Manganese iron ammonium phosphate and preparation method and application thereof
By controlling the pH value and process conditions of the reaction system of lithium iron manganese phosphate, ammonium iron manganese phosphate with secondary particles in the form of long flakes was successfully prepared, solving the problems of material performance and process complexity in the existing technology, and achieving high efficiency and high efficiency. Low-cost production of ferric ammonium manganese phosphate.
Patent Information
- Application Number
- CN202411079860.9
- Authority / Receiving Office
- CN · China
- Patent Type
- Applications(China)
- Current Assignee / Owner
- Filing Date
- 2024-08-07
- Publication Date
- 2024-10-15
- Estimated Expiration
- 2044-08-07
AI Technical Summary
The existing preparation process of lithium iron manganese phosphate has problems such as low electronic conductivity, small lithium ion diffusion coefficient, and low material compaction density. The process is complex and costly, and it is difficult to form uniform co-precipitated ammonium iron manganese phosphate materials.
Co-precipitation of divalent iron and divalent manganese with a phosphorus source is used. By controlling the pH value of the reaction system within the range of 2.0 to 6.0, water is used as the bottom liquid, the aging process is omitted, and the use of surfactants and organic solvents is avoided. Directly through solid-liquid separation, washing, drying and calcination, the secondary particles of ferric ammonium manganese phosphate are obtained in the form of long flakes.
The uniform co-precipitation of ammonium manganese phosphate is achieved, the amount of pH regulator is reduced, the process flow is simplified, it is suitable for industrial production, and a highly dispersible and low-cost ammonium ferromanganese phosphate material is obtained.
Smart Images

Figure CN118771341A_ABST
Abstract
Description
Technical Field
[0001] The invention belongs to the technical field of battery materials, and specifically discloses a precursor material of lithium manganese iron phosphate and a preparation method and application thereof. Background Art
[0002] Compared with traditional batteries, lithium-ion batteries have the advantages of high energy density, high voltage, long life, and environmental friendliness. They are widely used in electronic equipment, automobiles, aerospace and other fields. Lithium iron phosphate is a commonly used positive electrode material for lithium-ion batteries and has many advantages. However, due to its structural limitations, when used in batteries, it has the disadvantages of low electronic conductivity, small lithium ion diffusion coefficient, and low material compaction density, which greatly limits the application of lithium iron phosphate. In order to broaden the application of lithium iron phosphate, manganese compounds are currently introduced into lithium iron phosphate to form lithium iron manganese phosphate solid solution. Since manganese compounds have higher electrochemical reaction voltage and better electrolyte compatibility, lithium iron manganese phosphate solid solution obtains better capacity and cycle effect. Theoretically, it has a specific capacity of 171mAh / g and a discharge platform of about 4.1V. At the same time, it has the advantages of high safety, good cycle performance and safety and non-toxicity. This also makes lithium iron manganese phosphate an ideal positive electrode material for the new generation of lithium-ion power batteries.
[0003] CN115043387A discloses a method for preparing ammonium manganese iron phosphate, lithium manganese iron phosphate and its application, wherein a metal mixed salt solution, a diammonium phosphate solution and an organic solution are mixed to obtain a metal salt mixed solution and a phosphate mixed solution, and the metal salt mixed solution, the phosphate mixed solution and ammonia water are added to the bottom liquid in parallel to react, and the ammonium manganese iron phosphate is obtained by solid-liquid separation. The method controls the reaction pH to 8-9, uses a large amount of pH regulators such as ammonia water, and reacts in an organic solvent, which not only increases the cost but is also not conducive to washing.
[0004] CN114348982A discloses ferromanganese phosphate, lithium ferromanganese phosphate and preparation methods thereof, lithium ion batteries and electrical equipment, wherein raw materials including iron powder, manganese source and phosphoric acid are mixed, solid-liquid separation is performed to obtain ferromanganese phosphorus solution; the ferromanganese phosphorus solution is diluted with water and aged in an inert atmosphere to obtain ferromanganese phosphate trihydrate. This method requires acid dissolution, filtration and aging, has a long process flow, generates a large amount of wastewater and is relatively complicated to operate.
[0005] CN115231544A discloses a method for preparing ammonium manganese phosphate and a positive electrode material for a lithium ion battery. The method for preparing ammonium manganese phosphate comprises the following steps: mixing a manganese source solution, a phosphorus source solution and an ammonium source solution, aging the mixture, and then separating the solid from the liquid to obtain ammonium manganese phosphate. The method does not incorporate an iron source in the synthesis stage. If an iron source is introduced in a subsequent step, the process is complicated and it is difficult to form a homogeneous material.
[0006] CN116675204A discloses a preparation method of a dense ammonium manganese ferric phosphate precursor, a positive electrode material and a battery. The preparation method of the ammonium manganese ferric phosphate comprises the following steps: using pure water as a base liquid, feeding a phosphorus source, an iron-manganese mixed liquid and ammonia water in parallel, and finally performing post-treatment to obtain a spherical ammonium manganese ferric phosphate formed by accumulation of flaky primary particles. Summary of the invention
[0007] The purpose of the present invention is to provide an ammonium manganese iron phosphate material with secondary particles in the form of long thin flakes, and a preparation method and application thereof.
[0008] To achieve the above objectives, the present invention provides the following specific technical solutions.
[0009] Firstly, the present invention provides ammonium manganese ferric phosphate, the secondary particles of which are in the shape of long thin flakes.
[0010] In a further preferred embodiment, the tap density of the ammonium manganese iron phosphate is 0.5-1.5 g / cm 3 ; Specific surface area is 1~6m 2 / g.
[0011] Secondly, the present invention provides a method for preparing the above-mentioned ammonium manganese ferric phosphate, comprising the following steps: (1) dissolving a soluble divalent iron source, a divalent manganese source, and an antioxidant in water to obtain a mixed solution; (2) Using the mixed solution as the base solution, and flowing in the phosphorus source solution and the ammonia solution to carry out the reaction; maintaining the pH value of the reaction system at 2.0-6.0; (3) After the reaction is completed, the slurry obtained by the reaction is subjected to solid-liquid separation, and the solid phase obtained is washed, dried, and calcined. In a further preferred embodiment, the divalent iron source is one or more of ferrous sulfate, ferrous nitrate, ferrous chloride, ferrous oxalate and ferrous acetate.
[0012] In a further preferred embodiment, the divalent manganese source is one or more of manganese sulfate, manganese nitrate, manganese chloride and manganese carbonate.
[0013] In a further preferred embodiment, the antioxidant is one or more of sodium sulfite, ammonium sulfite, 2,6-di-tert-butyl-4-methylphenol (BHT), and ascorbic acid.
[0014] In a further preferred embodiment, in the mixed solution, the concentration of the divalent iron is 0.2-1.5 mol / L; the concentration of the divalent manganese is 0.5-2.0 mol / L; and the concentration of the antioxidant is 0.001-0.01 mol / L.
[0015] In a further preferred embodiment, the phosphorus source in the phosphorus source solution is one or more of phosphoric acid, monoammonium phosphate, diammonium hydrogen phosphate, ammonium dihydrogen phosphate, ammonium phosphate, disodium hydrogen phosphate, sodium dihydrogen phosphate, and sodium phosphate.
[0016] In a further preferred embodiment, the concentration of the phosphorus source solution is 2-6 mol / L.
[0017] In a further preferred embodiment, the feed flow rate of the phosphorus source solution is 100-1200 ml / min.
[0018] In a further preferred embodiment, the concentration of the aqueous ammonia solution is 4-12 mol / L; further preferably, it is 5-10 mol / L.
[0019] In a further preferred embodiment, the temperature of the reaction system is 50-80°C.
[0020] In a further preferred embodiment, the reaction is stirred during the reaction; and further preferably, the stirring speed is 100-1000 rpm.
[0021] In a further preferred embodiment, the calcination temperature is 400-700° C., and the calcination time is 1-6 hours.
[0022] Based on the same inventive concept, the present invention seeks to protect the lithium manganese iron phosphate material prepared using the aforementioned ammonium manganese iron phosphate as raw material.
[0023] In addition, the present invention claims protection for a battery comprising the aforementioned lithium manganese iron phosphate material.
[0024] Compared with the prior art, the above one or more technical solutions of the present invention can achieve at least one of the following beneficial effects: The invention adopts divalent iron and divalent manganese metal elements to co-precipitate with a phosphorus source, has simple operation, stable process control, and is suitable for industrial production.
[0025] In the present invention, the three elements of manganese, iron and phosphorus can be uniformly co-precipitated, and the chemical composition is close to the designed value.
[0026] In the process of preparing ammonium manganese iron phosphate, the present invention does not require surfactants, organic solvents, etc., the raw materials do not need to be oxidized in advance, and the aging process is omitted, which has the advantage of low cost.
[0027] The pH value of the synthetic ammonium manganese ferric phosphate of the invention is low, and the dosage of the pH regulator can be effectively reduced.
[0028] The secondary particles of the ammonium manganese ferric phosphate prepared by the invention are in the shape of long thin flakes, have a special morphology and good dispersibility, and are a new product. BRIEF DESCRIPTION OF THE DRAWINGS
[0029] Figure 1 This is the XRD pattern of the precursor material obtained in Example 1.
[0030] Figure 2 This is the SEM image of the precursor material obtained in Example 1.
[0031] Figure 3 This is the SEM image of the precursor material obtained in Comparative Example 1.
[0032] Figure 4 This is the SEM image of the precursor material obtained in Comparative Example 2.
[0033] Figure 5 This is the SEM image of the precursor material obtained in Comparative Example 3.
[0034] Figure 6 This is the SEM image of the precursor material obtained in Comparative Example 4. DETAILED DESCRIPTION
[0035] In the process of studying the precursor of lithium manganese iron phosphate, the applicant obtained ammonium manganese iron phosphate with secondary particles in the form of long thin sheets by changing the preparation process. In addition, it was found during the research process that the combination of the composition of the base liquid and the pH value of the reaction system has a great influence on the morphology of ammonium manganese iron phosphate. This will be reflected in the specific examples and comparative examples below.
[0036] Some embodiments provide ammonium manganese ferric phosphate, wherein the secondary particles of the ammonium manganese ferric phosphate are in the form of long thin flakes.
[0037] In some preferred embodiments, the tap density of the ammonium manganese iron phosphate is 0.5-1.5 g / cm 3 ; Specific surface area is 1~6m 2 / g.
[0038] The secondary particles are in the form of long thin flakes, which is a unique morphology of the ammonium manganese ferric phosphate obtained in the present invention and is the first creation of the applicant.
[0039] Some embodiments provide a method for preparing the above-mentioned ammonium manganese ferrous phosphate, comprising the following steps: (1) dissolving a soluble divalent iron source, a divalent manganese source, and an antioxidant in water to obtain a mixed solution; (2) Using the mixed solution as the base solution, and flowing in the phosphorus source solution and the ammonia solution to carry out the reaction; maintaining the pH value of the reaction system at 2.0-6.0; (3) After the reaction is completed, the slurry obtained by the reaction is subjected to solid-liquid separation, and the solid phase obtained is washed, dried, and calcined.
[0040] In the process of preparing ammonium manganese iron phosphate or other precursor materials by coprecipitation process, pure water or alkaline solution is generally used as the base liquid. For example, CN116675204A mentioned in the background technology uses pure water as the base liquid to obtain spherical ammonium manganese iron phosphate in which flaky primary particles are piled up. The present invention takes a different approach, using a mixed solution composed of a divalent iron source, a divalent manganese source and an antioxidant as the base liquid, and adjusting the pH value of the reaction system to 2.0~6.0 to obtain ammonium manganese iron phosphate in the form of long thin strips of secondary particles. The regulation of the base liquid and the pH value are indispensable.
[0041] In some preferred embodiments, the divalent iron source is one or more of ferrous sulfate, ferrous nitrate, ferrous chloride, ferrous oxalate, and ferrous acetate. In some preferred embodiments, the divalent manganese source is one or more of manganese sulfate, manganese nitrate, manganese chloride, manganese perchlorate, and manganese carbonate.
[0042] In some preferred embodiments, the antioxidant is one or more of sodium sulfite, ammonium sulfite, BHT, and ascorbic acid.
[0043] In some preferred embodiments, in the mixed solution, the concentration of the divalent iron is 0.2-1.5 mol / L; the concentration of the divalent manganese is 0.5-2.0 mol / L; and the concentration of the antioxidant is 0.001-0.01 mol / L.
[0044] In actual operation, the Mn / Fe molar ratio can be adjusted by controlling the concentrations of divalent iron and divalent manganese in the mixed solution. For example, the Mn / Fe molar ratio can be adjusted to 1.5.
[0045] In some preferred embodiments, the phosphorus source in the phosphorus source solution is one or more of phosphoric acid, monoammonium phosphate, diammonium hydrogen phosphate, ammonium dihydrogen phosphate, ammonium phosphate, disodium hydrogen phosphate, sodium dihydrogen phosphate, and sodium phosphate.
[0046] In some preferred embodiments, the concentration of the phosphorus source solution is 2-6 mol / L.
[0047] In some preferred embodiments, the feed flow rate of the phosphorus source solution is 100-1200 ml / min.
[0048] In some preferred embodiments, the concentration of the aqueous ammonia solution is 4-12 mol / L; more preferably, it is 5-10 mol / L.
[0049] In the reaction process of the present invention, aqueous ammonia serves as both a provider of ammonium and a pH regulator.
[0050] In some preferred embodiments, the temperature of the reaction system is 50-80° C. If the temperature is too high, the secondary particles become thicker and denser, and the BET decreases; if the temperature is too low, the coprecipitation reaction is incomplete, the Fe and P content in the supernatant exceeds the standard, and the metal ratio of the product is out of control.
[0051] In some preferred embodiments, the reaction is stirred during the reaction, and preferably the stirring speed is 100-1000 rpm. Stirring allows the materials in the reaction system to be mixed more fully and evenly.
[0052] In some preferred embodiments, the calcination temperature is 400-700° C., and the calcination time is 1-6 hours. The calcination process will affect the phase composition of the product. It is difficult to prepare pure ammonium manganese iron phosphate phase when the calcination temperature is too high or too low.
[0053] In order to facilitate the understanding of the present invention, the present invention will be described more comprehensively and meticulously below in conjunction with the accompanying drawings and preferred embodiments of the present invention, but the protection scope of the present invention is not limited to the following specific embodiments.
[0054] Unless otherwise defined, all the professional terms used below have the same meanings as those generally understood by those skilled in the art. The professional terms used herein are only for the purpose of describing specific embodiments and are not intended to limit the scope of protection of the present invention.
[0055] Unless otherwise specified, various raw materials, reagents, instruments and equipment used in the present invention can be purchased from the market or prepared by existing methods.
[0056] Example 1 Step S1, preparation of mixed solution: Dissolving ferrous sulfate, manganese sulfate and ascorbic acid in deionized water to prepare a manganese-iron mixed solution; in the manganese-iron mixed solution, the total concentration of manganese-iron metal ions is 1.5 mol / L, the concentration of manganese ions is 0.9 mol / L, the concentration of iron ions is 0.6 mol / L, and the molar concentration of ascorbic acid is 0.0028 mol / L; Step S2, preparation of phosphorus source solution: Dissolve monoammonium phosphate in deionized water to prepare a 4.2 mol / L solution; Step S3, preparing an ammonia solution: Prepare 6 mol / L ammonia solution; Step S4, synthesis reaction: Use 50L of manganese-iron mixed solution as the base liquid and stir at a speed of 523rpm; under stirring, introduce the phosphorus source solution and ammonia solution into the reactor in parallel, and control the flow rate of the phosphorus source solution at 200mL / min; maintain the temperature of the reaction system in the reactor at 65°C and the pH value at 4.5±0.1.
[0057] After 35 L of phosphorus source solution was added, the feeding was stopped to obtain a reaction slurry; Step S5: The reaction slurry is subjected to solid-liquid separation to obtain a filter cake, and the filter cake is washed and centrifuged for dehydration; Step S6: The dehydrated material was placed in an oven and dried at 120° C. for 10 h; then it was transported to a muffle furnace and calcined at 400° C. for 2 h to obtain a precursor material.
[0058] Comparative Example 1 The difference between Comparative Example 1 and Example 1 is that the synthesis reaction is different, specifically: Step S4, synthesis reaction: Use 50L of deionized water as the base liquid and stir at a speed of 523rpm; under stirring, introduce the iron-manganese mixed solution, phosphorus source solution and ammonia solution into the reactor in parallel, the flow rate of the phosphorus source solution is controlled at 140mL / min, and the flow rate of the iron-manganese mixed solution is 200mL / min; maintain the temperature of the reaction system in the reactor at 65°C and the pH value at 4.5±0.1.
[0059] After 50 L of the iron-manganese mixed solution and 35 L of the phosphorus source solution were fed, the feeding was stopped to obtain a reaction slurry.
[0060] Comparative Example 2 The difference between Comparative Example 2 and Example 1 is that the synthesis reaction is different, specifically: Step S4, synthesis reaction: Use 50L of 6.0mol / L ammonia solution as the base liquid and stir at a speed of 523rpm; under stirring, introduce the iron-manganese mixed solution and the phosphorus source solution into the reactor in parallel, the flow rate of the phosphorus source solution is controlled at 140mL / min, and the flow rate of the iron-manganese mixed solution is 200mL / min; maintain the temperature of the reaction system in the reactor at 65°C.
[0061] After 50 L of the iron-manganese mixed solution and 35 L of the phosphorus source solution were fed, the feeding was stopped to obtain a reaction slurry.
[0062] Comparative Example 3 The difference between Comparative Example 3 and Example 1 is that: in step S4, during the synthesis reaction, the temperature of the reaction system in the reactor is maintained at 65° C. and the pH value is maintained at 6.5±0.1.
[0063] Comparative Example 4 The difference between Comparative Example 4 and Example 1 is that: in step S4, during the synthesis reaction, the temperature of the reaction system in the reactor is maintained at 65° C. and the pH value is maintained at 1.5±0.1.
[0064] Example 2 Step S1, preparation of mixed solution: Dissolving ferrous nitrate, manganese chloride and sodium sulfite in deionized water to prepare a manganese-iron mixed solution; in the manganese-iron mixed solution, the total concentration of manganese-iron metal ions is 1.0 mol / L, the concentration of manganese ions is 0.6 mol / L, the concentration of iron ions is 0.4 mol / L, and the concentration of sodium sulfite is 0.005 mol / L; Step S2, preparation of phosphorus source solution: Dissolve diammonium hydrogen phosphate in deionized water to prepare a 5 mol / L solution; Step S3, preparing an ammonia solution: Prepare 5 mol / L ammonia solution; Step S4, synthesis reaction: Use 50L of manganese-iron mixed solution as the base liquid and stir at a speed of 800rpm; under stirring, introduce the phosphorus source solution and ammonia solution into the reactor in parallel, and control the flow rate of the phosphorus source solution at 500mL / min; maintain the temperature of the reaction system in the reactor at 80°C and the pH value at 2.5±0.5.
[0065] After 20 L of phosphorus source solution was added, the feeding was stopped to obtain a reaction slurry; Step S5: The reaction slurry is subjected to solid-liquid separation to obtain a filter cake, and the filter cake is washed and centrifuged for dehydration; Step S6: The dehydrated material was placed in an oven and dried at 120° C. for 10 h; then it was transported to a muffle furnace and calcined at 600° C. for 2 h to obtain a precursor material.
[0066] Example 3 Step S1, preparation of mixed solution: Dissolving ferrous oxalate, manganese carbonate and ammonium sulfite in deionized water to prepare a manganese-iron mixed solution; in the manganese-iron mixed solution, the total concentration of manganese-iron metal ions is 1.25 mol / L, the concentration of manganese ions is 0.75 mol / L, the concentration of iron ions is 0.5 mol / L, and the concentration of ammonium sulfite is 0.01 mol / L; Step S2, preparation of phosphorus source solution: Dissolve phosphoric acid in deionized water to prepare a 6 mol / L solution; Step S3, preparing an ammonia solution: Prepare 4 mol / L ammonia solution; Step S4, synthesis reaction: Use 50L of manganese-iron mixed solution as the base liquid and stir at a stirring speed of 300rpm; under stirring, introduce the phosphorus source solution and ammonia solution into the reactor in parallel, and control the flow rate of the phosphorus source solution at 1200mL / min; maintain the temperature of the reaction system in the reactor at 50°C and the pH value at 5.5±0.5.
[0067] After 20.8 L of phosphorus source solution was added, the feeding was stopped to obtain a reaction slurry; Step S5: The reaction slurry is subjected to solid-liquid separation to obtain a filter cake, and the filter cake is washed and centrifuged for dehydration; Step S6: The dehydrated material was placed in an oven and dried at 120° C. for 10 h; then it was transported to a muffle furnace and calcined at 700° C. for 2 h to obtain a precursor material.
[0068] Example 4 Step S1, preparation of mixed solution: Dissolve ferrous sulfate, manganese sulfate and BHT in deionized water to prepare a manganese-iron mixed solution; in the manganese-iron mixed solution, the total concentration of manganese-iron metal ions is 1.75 mol / L, the concentration of manganese ions is 1.05 mol / L, the concentration of iron ions is 0.7 mol / L, and the molar concentration of BHT is 0.001 mol / L; Step S2, preparation of phosphorus source solution: Dissolve sodium dihydrogen phosphate in deionized water to prepare a 4 mol / L solution; Step S3, preparing an ammonia solution: Prepare 8 mol / L ammonia solution; Step S4, synthesis reaction: Use 50L of manganese-iron mixed solution as the base liquid and stir at a speed of 100rpm; under stirring, introduce the phosphorus source solution and ammonia solution into the reactor in parallel, and control the flow rate of the phosphorus source solution at 100mL / min; maintain the temperature of the reaction system in the reactor at 75±5℃ and the pH value at 5±1.
[0069] After 43.75 L of phosphorus source solution was added, the feeding was stopped to obtain a reaction slurry; Step S5: The reaction slurry is subjected to solid-liquid separation to obtain a filter cake, and the filter cake is washed and centrifuged for dehydration; Step S6: The dehydrated material was placed in an oven and dried at 120° C. for 10 h; then it was transported to a muffle furnace and calcined at 500° C. for 6 h to obtain a precursor material.
[0070] Figure 1 This is the XRD diagram of the precursor material obtained in Example 1. It can be seen that the precursor material is ammonium manganese ferrous phosphate.
[0071] Figure 2 This is the SEM image of the precursor material obtained in Example 1. It can be seen that the precursor material is in the form of long thin flakes with good dispersibility.
[0072] Figure 3 This is the SEM picture of the precursor material obtained in Comparative Example 1. It can be seen that the precursor material is a sphere with high sphericity formed by stacking sheets in series.
[0073] Figure 4 This is the SEM picture of the precursor material obtained in Comparative Example 2. It can be seen that the precursor material is a spherical shape formed by oblique stacking of sheets, and the sphericity is relatively low.
[0074] Figure 5 This is the SEM image of the precursor material obtained in Comparative Example 3. It can be seen that the precursor material is in the form of irregularly shaped flakes.
[0075] Figure 6 This is a SEM image of the precursor material obtained in Comparative Example 4. It can be seen that the precursor material is a thick sheet formed by stacking irregularly shaped sheets.
[0076] By comparing and analyzing the reactor bottom liquid of Example 1 and Comparative Examples 1-4, the pH control of the reaction system, and the SEM images of the obtained precursor materials, it is not difficult to determine that the present invention has taken a different approach and successfully prepared long thin sheet precursor materials by selecting the reactor bottom liquid and regulating the pH of the reaction process; if the reactor bottom liquid is different or the pH of the reaction process is not regulated within the range of 2 to 6, the long thin sheet precursor material cannot be obtained.
[0077] The tap density and specific surface area of the precursor materials obtained in Examples 1-4 and Comparative Examples 1-4 were measured in the following manner.
[0078] Tap density: measured by a BT-313 tap density meter.
[0079] Specific surface area: measured by a specific surface area tester model BSD-BET400.
[0080] The test results are shown in Table 1.
[0081] Table 1 The above is only a preferred embodiment of the present invention. It should be pointed out that for ordinary technicians in this technical field, several improvements and modifications can be made without departing from the principle of the present invention. These improvements and modifications should also be regarded as the scope of protection of the present invention.
Claims
1. Ammonium ferromanganese phosphate, It is characterized in that The secondary particles of the ammonium manganese ferric phosphate are in the shape of long thin flakes.
2. Ammonium ferric manganese phosphate as claimed in claim 1, It is characterized in that The tap density of the ammonium manganese iron phosphate is 0.5-1.5 g / cm 3 ; Specific surface area is 1~6m 2 / g.
3. A method for preparing ammonium manganese ferrophosphate, It is characterized in that The following steps are involved: (1) dissolving a soluble divalent iron source, a divalent manganese source, and an antioxidant in water to obtain a mixed solution; (2) Using the mixed solution as the base solution, and flowing in the phosphorus source solution and the ammonia solution to carry out the reaction; maintaining the pH value of the reaction system at 2.0-6.0; (3) After the reaction is completed, the slurry obtained by the reaction is subjected to solid-liquid separation, and the solid phase obtained is washed, dried, and calcined.
4. The preparation method according to claim 3, It is characterized in that The divalent iron source is one or more of ferrous sulfate, ferrous nitrate, ferrous chloride, ferrous oxalate, and ferrous acetate; Preferably, the divalent manganese source is one or more of manganese sulfate, manganese nitrate, manganese chloride and manganese carbonate; Preferably, the antioxidant is one or more of sodium sulfite, ammonium sulfite, 2,6-di-tert-butyl-4-methylphenol (BHT), and ascorbic acid.
5. The preparation method according to claim 3 or 4, It is characterized in that In the mixed solution, the concentration of the divalent iron is 0.2-1.5 mol / L; Preferably, the concentration of divalent manganese is 0.5-2.0 mol / L; Preferably, the concentration of the antioxidant is 0.001-0.01 mol / L.
6. The preparation method according to claim 3, It is characterized in that The phosphorus source in the phosphorus source solution is one or more of phosphoric acid, monoammonium phosphate, diammonium hydrogen phosphate, ammonium dihydrogen phosphate, ammonium phosphate, disodium hydrogen phosphate, sodium dihydrogen phosphate, and sodium phosphate; Preferably, the concentration of the phosphorus source solution is 2-6 mol / L; Preferably, the feed flow rate of the phosphorus source solution is 100-1200 ml / min; Preferably, the concentration of the aqueous ammonia solution is 4-12 mol / L; more preferably, it is 5-10 mol / L.
7. The preparation method according to claim 3, It is characterized in that In step (2), the temperature of the reaction system is 50-80°C; Preferably, the reaction is stirred during the reaction; more preferably, the stirring speed is 100-1000 rpm.
8. The preparation method according to any one of claims 3 to 7, It is characterized in that In step (3), the calcination temperature is 400-700°C; Preferably, the calcination time is 1 to 6 hours.
9. A lithium iron manganese phosphate material, It is characterized in that The method is prepared using the ammonium manganese ferric phosphate described in claim 1 or 2 or the ammonium manganese ferric phosphate prepared by the preparation method according to any one of claims 3 to 8 as a raw material.
10. A battery, It is characterized in that Including the lithium manganese iron phosphate material as described in claim 9.
Citation Information
Patent Citations
Method for preparing high-density lithium iron manganese phosphate for lithium ion battery positive electrode material
CN101764203A
Cathode material, preparation method of cathode material, and lithium ion battery
CN110759325A
Lithium iron phosphate and continuous production method thereof
CN116062726A
Doped lithium iron manganese phosphate material, preparation method and application
CN116259754A
Lithium manganese iron phosphate precursor as well as preparation method and application thereof
CN117125690A