A lithium iron phosphate material and its preparation method and application

The titanium source is prepared by using amino acids and titanium tetrachloride coordination complexing reaction in lithium iron phosphate materials, and sintered in combination with high-temperature solid phase method of lithium carbonate and iron phosphate to form a material with a uniform carbon coating layer and through nitrogen Element doping solves the problem of insufficient conductivity of lithium iron phosphate materials, significantly improves its rate performance and cycling performance, and expands its application range.

CN118771343BActive Publication Date: 2024-12-03HUNAN YUNENG NEW ENERGY BATTERY MATERIALS CO LTD
View PDF 2 Cites 0 Cited by

Patent Information

Application Number
CN202411257686.2
Authority / Receiving Office
CN · China
Patent Type
Patents(China)
Current Assignee / Owner
Filing Date
2024-09-09
Publication Date
2024-12-03
Estimated Expiration
2044-09-09

AI Technical Summary

Technical Problem

The conductivity of lithium iron phosphate materials is poor, and the lithium ion diffusion performance and tap density are insufficient, which limits its application in high-power electric equipment.

Method used

The titanium source is prepared by the coordination complex reaction of amino acids and titanium tetrachloride, combined with lithium carbonate and iron phosphate, and high-temperature solid phase sintering is carried out to form a lithium iron phosphate material with a uniform carbon coating layer, and doped by nitrogen element Improve electron conductivity and ionic conductivity.

Benefits of technology

It significantly improves the electronic conductivity and ionic conductivity of lithium iron phosphate material, improves its rate performance and cycling performance, broadens its application range as a battery positive electrode material, simplifies the preparation process, and reduces production costs.

✦ Generated by Eureka AI based on patent content.

Smart Images

  • Figure SMS_1
    Figure SMS_1
Patent Text Reader

Abstract

The invention discloses a lithium iron phosphate material and a preparation method and application thereof, belonging to the technical field of lithium ion batteries, and the preparation method of the lithium iron phosphate material comprises the following steps: step 1, under an argon atmosphere, adding amino acid to benzene and stirring, adding titanium tetrachloride, stirring for 20-30min, reducing pressure, adding dichloromethane and continuing stirring, evaporating, filtering, and vacuum drying to obtain a titanium source; step 2, adding lithium carbonate, iron phosphate and titanium source to deionized water for mixing, followed by grinding treatment to obtain a slurry; step 3, drying the slurry obtained in step 2; step 4, under a nitrogen atmosphere, sintering the dried slurry in step 3, cooling to room temperature, and obtaining a lithium iron phosphate material. The obtained lithium iron phosphate material has excellent ion electron transfer rate, rate performance and capacity performance, etc., and can be used to prepare a lithium ion battery with good conductivity, high specific capacity and high power density.
Need to check novelty before this filing date? Find Prior Art

Description

Technical Field

[0001] The present invention belongs to the technical field of lithium ion batteries, and in particular relates to a lithium iron phosphate material and a preparation method and application thereof. Background Art

[0002] As a positive electrode material for lithium-ion batteries, lithium iron phosphate (LiFePO 4 ) is considered to be one of the best positive electrode materials for preparing long-life, high-power, high-safety, low-cost lithium-ion power batteries or energy storage batteries because of its stable olivine structure, ability to reversibly insert and extract lithium, high voltage, high specific capacity, good cycle performance, stable electrochemical properties, low raw material price, and environmental friendliness.

[0003] However, as a positive electrode material, lithium iron phosphate still has some inherent structural defects: the lithium ion migration rate, electronic conductivity and tap density of the material are all low. The lithium ion diffusion coefficient in lithium iron phosphate materials is relatively low, so that the rate performance of the material cannot meet the needs of high-power electric equipment, thus limiting the application scope of lithium iron phosphate. Due to the poor conductivity and low lithium ion diffusion coefficient of lithium iron phosphate positive electrode materials themselves, domestic and foreign researchers have conducted a lot of research in these aspects and achieved some good results. Researchers mostly use technical means such as morphology and size control, carbon coating and ion doping to overcome the inherent defects of the material. Nano-sizing of particles can increase the specific surface area of ​​the material, effectively shorten the diffusion path of lithium ions and thus improve its diffusion rate; the special morphology structure can increase the contact between the material and the electrolyte, provide more electrochemically active sites, and facilitate the rapid insertion and extraction of lithium ions. Doping with metal ions can cause lattice defects in lithium iron phosphate, broaden the diffusion channel of ions, reduce the energy gap width to improve the electronic conductivity of the material, but there are still disadvantages such as difficulty in preparation, uneven doping of metal compounds, and failure to fully and evenly mix with lithium source, phosphorus source, and iron source, which leads to insignificant improvement in conductivity. Carbon coating can not only improve the conductivity of the material, but also limit the growth of grains and inhibit the agglomeration of particles. Although carbon coating can improve the battery performance of lithium iron phosphate to a certain extent, there are many difficulties and challenges in carbon coating in actual production. For example: However, carbon coating has the following problems: (1) The process is complicated and the coating process is difficult to control; (2) After coating with a layer of carbon, the compaction density is low and it cannot be broken by force, which easily causes the coated carbon layer to peel off, thereby affecting the electrical performance; (3) For lithium iron phosphate particles, the addition of carbon source can improve the conductivity of the material to a certain extent, but this only changes the conductivity between particles, and the conductivity of the electrons inside the particles does not change, and its conductivity is still insufficient.

[0004] Therefore, it is urgent to develop a lithium iron phosphate positive electrode material with high conductivity, excellent lithium ion diffusion performance, high tap density and simple process, so as to expand its application range. Summary of the invention

[0005] The object of the present invention is to provide a lithium iron phosphate material and a preparation method and application thereof, so as to solve the problem of poor conductivity of lithium iron phosphate materials in the prior art.

[0006] The purpose of the present invention can be achieved through the following technical solutions:

[0007] A first aspect of the present invention provides a method for preparing a lithium iron phosphate material, comprising the following steps:

[0008] Step 1. Under an argon atmosphere, add amino acid to benzene and stir, add titanium tetrachloride, stir for 20-30 minutes, reduce pressure, add dichloromethane and continue stirring, evaporate, filter, and vacuum dry to obtain a titanium source; the titanium source is obtained by using amino acid and titanium tetrachloride through coordination complex reaction. Compared with directly adding titanium tetrachloride as the titanium source, the amino acid is coordinated with titanium ions, so that the surface of the titanium source particles is smoother, the particle size distribution is uniform, and the titanium source has a good dispersion effect.

[0009] Step 2, adding lithium carbonate, iron phosphate and the titanium source into deionized water for mixing, and then grinding to obtain a slurry;

[0010] Step 3, drying the slurry obtained in step 2;

[0011] Step 4: Under a nitrogen atmosphere, sinter the slurry dried in step 3 and cool it to room temperature to obtain a lithium iron phosphate material.

[0012] As a further embodiment of the present invention, the ratio of the amino acid, benzene and titanium tetrachloride used in step 1 is 2-2.2 mmol: 15 mL: 1-1.1 mmol.

[0013] As a further embodiment of the present invention, the amino acid in step 1 is one of valine, leucine, methionine and proline.

[0014] As a further solution of the present invention, the grinding treatment method in step 2 is: ball milling treatment and sand milling treatment in sequence.

[0015] As a further solution of the present invention, during the ball milling treatment, the rotation speed is 300-350 r / min and the ball milling time is 10-12 h.

[0016] As a further solution of the present invention, in the sand grinding process, the particles are sand ground to a particle size of 200-400 nm.

[0017] As a further solution of the present invention, in step 2, the mass ratio of lithium carbonate: iron phosphate: titanium source is 10-30: 60-85: 0.5-1.

[0018] As a further solution of the present invention, in step 3, the drying temperature is 80-90° C., and the drying time is 1-1.5 hours; in step 4, the sintering temperature is 700-800° C., and the sintering time is 10-12 hours.

[0019] The second aspect of the present invention provides a lithium iron phosphate material obtained by the preparation method described in the first aspect.

[0020] The third aspect of the present invention provides the use of the lithium iron phosphate material described in the second aspect in a lithium ion battery.

[0021] Beneficial effects of the present invention:

[0022] The present invention uses lithium carbonate, iron phosphate and titanium source as raw materials, and prepares lithium iron phosphate material with excellent electrochemical performance through high temperature solid phase method. At the same time, the raw materials used are widely available, the preparation method is simple, and industrial mass production can be carried out. The addition of Ti in the raw materials effectively improves the electrochemical performance of lithium iron phosphate materials. 4+ The ionic radius of Li + The ionic radius of Ti is the same, so 4+ It tends to occupy the Li position, reducing the interplanar spacing and particle size, and it is easy to form Fe in the lattice. 2+ / Fe 3+ The mixed valence state of the lithium iron phosphate material is improved, thereby improving the charge-discharge performance and cycle performance of the lithium iron phosphate material. At the same time, the homemade titanium source contains amino acids, which are a natural organic carbon source and organic nitrogen source. While doping titanium, the carbon coating of the lithium iron phosphate is achieved, forming a uniform carbon layer. At this time, the nitrogen element is also evenly distributed in the network structure of the carbon coating layer. The nitrogen element has a higher electronegativity than the carbon element. After the nitrogen element is doped into the carbon network structure, a non-intrinsic, disordered carbon structure and a continuous electronic conductive layer are formed, which can promote the kinetic process of lithium ion embedding or extraction, and significantly improve the rate performance of the material; and the lone pair of electrons of the nitrogen element itself will promote the electrical properties and chemical activity of the nearby carbon elements, thereby significantly improving the electrochemical properties of the lithium iron phosphate material.

[0023] Furthermore, in the present invention, valine, leucine, methionine and proline, each of which contains only one amino group and one carboxyl group, are selected as ligands to undergo a chelating reaction with titanium tetrachloride, and the obtained amino acid titanium chelate has a large specific surface area and high porosity, providing a large number of active sites that can absorb lithium ions, promoting their release or embedding, thereby improving the capacity of the lithium iron phosphate material.

[0024] The present invention improves the electronic conductivity and ionic conductivity of the lithium iron phosphate material through carbon coating, nitrogen doping and titanium doping, significantly improves its lithium ion transmission rate, rate performance and capacity performance, and further broadens the application scope of the lithium iron phosphate material as a battery positive electrode material.

[0025] The preparation method of the present invention has simple process, low energy consumption and production cost, can be industrialized for continuous, large-scale and stable production, and the produced lithium iron phosphate positive electrode material has good electrochemical properties and excellent processing performance. DETAILED DESCRIPTION

[0026] The following will be combined with the embodiments of the present invention to clearly and completely describe the technical solutions in the embodiments of the present invention. Obviously, the described embodiments are only part of the embodiments of the present invention, not all of the embodiments. Based on the embodiments of the present invention, all other embodiments obtained by ordinary technicians in this field without creative work are within the scope of protection of the present invention.

[0027] Example 1

[0028] This embodiment provides a method for preparing a lithium iron phosphate material, and the preparation steps are as follows:

[0029] Step 1, under argon atmosphere, add 2 mmol of valine to 15 mL of benzene and stir, add 1 mmol of titanium tetrachloride, stir for 20 min, remove benzene under reduced pressure, add 8 mL of dichloromethane, continue stirring, evaporate and remove dichloromethane, filter, and dry in a vacuum drying oven at 60°C for 3.5 h to obtain a titanium source;

[0030] Step 2, adding 15g of lithium carbonate, 65g of iron phosphate and 0.5g of the titanium source obtained in step 1 into deionized water for mixing, and then ball milling, the rotation speed during the ball milling process is 300r / min, the ball milling time is 10h, and then sand milling is performed to a particle size of 250nm to obtain a slurry;

[0031] Step 3: Place the slurry obtained in step 2 in an oven for drying at a temperature of 85°C for 1.5 hours;

[0032] Step 4: In a nitrogen atmosphere, the dried slurry in step 3 is placed in a tubular furnace for sintering at a temperature of 700° C. for 12 h, and then cooled to room temperature to obtain a lithium iron phosphate material.

[0033] The lithium iron phosphate material is prepared through the above steps.

[0034] Example 2

[0035] Compared with Example 1, the only difference is:

[0036] Replace valine with leucine in step 1, using the same amount.

[0037] Example 3

[0038] Compared with Example 1, the only difference is:

[0039] Replace valine with methionine in step 1, using the same amount.

[0040] Example 4

[0041] Compared with Example 1, the only difference is:

[0042] Replace valine with proline in step 1, using the same amount.

[0043] Example 5

[0044] Compared with Example 1, the only difference is:

[0045] Step 1. Under argon atmosphere, add 2.2 mmol of valine to 15 mL of benzene and stir, add 1.1 mmol of titanium tetrachloride, stir for 20 min, remove benzene under reduced pressure, add 8 mL of dichloromethane, continue stirring, evaporate and remove dichloromethane, filter, and dry in a vacuum drying oven at 60°C for 3.5 h to obtain a titanium source.

[0046] Example 6

[0047] Compared with Example 1, the only difference is:

[0048] Step 2: Add 20 g of lithium carbonate, 70 g of iron phosphate and 0.8 g of the titanium source obtained in step 1 into deionized water and mix them, then perform ball milling at a rotation speed of 300 r / min for 11 h, and then perform sand milling until the particle size is 250 nm to obtain a slurry.

[0049] Example 7

[0050] Compared with Example 1, the only difference is:

[0051] Step 2: Add 25 g of lithium carbonate, 80 g of iron phosphate and 1 g of the titanium source obtained in step 1 into deionized water and mix them, then perform ball milling at a rotation speed of 350 r / min for 10 h, and then perform sand milling until the particle size is 350 nm to obtain a slurry.

[0052] Example 8

[0053] Compared with Example 1, the only difference is:

[0054] Step 3: Place the slurry obtained in step 2 in an oven for drying at a temperature of 90° C. for 1 h.

[0055] Example 9

[0056] Compared with Example 1, the only difference is:

[0057] Step 4: Under a nitrogen atmosphere, the dried slurry in step 3 is placed in a tubular furnace for sintering at a sintering temperature of 780° C. for 11 hours, and then cooled to room temperature to obtain a lithium iron phosphate material.

[0058] Comparative Example 1

[0059] Compared with Example 1, the only difference is:

[0060] Replace valine with alanine in step 1, using the same amount.

[0061] Comparative Example 2

[0062] Compared with Example 1, the only difference is:

[0063] Replace valine with glutamic acid in step 1, using the same amount.

[0064] Comparative Example 3

[0065] Compared with Example 1, the only difference is:

[0066] Step 1. Under argon atmosphere, add 1.5 mmol of valine to 15 mL of benzene and stir, add 1 mmol of titanium tetrachloride, stir for 20 min, remove benzene under reduced pressure, add 8 mL of dichloromethane, continue stirring, evaporate and remove dichloromethane, filter, and dry in a vacuum drying oven at 60°C for 3.5 h to obtain a titanium source.

[0067] Comparative Example 4

[0068] Compared with Example 1, the only difference is:

[0069] Step 2: Add 5 g of lithium carbonate, 65 g of iron phosphate and 0.5 g of the titanium source obtained in step 1 into deionized water and mix them, then perform ball milling at a rotation speed of 300 r / min for 10 h, and then perform sand milling until the particle size is 250 nm to obtain a slurry.

[0070] Comparative Example 5

[0071] Compared with Example 1, the only difference is:

[0072] Step 2: Add 15 g of lithium carbonate, 50 g of iron phosphate and 0.5 g of the titanium source obtained in step 1 into deionized water and mix them, then perform ball milling at a rotation speed of 300 r / min for 10 h, and then perform sand milling until the particle size is 250 nm to obtain a slurry.

[0073] Comparative Example 6

[0074] Compared with Example 1, the only difference is:

[0075] Step 2: Add 15 g of lithium carbonate, 65 g of iron phosphate and 0.5 g of the titanium source obtained in step 1 into deionized water and mix them, then perform ball milling at a rotation speed of 300 r / min for 10 h, and then perform sand milling to a particle size of 500 nm to obtain a slurry.

[0076] Comparative Example 7

[0077] Compared with Example 1, the only difference is:

[0078] Step 3: Place the slurry obtained in step 2 in an oven for drying at a temperature of 70° C. for 1.5 h.

[0079] Comparative Example 8

[0080] Compared with Example 1, the only difference is:

[0081] Step 4: Under a nitrogen atmosphere, the dried slurry in step 3 is placed in a tubular furnace for sintering at a temperature of 600° C. for 12 h, and then cooled to room temperature to obtain a lithium iron phosphate material.

[0082] Comparative Example 9

[0083] This comparative example provides a method for preparing a lithium iron phosphate material, and the preparation steps are as follows:

[0084] Step 1, 15g of lithium carbonate, 65g of iron phosphate and 0.5g of titanium tetrachloride are added to deionized water and mixed, followed by ball milling, the rotation speed during the ball milling is 300r / min, the ball milling time is 10h, and then sand milling is performed to a particle size of 250nm to obtain a slurry;

[0085] Step 2: Place the slurry obtained in step 2 in an oven for drying at a temperature of 85°C for 1.5 hours;

[0086] Step 3: In a nitrogen atmosphere, the dried slurry in step 3 is placed in a tubular furnace for sintering at a temperature of 700° C. for 12 h, and then cooled to room temperature to obtain a lithium iron phosphate material.

[0087] The lithium iron phosphate material is prepared through the above steps.

[0088] Comparative Example 10

[0089] This comparative example provides a method for preparing a lithium iron phosphate material, and the preparation steps are as follows:

[0090] Step 1, 15g of lithium carbonate, 65g of iron phosphate and 0.5g of valine are added to deionized water and mixed, followed by ball milling, the rotation speed during the ball milling is 300r / min, the ball milling time is 10h, and then sand milling is performed to a particle size of 250nm to obtain a slurry;

[0091] Step 2: Place the slurry obtained in step 2 in an oven for drying at a temperature of 85°C for 1.5 hours;

[0092] Step 3: In a nitrogen atmosphere, the dried slurry in step 3 is placed in a tubular furnace for sintering at a temperature of 700° C. for 12 h, and then cooled to room temperature to obtain a lithium iron phosphate material.

[0093] The lithium iron phosphate material is prepared through the above steps.

[0094] Comparative Example 11

[0095] This comparative example provides a method for preparing a lithium iron phosphate material, and the preparation steps are as follows:

[0096] Step 1, 15g lithium carbonate, 65g iron phosphate, 0.3g titanium tetrachloride and 0.2g valine are added to deionized water and mixed, followed by ball milling, the rotation speed during the ball milling is 300r / min, the ball milling time is 10h, and then sand milling is performed to a particle size of 250nm to obtain a slurry;

[0097] Step 2: Place the slurry obtained in step 2 in an oven for drying at a temperature of 85°C for 1.5 hours;

[0098] Step 3: In a nitrogen atmosphere, the dried slurry in step 3 is placed in a tubular furnace for sintering at a temperature of 700° C. for 12 h, and then cooled to room temperature to obtain a lithium iron phosphate material.

[0099] The lithium iron phosphate material is prepared through the above steps.

[0100] Comparative Example 12

[0101] This comparative example provides a method for preparing a lithium iron phosphate material, and the preparation steps are as follows:

[0102] Step 1, 15g of lithium carbonate and 65g of iron phosphate are added to deionized water and mixed, followed by ball milling, the rotation speed during the ball milling is 300r / min, the ball milling time is 10h, and then sand milling is performed to a particle size of 250nm to obtain a slurry;

[0103] Step 2: Place the slurry obtained in step 2 in an oven for drying at a temperature of 85°C for 1.5 hours;

[0104] Step 3: In a nitrogen atmosphere, the dried slurry in step 3 is placed in a tubular furnace for sintering at a temperature of 700° C. for 12 h, and then cooled to room temperature to obtain a lithium iron phosphate material.

[0105] The lithium iron phosphate material is prepared through the above steps.

[0106] Application and performance tests were performed on Examples 1-9 and Comparative Examples 1-12:

[0107] The lithium iron phosphate obtained in the examples and comparative examples was used as the positive electrode material, wherein the weight ratio of lithium iron phosphate positive electrode material: acetylene black: polyvinylidene fluoride (PVDF) was 93:3:4, and a proper amount of N-methylpyrrolidone (NMP) solvent was added to form a slurry, and the slurry was coated on an aluminum foil after stirring. The coated aluminum foil was placed in a vacuum drying oven and dried at 110°C for 8 hours to obtain a positive electrode sheet, a metal lithium sheet was used as the counter electrode, and the electrolyte was 1 mol / L LiPF 6 / EC+DEC+DMC, where LiPF 6 The weight ratio of / EC:DEC:DMC is 1:1:1, and the polypropylene microporous membrane is used as the separator. The battery is assembled, the charge and discharge voltage is 2.0-3.75V, and the charge and discharge rate is 0.2C. The battery performance is tested. The test results are shown in Table 1:

[0108]

[0109] It can be seen from Table 1 that the preparation method of a lithium iron phosphate material provided in the present invention and the prepared lithium iron phosphate material have good electrochemical properties. It can be seen that the present invention has a good effect on improving the conductivity and ion diffusion mass transfer rate of lithium iron phosphate, and further expands the application field of lithium ion batteries.

[0110] It can be seen from Examples 1-9 and Comparative Examples 1-8 that the initial discharge capacity, discharge rate and capacity retention rate after 500 cycles in Comparative Examples 1-8 are all lower than those in Examples 1-9. This shows that the type of amino acid in the preparation process of the lithium iron phosphate material, the raw material ratio in the preparation process of the titanium source, the raw material ratio of the lithium iron phosphate material and the different parameters in the preparation process will all affect the electrochemical properties of lithium iron phosphate.

[0111] It can be seen from Example 1 and Comparative Examples 9 and 10 that the raw material of the lithium iron phosphate material in Comparative Example 9 is doped with only metallic titanium, and the raw material of the lithium iron phosphate material in Comparative Example 10 is added with only the carbon source valine, and the electrochemical properties of the resulting lithium iron phosphate materials are lower than those in Example 1. It can be seen that under the dual effects of carbon coating and titanium doping, the electronic conductivity and ionic conductivity of the lithium iron phosphate material are improved, and its lithium ion transmission rate, rate performance and capacity performance are significantly improved.

[0112] It can be seen from Example 1 and Comparative Example 11 that titanium tetrachloride and valine are directly used in Comparative Example 11, while amino acid titanium chelate is used for addition in the present invention. The electrochemical performance of Comparative Example 11 is lower than that of Example 1. It can be seen that compared with the use of titanium source and carbon source alone to improve the electron transfer rate, conductivity and other properties of lithium iron phosphate materials, the directly used amino acid titanium chelate has more significant improvements in electron transfer rate, conductivity and other aspects.

[0113] It should be noted that, in this article, relational terms such as first and second, etc. are only used to distinguish one entity or operation from another entity or operation, and do not necessarily require or imply any such actual relationship or order between these entities or operations. Moreover, the terms "include", "comprises" or any other variations thereof are intended to cover non-exclusive inclusion, so that a process, method, article or device including a series of elements includes not only those elements, but also other elements not explicitly listed, or also includes elements inherent to such process, method, article or device.

[0114] Although embodiments of the present invention have been shown and described, it will be appreciated by those skilled in the art that various changes, modifications, substitutions and variations may be made to the embodiments without departing from the principles and spirit of the present invention, and that the scope of the present invention is defined by the appended claims and their equivalents.

Claims

1. A method for preparing a lithium iron phosphate material, characterized in that: The following steps are involved: Step 1, under argon atmosphere, add amino acid to benzene and stir, add titanium tetrachloride, stir for 20-30 min, reduce pressure, add dichloromethane and continue stirring, evaporate, filter, and vacuum dry to obtain a titanium source; Step 2, adding lithium carbonate, iron phosphate and the titanium source into deionized water for mixing, and then grinding to obtain a slurry; Step 3, drying the slurry obtained in step 2; Step 4: Sintering the dried slurry in step 3 under a nitrogen atmosphere, and cooling to room temperature to obtain a lithium iron phosphate material; In step 1, the ratio of amino acid, benzene and titanium tetrachloride is 2-2.2 mmol:15 mL:1-1.1 mmol; The amino acid in step 1 is one of valine, leucine, methionine and proline.

2. The method for preparing a lithium iron phosphate material according to claim 1, characterized in that: The grinding method in step 2 is: ball milling and sand milling in sequence.

3. The method for preparing a lithium iron phosphate material according to claim 2, characterized in that: During the ball milling process, the rotation speed is 300-350r / min and the ball milling time is 10-12h.

4. The method for preparing a lithium iron phosphate material according to claim 2, characterized in that: In the sand milling process, the particles are sand milled to a particle size of 200-400 nm.

5. The method for preparing a lithium iron phosphate material according to claim 1, characterized in that: In step 2, the mass ratio of lithium carbonate: iron phosphate: titanium source is 10-30: 60-85: 0.5-1.

6. The method for preparing a lithium iron phosphate material according to claim 1, characterized in that: In step 3, the drying temperature is 80-90° C. and the drying time is 1-1.5 h; in step 4, the sintering temperature is 700-800° C. and the sintering time is 10-12 h.

7. A lithium iron phosphate material, characterized in that: Prepared by the preparation method according to any one of claims 1 to 6.

8. Use of the lithium iron phosphate material as claimed in claim 7 in a lithium ion battery.

Citation Information

Patent Citations

  • Preparation method of high-rate lithium iron phosphate positive electrode material

    CN113929070A

  • Preparation method of ultra-high-compaction lithium iron phosphate positive electrode material and lithium battery

    CN118373398A