Rock wool decorative plate production process and rock wool decorative plate

Through the automated rock wool decorative board production process and the use of mechanical integration equipment to simplify the production process, it solves the problems of complex operations and low efficiency in the existing technology, realizes the production of high-efficiency, low-strength rock wool boards, and produces waterproof and fire-proof products. and aesthetic properties.

CN118769626APending Publication Date: 2024-10-15NANJING HENGXIANG INSULATION MATERIALS MFG CO LTD
View PDF 14 Cites 0 Cited by

Patent Information

Application Number
CN202410754058.9
Authority / Receiving Office
CN · China
Patent Type
Applications(China)
Current Assignee / Owner
Filing Date
2024-06-12
Publication Date
2024-10-15

AI Technical Summary

Technical Problem

The existing production process of rock wool decorative panels is complex and requires the participation of multiple operators, resulting in high labor intensity and low efficiency.

Method used

Adopt automated processes, including rock wool pretreatment, dispersion, sorting, metering, sizing, pre-pressing, molding, defective product rejection and deep processing, and use mechanically integrated equipment such as crushers, cyclones, continuous presses and Grinding device reduces manual operations and improves automation.

Benefits of technology

It significantly reduces the labor intensity of operators, improves work efficiency, and produces rock wool decorative boards that are waterproof, fireproof, durable and beautiful.

✦ Generated by Eureka AI based on patent content.

Smart Images

  • Figure CN118769626A_ABST
    Figure CN118769626A_ABST
Patent Text Reader

Abstract

The invention discloses a rock wool decorative plate production process and a rock wool decorative plate, and the process comprises the following steps: conveying rock wool into a crusher to crush into fibers with a set length, spraying water containing a water repellent, a dispersing agent and a coupling agent, and mixing; conveying the mixed material to a fiber beater, and scattering fibers in the mixed material; impurities and caked materials are screened out, and mixed materials with scattered fibers are conveyed to the next step; the materials are metered and subjected to secondary scattering; spraying powdery glue into the mixed material, stirring, and scattering the mixed material after glue spraying; the mixed material obtained after glue spraying is evenly laid into a plate blank, and the plate blank is weighed; the plate blank is pre-pressed by a pre-pressing machine, and meanwhile steam is applied for heating; the plate blank with the metal impurities removed is conveyed to a continuous press to be subjected to thermocuring forming; and trimming the plate without the defective products, polishing the surface, and storing. The device is high in automation degree, the labor intensity of operators is reduced, and the working efficiency is improved.
Need to check novelty before this filing date? Find Prior Art

Description

Technical Field

[0001] The invention relates to the technical field of plate processing, and in particular to a production process of a rock wool decorative plate and a rock wool decorative plate. Background Art

[0002] Rock wool insulation decorative board, also known as rock wool board, is a commonly used insulation material and is widely used in building materials engineering. Rock wool is a green product derived from natural minerals, non-toxic and harmless, with good fire resistance, good durability, and the ability to synchronize with the life of the building. It has the advantages of low thermal conductivity, good air permeability, and high combustion performance level. Existing rock wool decorative boards often require multiple operators to perform numerous processing steps before they can be produced and processed, which greatly increases the difficulty of processing and production and the labor intensity of operators. Summary of the invention

[0003] The purpose of the present invention is to provide a rock wool decorative board production process and a rock wool decorative board to solve the problems existing in the above-mentioned prior art, with a high degree of automation, reducing the labor intensity of operators and improving work efficiency.

[0004] To achieve the above object, the present invention provides the following solutions:

[0005] The present invention provides a production process of a rock wool decorative board, comprising the following steps:

[0006] Step 1: rock wool pretreatment: the rock wool is transported to a crusher and crushed into fibers of a set length, sprayed with water containing a hydrophobic agent, a dispersant and a coupling agent, and mixed;

[0007] Step 2: breaking up the mixed materials, conveying them to a fiber breaking machine to break up the fibers in the mixed materials;

[0008] Step 3: sorting, screening out impurities and agglomerated materials in step 2. The impurities are mainly slag balls. The mixed materials after fiber is dispersed are transported to the second cyclone and then enter the next step;

[0009] Step 4: The material is weighed and broken up for the second time. The material enters the breaking up roller through the bottom of the second cyclone. After the second breaking up, it enters the metering bin for weighing. The weighed material is broken up again and then enters the glue cylinder.

[0010] Step 5: 4 to 10 (preferably 4 to 6) nozzles are provided in the glue barrel, and the powdered glue is sprayed onto the surface of the material with compressed air, and the powdered glue is sprayed into the mixed material, stirred, and then the mixed material after the spraying is dispersed;

[0011] Step 6, breaking up the sprayed mixed material and evenly paving it into a slab, and weighing it;

[0012] Step 7, pre-pressing the slab, the pre-pressing machine of the pre-pressing steam heating system pre-presses the slab, and applies steam heating at the same time, the steam penetrates from the bottom surface to the core layer, and then penetrates to the surface, increases the temperature of the core layer, facilitates the curing of the core layer, and reduces the curing time; increases the temperature of the core layer, and facilitates the subsequent heating and curing;

[0013] Step eight, sheet forming, the slab after removing metal impurities is transported to a continuous press, 225-280 degrees (preferably 235-270 degrees), the upper and lower steel belts extrude the slab for thermal curing forming;

[0014] Step nine, reject defective products. After rejecting defective products, the boards are trimmed. When the core layer curing quality is poor, the boards are prone to bubbling. Therefore, it is necessary to detect whether the boards have bubbles. If so, they are set as defective products and rejected. Genuine boards without bubbles are transported to the cooling machine for cooling after passing the inspection. After cooling, the upper and lower surfaces are polished and then film is applied and stored.

[0015] Optionally, step eight includes metal impurity removal, a first conveyor belt is provided at the front end of the continuous press, a second conveyor belt is provided at the rear end of the pre-press, and the pre-pressed slab can be transferred to the first conveyor belt via the second conveyor belt; an impurity storage box is provided below between the first conveyor belt and the second conveyor belt, a tensioning wheel and a support wheel are provided at one end of the second conveyor belt close to the first conveyor belt, and the support wheel can drive the end of the second conveyor belt to move downward; a metal detector is provided on the second conveyor belt.

[0016] Optionally, the surface of the board is prone to over-curing due to high temperature, resulting in low strength and poor smoothness. After grinding off the over-cured layer of 0.3 to 0.8 mm, it is painted and further processed by laminating with melamine layer, PP film, aluminum skin, etc.

[0017] Optionally, the content of water sprayed in step one is 2-8% of the fiber raw material, preferably 3-6%; the content of water repellent in water is 3‰-8%, preferably 1-5%, and is sprayed on the surface of the material to make the board waterproof. Since the fibers are easy to agglomerate, which affects the use, in order to avoid their agglomeration, the content of dispersant added is 1-8%, preferably 1-5%, the content of coupling agent is 3‰-5%, preferably 1-3%, and the content of flame retardant is 1-8%, preferably 1-5%. This can increase the bonding viscosity between glue and glue when spraying, and then increase the strength of the board when curing.

[0018] Optionally, in step 1, the length of the fibers after being crushed is 250 um to 4500 um, preferably 250 um to 1500 um.

[0019] Optionally, the bottom of the crusher is connected to a cyclone through a conveying pipe, a fan is provided at one end of the conveying pipe away from the cyclone, and a negative pressure fan is provided at one end of the cyclone away from the conveying pipe; the fan and the negative pressure fan can convey the crushed and water-sprayed materials into the cyclone, and the bottom of the cyclone is connected to a fiber breakup machine through a valve.

[0020] Optionally, the powdered glue is powdered resin glue, and a flame retardant is added to the powdered glue.

[0021] Optionally, before paving the slab, the moisture content of the material is tested by an infrared moisture meter and the moisture content is adjusted to a set range; in step six, the paving slab is wider than the set plate material, so it is necessary to cut off the longitudinal edge of the slab before weighing the paving slab to make its width within the set range value.

[0022] The present invention also provides a rock wool decorative board, comprising a board body, the surface of which is spray-painted, and a melamine layer, a PP film or an aluminum sheet is attached, or the surface is subjected to a painting process.

[0023] Compared with the prior art, the present invention has achieved the following technical effects:

[0024] The present invention adopts rock wool fiber to make the board, which is pollution-free, recyclable and resource-saving. The whole processing and manufacturing process adopts mechanical integration, which reduces the labor intensity of operators and has high work efficiency. After the board is painted and film-laminated, various patterns can be formed on the surface, which is beautiful and durable. BRIEF DESCRIPTION OF THE DRAWINGS

[0025] In order to more clearly illustrate the embodiments of the present invention or the technical solutions in the prior art, the drawings required for use in the embodiments will be briefly introduced below. Obviously, the drawings described below are only some embodiments of the present invention. For ordinary technicians in this field, other drawings can be obtained based on these drawings without paying creative work.

[0026] Figure 1 This is a schematic diagram of the production process of the rock wool decorative board of the present invention;

[0027] Explanation of the reference numerals: 1-crusher, 2-nozzle, 3-conveying pipeline, 4-cyclone, 5-fan, 6-negative pressure fan, 7-bag dust collector, 8-fiber scatterer, 9-sorter, 10-scattering roller, 11-metering bin, 12-glue cylinder, 13-stirring mixer, 14-infrared moisture content meter, 15-paving mechanism, 16-edge saw, 17-pre-pressure steam heating system, 18-continuous press, 19-first conveyor belt, 20-second conveyor belt, 21-metal detector, 22-impurity storage box, 23-tensioning wheel, 24-support wheel, 25-bubble detection device, 26-double-sided polishing device. DETAILED DESCRIPTION

[0028] The following will be combined with the drawings in the embodiments of the present invention to clearly and completely describe the technical solutions in the embodiments of the present invention. Obviously, the described embodiments are only part of the embodiments of the present invention, not all of the embodiments. Based on the embodiments of the present invention, all other embodiments obtained by ordinary technicians in this field without creative work are within the scope of protection of the present invention.

[0029] The purpose of the present invention is to provide a rock wool decorative board production process and a rock wool decorative board to solve the problems existing in the above-mentioned prior art, with a high degree of automation, reducing the labor intensity of operators and improving work efficiency.

[0030] In order to make the above-mentioned objects, features and advantages of the present invention more obvious and easy to understand, the present invention is further described in detail below with reference to the accompanying drawings and specific embodiments.

[0031] The present invention provides a production process for rock wool decorative panels. Figure 1 As shown, the following steps are included:

[0032] Step 1: rock wool pretreatment. The rock wool after preliminary crushing is transported to the crusher 1 and crushed into fibers of a set length. The length of the fibers after crushing is 250um to 1500um. The nozzle 2 is used to spray water containing a hydrophobic agent, a dispersant and a coupling agent, and the mixture is mixed. The content of the sprayed water is 2 to 8% of the fiber raw material. The content of the hydrophobic agent in the water is 3‰ to 8%, which is sprayed on the surface of each fiber to make the board waterproof. Since the fibers are easy to agglomerate, thus affecting the use, in order to avoid agglomeration, a dispersant content of 1 to 8%, a coupling agent content of 3‰ to 5%, and a flame retardant content of 1-8% are added, which can increase the adhesion between glue and glue when spraying glue. The adhesive viscosity between the glues increases, thereby increasing the strength of the board when the board is solidified; the bottom of the crusher 1 is connected to a cyclone 4 through a conveying pipe 3, and a fan 5 is provided at the end of the conveying pipe 3 away from the cyclone 4, and a negative pressure fan 6 is provided at the end of the cyclone 4 away from the conveying pipe 3; under the high-pressure blowing action of the fan 5 and the suction action of the negative pressure fan 6, the crushed and water-sprayed mixed materials can be transported to the cyclone 4, and a bag dust collector 7 is provided on one side of the negative pressure fan 6, which can absorb smaller impurities such as rock wool debris. At the same time, the impurities in the bag dust collector 7 can be recycled, melted and reused to avoid waste; the bottom of the cyclone 4 is connected to a fiber scatterer 8 through a valve;

[0033] Step 2: Break up. Open the valve at the bottom of the cyclone 4, and the mixed material is transported to the fiber break up machine 8, where the fibers in the mixed material are broken up by the rotation of multiple rollers.

[0034] Step 3: sorting. The materials in the fiber breaker 8 are transported to the sorting machine 9. A fan 5 is connected to one side of the sorting machine 9. The fan 5 can screen out the impurities and agglomerated materials in step 2 through the sweeping effect of the high-pressure fan. The impurities are mainly slag balls, and the slag balls and agglomerated materials can be recycled and reused. The fiber-dispersed mixed material is transported to the second cyclone 4. A negative pressure fan 6 is also provided on one side of the second cyclone 4, and is connected to the bag dust collector 7 through a pipeline to assist in material transportation, and then enter the next step.

[0035] Step 4: the material is measured and broken up for the second time. The material enters the breaking roller 10 through the valve at the bottom of the second cyclone 4. After the second breaking up, it enters the metering bin 11 for weighing. The weighed material is broken up again and then enters the glue cylinder 12.

[0036] Step 5, four nozzles are provided in the glue barrel 12, and the powdered glue is atomized and sprayed onto the surface of the material with compressed air, and the powdered glue is sprayed into the mixed material. The powdered glue is a powder ball resin glue, and a flame retardant is added to the powdered glue to increase the fire resistance of the board and improve the fire resistance level of the board. The mixed material after spraying glue is stirred, and then the stirring mixer 13 is used to disperse and mix the mixed material;

[0037] Step 6: After the sprayed mixed material is broken up, it is evenly paved into a slab by a paving mechanism 15. The paving mechanism 15 is an existing device and will not be described in detail here. Before paving the slab, it is necessary to detect the moisture content of the material by an infrared moisture meter 14 and adjust the moisture content to a set range; in order to ensure that the final size of the board is qualified, the paved slab is wider than the set board, and it is necessary to cut off the longitudinal edge of the slab by an edge saw 16 before weighing the paved slab to make its width within the set range;

[0038] Step seven, pre-pressing the slab, the pre-pressing machine of the pre-pressing steam heating system 17 pre-presses the slab, the pre-pressing machine can use the pressing rollers arranged up and down to realize the pre-pressing of the slab, and the steam engine is used to apply steam heating during the pre-pressing process, the steam penetrates from the bottom surface to the core layer, and then penetrates to the surface, increasing the temperature of the core layer, facilitating the curing of the core layer, and reducing the curing time; increasing the temperature of the core layer, facilitating the subsequent heating and curing;

[0039] Step eight, sheet forming, a first conveyor belt 19 is provided at the front end of the continuous press 18, a second conveyor belt 20 is provided at the rear end of the pre-press, a metal detector 21 is provided on the second conveyor belt 20, and the pre-pressed sheet can be transferred to the first conveyor belt 19 via the second conveyor belt 20; an impurity storage box 22 is provided below between the first conveyor belt 19 and the second conveyor belt 20, a tensioning wheel 23 and a supporting wheel 24 are provided at one end of the second conveyor belt 20 close to the first conveyor belt 19, the second conveyor belt 20 is sequentially wound around the supporting wheel 24 and the tensioning wheel 23, and is used to support the second conveyor belt 20, and the supporting wheel 24 can drive the end of the second conveyor belt 20 to move downward, so that the end of the second conveyor belt 20 is inclined The slab containing metal impurities can be transported to the impurity storage box 22 below, and the support wheel 24 moves upward, driving the second conveyor belt 20 to move to a horizontal position. At this time, the slab without metal impurities can be transferred to the first conveyor belt 19, and the slab after removing the metal impurities is transported to the continuous press 18. The temperature in the continuous press 18 is raised to 225°~270°. Two closed steel belts arranged symmetrically up and down are arranged in the continuous press 18. The slab is located between the two steel belts. The upper and lower steel belts squeeze the slab for thermal curing and forming. The sheet forming process is connected to a bag dust collector at the paving step to recover impurities and dust generated in the process to ensure a safe processing environment.

[0040] Step nine, rejecting defective products. After rejecting defective products, the board is trimmed. When the core layer curing quality is poor, the board is prone to bubbling. Therefore, a bubbling detection device 25 is needed to detect whether the board has bubbles. The bubbling detection device 25 can use an infrared detector or a level meter, etc. If there are bubbles, it will be set as a defective product and rejected. The genuine board without bubbles is polished on the upper and lower surfaces by the double-sided polishing device 26 and then stored. The double-sided polishing device 26 has a thickness setting function. The board can be polished according to the required thickness requirements until it meets the set thickness requirements. The surface grinding device can use two grinding devices to grind the two sides of the plate respectively. The ground material can be melted and reused after being recovered by the recovery device to avoid waste. The recovery device includes a cyclone 4, a negative pressure fan 6 and a bag dust collector 7. The various components are used together to recover impurities generated during the grinding process. The surface of the plate is easily over-cured due to excessive temperature, with low strength and poor smoothness. After grinding off the over-cured layer of 0.3 to 0.8 mm, it is painted and subjected to deep processing processes such as melamine layer, PP film, and aluminum skin.

[0041] Further preferably, the present invention also provides a rock wool decorative board, comprising a board body, the surface of the board body is sprayed with paint, and is laminated with a melamine layer, a PP film or an aluminum sheet.

[0042] In the description of the present invention, it should be noted that the terms "center", "top", "bottom", "left", "right", "vertical", "horizontal", "inside", "outside" and the like indicate positions or positional relationships based on the positions or positional relationships shown in the accompanying drawings, which are only for the convenience of describing the present invention and simplifying the description, and do not indicate or imply that the device or element referred to must have a specific orientation, be constructed and operated in a specific orientation, and therefore cannot be understood as limiting the present invention. In addition, the terms "first" and "second" are used for descriptive purposes only and cannot be understood as indicating or implying relative importance.

[0043] The present invention uses specific examples to illustrate the principles and implementation methods of the present invention. The above examples are only used to help understand the method and core ideas of the present invention. At the same time, for those skilled in the art, according to the ideas of the present invention, there will be changes in the specific implementation methods and application scope. In summary, the content of this specification should not be understood as limiting the present invention.

Claims

1. A production process of rock wool decorative board, characterized by: The steps include: Step 1: rock wool pretreatment: the rock wool is transported to a crusher and crushed into fibers of a set length, sprayed with water containing a hydrophobic agent, a dispersant and a coupling agent, and mixed; Step 2: breaking up the mixed materials, conveying them to a fiber breaking machine to break up the fibers in the mixed materials; Step 3: sorting, screening out impurities and agglomerated materials in step 2, and conveying the mixed materials after fiber breaking to the next step; Step 4: Material measurement and secondary breaking; Step 5, spraying powdered glue into the mixed material, stirring, and then breaking up the sprayed mixed material; Step 6, breaking up the sprayed mixed material and evenly paving it into a slab, and weighing it; Step 7, pre-pressing the slab, the pre-pressing machine pre-presses the slab and applies steam heating at the same time; Step eight, sheet forming, the sheet blank after removing metal impurities is transported to a continuous press for thermal curing forming; Step nine, reject defective products, trim the edges of the boards after rejecting defective products, polish the surface and then store them.

2. The production process of rock wool decorative board according to claim 1, characterized in that: Step eight includes metal impurity removal. A first conveyor belt is provided at the front end of the continuous press, and a second conveyor belt is provided at the rear end of the pre-press. The pre-pressed slab can be transferred to the first conveyor belt via the second conveyor belt. An impurity storage box is provided below between the first conveyor belt and the second conveyor belt. A tensioning wheel and a support wheel are provided at one end of the second conveyor belt close to the first conveyor belt, and the support wheel can drive the end of the second conveyor belt to move downward. A metal detector is provided on the second conveyor belt.

3. The production process of rock wool decorative board according to claim 1, characterized in that: After grinding off the over-cured layer of 0.3 to 0.8 mm on the surface of the board, it is sprayed with paint and further processed by laminating with melamine layer or PP film.

4. The production process of rock wool decorative board according to claim 1, characterized in that: The content of the sprayed water in step 1 is 2-8% of the fiber raw material; the content of the hydrophobic agent in the water is 3‰-8%, the content of the dispersant is 1-8%, the content of the coupling agent is 3‰-5%, and the content of the flame retardant is 1-8%.

5. The production process of rock wool decorative board according to claim 1, characterized in that: In step 1, the length of the fiber after crushing is 250-4500um.

6. The production process of rock wool decorative board according to claim 1, characterized in that: The bottom of the crusher is connected to a cyclone through a conveying pipe, a fan is provided at one end of the conveying pipe away from the cyclone, and a negative pressure fan is provided at one end of the cyclone away from the conveying pipe; the fan and the negative pressure fan can convey the crushed and water-sprayed materials into the cyclone, and the bottom of the cyclone is connected to a fiber breakup machine.

7. The production process of rock wool decorative board according to claim 1, characterized in that: Flame retardant is added to the powdered glue.

8. The production process of rock wool decorative board according to claim 1, characterized in that: Before paving the slab, the moisture content of the material is detected and adjusted to the set range; in step six, the longitudinal edge of the slab is cut off before weighing the slab.

9. A rock wool decorative board, characterized in that: The utility model comprises a plate body, the surface of which is laminated with a melamine layer, a PP film or an aluminum sheet or is painted.

Citation Information

Patent Citations

  • Novel method for preparing mineral wool Vacuum Insulation Panel (VIP) core material

    CN102942305A

  • Modified mineral fiber cotton and preparation method thereof

    CN108947276A

  • Manufacturing method of silencing rock wool board heat-insulating system for building curtain wall

    CN110054416A

  • Method for manufacturing fireproof density plate

    CN110341216A

  • Rock fiber decorative sheet production process

    CN116198154A