washing solution, comprising: placing the first nickel solid and the second nickel solid in the reactor, adding ammonia water, and introducing nitrogen gas into the reactor for a third preset time; The internal temperature of the reactor is adjusted to a third preset temperature and maintained for a fourth preset time to obtain a third nickel solid and an ammonia washing solution.

5. The method for preparing nickel element according to claim 4, characterized in that: The ammonia wash solution is added with hydrazine hydrate for reduction treatment to obtain a fourth nickel solid, comprising: The ammonia wash solution is added to hydrazine hydrate, and after being fully mixed, a heating treatment is performed at a second preset temperature and for a second preset time to obtain a fourth nickel solid.

6. The method for preparing nickel element according to claim 5, characterized in that: The third nickel solid and the fourth nickel solid are added with ultrapure water for washing, and then dried to obtain a nickel single substance, including: The third nickel solid and the fourth nickel solid are placed in the reactor, and ultrapure water is added for stirring; The inner temperature of the reactor is heated to a fourth preset temperature and maintained for a fifth preset time, and then cooled to room temperature to obtain nickel solid; The nickel solid is dried at a fifth preset temperature to obtain nickel element.

7. The method for preparing a nickel single substance according to any one of claims 1 to 6, characterized in that: The mass fraction of the hydrazine hydrate is 80%.

8. The method for preparing nickel simple substance according to claim 3, characterized in that: The diluent is added with 80% hydrazine hydrate at a ratio of 3 to 4 times the amount of tetrakis(trifluorophosphine)nickel added.

9. The method for preparing a simple nickel substance according to claim 5, characterized in that: The ammonia wash solution is added with 80% hydrazine hydrate at a ratio of 1.0 to 1.1 times the amount of tetrakis(trifluorophosphine)nickel added.

10. The method for preparing nickel element according to claim 2, characterized in that: The ammonia solution is poured into a reaction kettle, the internal temperature of the reaction kettle is adjusted to a first preset temperature, and nitrogen is introduced for a first preset time, comprising: The ammonia water was poured into the reaction kettle, the internal temperature of the reaction kettle was adjusted to -25°C to -15°C, and nitrogen was introduced for 3 to 5 minutes.

11. The method for preparing nickel element according to claim 2, characterized in that: The pH value of the suspension is detected, when the pH value reaches a first preset value, nitrogen is introduced for a first preset time and heating is performed, and when the pH value reaches a second preset value, heating is stopped to obtain a first nickel solid and a reaction liquid, comprising: The pH value of the suspension is detected. When the pH value reaches 10.5 to 11.0, nitrogen is introduced for 3 to 5 minutes and heating is performed. When the pH value reaches 6.5 to 7.0, heating is stopped to obtain a first nickel solid and a reaction solution.

12. The method for preparing nickel element according to claim 3, characterized in that: The diluent is added to hydrazine hydrate, and after being fully mixed, a heating treatment is performed at a second preset temperature and for a second preset time to obtain a second nickel solid, comprising: The diluted solution is added with hydrazine hydrate, and after being fully mixed, a heating treatment is performed at 140° C. to 160° C. for 1.5 h to 2.5 h to obtain a second nickel solid.

13. The method for preparing nickel element according to claim 4, characterized in that: Placing the first nickel solid and the second nickel solid in the reactor, adding ammonia water, and introducing nitrogen gas into the reactor for a third preset time, comprising: The first nickel solid and the second nickel solid are placed in the reactor, ammonia water is added, and nitrogen is introduced into the reactor for 1 to 2 minutes.

14. The method for preparing nickel element according to claim 4, characterized in that: Adjusting the inner temperature of the reactor to a third preset temperature and maintaining it for a fourth preset time to obtain a third nickel solid and an ammonia wash solution, comprising: The internal temperature of the reactor is adjusted to 80° C. to 90° C. and maintained for 1 h to 1.5 h to obtain a third nickel solid and an ammonia washing solution.

15. The method for preparing nickel element according to claim 5, characterized in that: The ammonia wash solution is added to hydrazine hydrate, and after being fully mixed, a heating treatment is performed at a second preset temperature and for a second preset time to obtain a fourth nickel solid, comprising: The ammonia wash solution is added to hydrazine hydrate, and after being fully mixed, a heating treatment is performed at 140° C. to 160° C. for 1.5 h to 2.5 h to obtain a fourth nickel solid.

16. The method for preparing nickel element according to claim 6, characterized in that: The inner temperature of the reactor is heated to a fourth preset temperature and maintained for a fifth preset time, and then cooled to room temperature to obtain nickel solid, comprising: The inner temperature of the reactor is heated to 90° C. to 100° C. and maintained for 1 to 1.5 hours, and then cooled to room temperature to obtain nickel solid.

17. The method for preparing nickel element according to claim 6, characterized in that: The nickel solid is dried at a fifth preset temperature to obtain a nickel single substance, comprising: The nickel solid is dried at 150° C. to 200° C. to obtain nickel element.

18. The method for preparing nickel element according to claim 6, characterized in that: The third nickel solid and the fourth nickel solid are placed in the reactor, and ultrapure water is added for stirring, comprising: The third nickel solid and the fourth nickel solid are placed in the reactor, and ultrapure water is added to perform water washing treatment at least three times.

Citation Information

Patent Citations

  • Method for recycling nickel in chemical nickel plating wastewater through multiple times of precipitation

    CN111153476A

  • Nickel recovery method

    CN113215415A

  • Hydrolysis sampling method and device of nickel tetratrifluorophosphine

    CN116223089A

  • Hydrothermal reduction preparation method of nickel isotope elementary substance and nickel isotope elementary substance prepared by hydrothermal reduction preparation method

    CN117987660A

  • Method of producing tetrakis-(trifluorophosphine) of isotope-enriched nickel

    RU2707035C1