Preparation and application of sodium vanadyl fluorophosphate composite microspheres constructed by one-dimensional carbon nanotubes and supported by three-dimensional network skeleton
By constructing a three-dimensional network skeleton of one-dimensional carbon nanotubes in the sodium vanadium fluorophosphate material, the problem of voltage drop of the material at high current density is solved, high rate and long cycle stability are achieved, and it is suitable for high-power sodium-ion batteries. .
Patent Information
- Application Number
- CN202410770903.1
- Authority / Receiving Office
- CN · China
- Patent Type
- Applications(China)
- Current Assignee / Owner
- Filing Date
- 2024-06-14
- Publication Date
- 2024-10-15
AI Technical Summary
Existing sodium vanadium fluorophosphate materials have a large ohmic voltage drop when discharged at high current densities, which limits the practical application of sodium-ion batteries. The electronic conductivity and cycle life need to be improved.
Sodium vanadium fluorophosphate composite microspheres are supported by a three-dimensional network skeleton constructed of one-dimensional carbon nanotubes. Through spray drying and high-temperature calcination technology, the electronic conductivity and cycle stability of the material are enhanced.
It achieves high rate performance and long cycle stability. The first discharge specific capacity reaches 110.7 mAh g-1 at 0.2 C. The capacity retention rate is 100% after 100 cycles and 80.3% at 50 C. It is suitable for high power and long-term use. Long-life sodium-ion battery applications.
Smart Images

Figure CN118771345A_ABST
Abstract
Description
Technical Field
[0001] The invention belongs to the technical field of nanomaterials and electrochemical technology, and specifically relates to a sodium vanadium fluorophosphate composite microsphere supported by a three-dimensional network skeleton constructed by one-dimensional carbon nanotubes and a preparation method thereof. The material can be used as a positive electrode active material for a fast-charging, long-life sodium ion battery. Background Art
[0002] As energy shortages and environmental pollution become increasingly serious, the development of clean and sustainable new energy sources has become an urgent problem to be solved. At present, lithium-ion batteries have been widely used in portable electronic devices such as mobile phones and notebooks due to their high energy density and long cycle life, and are regarded as the best choice for mobile power sources. However, the limited reserves and uneven distribution of lithium have restricted the development of large-scale energy storage.
[0003] Sodium-ion batteries have the advantages of abundant resources and low price. They are one of the most promising alternatives to lithium-ion batteries and are a very suitable choice for large-scale energy storage systems. The positive electrode material is one of the key factors that determine the electrochemical performance of sodium-ion batteries. Therefore, the development of high-performance positive electrode materials is of great significance for the further development of sodium-ion batteries.
[0004] The polyanionic compound sodium vanadyl fluorophosphate (Na3V2O2(PO4)2F, NVOPF) has a stable framework structure and high working potential (>3.9 V vs. Na + / Na) and a high theoretical specific capacity (130 mAh g -1 ) and other advantages, making it an ideal candidate for the positive electrode material of sodium-ion batteries. However, its relatively low intrinsic electronic conductivity causes a large ohmic voltage drop when the material is discharged at a high current density, resulting in poor capacity and cycle performance, and ultimately causing a loss in battery energy density, which greatly limits the practical application of the material.
[0005] In recent years, people have mainly used nano-sizing, carbon coating and doping technologies to modify the material, but the rate performance and cycle life still need to be improved. Increasing the contact area between carbon nanotubes and nanomaterials is the top priority for improving electronic conductivity and ion conductivity, and it is also a technical problem that needs to be solved urgently. Summary of the invention
[0006] The technical problem to be solved by the present invention is to propose a sodium vanadium fluorophosphate composite microsphere supported by a three-dimensional network skeleton constructed by one-dimensional carbon nanotubes and a preparation method thereof in response to the above-mentioned prior art. The process is simple, the output is high and the production cost is low; the prepared sodium vanadium fluorophosphate composite microsphere supported by the three-dimensional carbon nanotube network skeleton has high electronic conductivity and can obtain excellent electrochemical performance when used as a positive electrode material for a sodium ion battery.
[0007] A method for preparing sodium vanadium fluorophosphate composite microspheres supported by a three-dimensional network skeleton composed of one-dimensional carbon nanotubes. The composite microspheres are prepared by the following method: (1) dispersing sodium vanadyl fluorophosphate in water, adding hydroxylated multi-walled carbon nanotubes under continuous stirring, and ultrasonically dispersing in an ice-water bath to obtain solution A; (2) spray drying the solution A obtained in step (1) to obtain a spherical powder sample; (3) The spherical powder sample obtained in step (2) is subjected to high temperature calcination to obtain sodium vanadium fluorophosphate composite microspheres supported by a three-dimensional network skeleton composed of one-dimensional carbon nanotubes.
[0008] The sodium vanadyl fluorophosphate is a product obtained by mixing a solution formed by a vanadium source, a phosphorus source, a sodium source and a fluorine source and then subjecting the solution to a hydrothermal reaction.
[0009] The vanadium source is one or more of ammonium metavanadate, vanadyl sulfate, vanadium trichloride, vanadium acetylacetonate, vanadyl acetylacetonate, vanadium pentoxide, vanadium dioxide, vanadium trioxide, sodium metavanadate and sodium vanadate; the phosphorus source is one or more of phosphoric acid, ammonium dihydrogen phosphate, diammonium hydrogen phosphate, sodium dihydrogen phosphate, disodium hydrogen phosphate, sodium phosphate and ammonium phosphate; the sodium source is at least one of sodium oleate, sodium carbonate, sodium bicarbonate, sodium acetate, sodium dihydrogen phosphate and disodium hydrogen phosphate; the fluorine source is at least one of ammonium fluoride, sodium fluoride, hydrogen fluoride, magnesium fluoride or potassium fluoride.
[0010] The specifications of the hydroxylated multi-walled carbon nanotubes are: particle size 10-30 μm, and the added amount is 10-15% of the mass of sodium vanadium fluorophosphate. Too little addition of hydroxylated multi-walled carbon nanotubes, such as less than 10%, will affect the performance of the product.
[0011] In step (1), ultrasonic oscillation treatment is performed in an ice water bath for 3-5 h. The ultrasonic cavitation bubbles generated by the high-frequency ultrasonic wave in the ultrasonic field can generate local impact force when they explode, which helps to effectively disperse the multi-walled carbon nanotubes in agglomerated state, so that the excellent mechanical and electrical properties of a single carbon nanotube can be fully exposed. The use of an ice water bath during the ultrasonic process is to prevent the multi-walled carbon nanotubes from self-aggregating due to the high solution temperature, and to prevent uneven dispersion of the precursor solution that is finally subjected to spray treatment.
[0012] In some embodiments, the spraying conditions described in step (2) are as follows: the temperature in the drying chamber is 160-190°C, the air volume (Aspirator) is 85-95%, the injection rate (Pump) is 10-18%, and the number of nozzles is 1-2 times / min.
[0013] Further in some embodiments, the spray conditions used are that the temperature in the drying chamber is 170°C, the air intake (Aspirator) is 95%, the injection rate (Pump) is 15%, and the number of impact samples (Nozzle) is 2 times / min. The precursor solution can be gradually dried in the form of droplets through the spray drying technology. The precursor solution enters the needle through the peristaltic pump and enters the drying tower in the form of droplets. A certain amount of airflow is sprayed from the needle to break up the droplets into mist. The water in the droplets can be quickly evaporated in the drying tower. The remaining precursor powder is collected by the cyclone, and finally the dry powder is obtained in the collector.
[0014] The high temperature calcination system is: heating rate is 1-5℃ min ‒1 The calcination temperature is 400-600 ℃, the calcination time is 1-3 h; the calcination atmosphere is a hydrogen-argon mixture.
[0015] Another technical concept of the present invention is to use the sodium vanadyl fluorophosphate composite microspheres supported by the three-dimensional network skeleton constructed by the one-dimensional carbon nanotubes obtained by the above-mentioned preparation technology as the positive electrode active material of the sodium ion battery.
[0016] The present invention provides a spray drying-carbonization method suitable for mass production. By utilizing the high flexibility of carbon nanotubes, a sodium vanadium fluorophosphate composite microsphere supported by a three-dimensional network skeleton constructed by one-dimensional carbon nanotubes is designed for the first time, wherein sodium vanadium fluorophosphate nanoparticles are uniformly embedded between the three-dimensional conductive networks formed by cross-linking carbon nanotubes. The three-dimensional carbon nanotube conductive network can enhance the overall charge transport capacity of the material and effectively buffer the volume expansion caused by ion extraction / embedding during the charge and discharge process, thereby obtaining excellent high rate performance and long cycle stability.
[0017] The beneficial effects of the present invention are: based on the self-buffering mechanism, the spray drying technology is used to cleverly construct a three-dimensional carbon nanotube network skeleton with high flexibility and high conductivity, and the nano-sized sodium vanadium fluorophosphate is effectively dispersed. By high-temperature calcination, the sodium vanadium fluorophosphate composite microspheres supported by the three-dimensional carbon nanotube network skeleton are obtained. When the present invention is used as a positive electrode active material for sodium ion batteries, the composite microspheres exhibit excellent cycle stability and high rate characteristics, and are potential application materials for high-power, long-life sodium ion batteries. As a positive electrode active material for sodium ion batteries, at a current density of 0.2 C, the first discharge specific capacity is 110.7 mAh g ‒1 The capacity retention rate is 100% after 100 cycles; at a high current density of 50 C, the first discharge specific capacity can reach 87.7 mAh g ‒1, the capacity retention rate after 9000 cycles is 80.3%. The process of the present invention is simple, the spray drying-carbonization method adopted is universal, the equipment requirements are low, the prepared material has high purity and good dispersibility, and it is easy to mass-produce on a large scale, which is very conducive to market promotion. BRIEF DESCRIPTION OF THE DRAWINGS
[0018] Figure 1 This is a scanning electron microscope image of the composite of one-dimensional carbon nanotubes and sodium vanadyl fluorophosphate according to Example 1 of the present invention.
[0019] Figure 2 This is the XRD diagram of the sodium vanadium oxyfluorophosphate composite microspheres supported by the three-dimensional network skeleton constructed by one-dimensional carbon nanotubes in Example 2 of the present invention.
[0020] Figure 3 This is a scanning electron microscope image of the sodium vanadium oxyfluorophosphate composite microsphere supported by the three-dimensional network skeleton constructed by one-dimensional carbon nanotubes according to Example 2 of the present invention.
[0021] Figure 4 This is a transmission electron microscope image of the sodium oxyvanadium fluorophosphate composite microsphere supported by the three-dimensional network skeleton constructed by one-dimensional carbon nanotubes according to Example 2 of the present invention.
[0022] Figure 5 This is a battery cycle performance diagram of sodium vanadium fluorophosphate composite microspheres supported by a three-dimensional network skeleton constructed by one-dimensional carbon nanotubes in Example 2 of the present invention at a current density of 0.2 C.
[0023] Figure 6 This is a battery cycle performance diagram of sodium vanadium fluorophosphate composite microspheres supported by a three-dimensional network skeleton constructed by one-dimensional carbon nanotubes in Example 2 of the present invention at a current density of 50 C.
[0024] Figure 7 This is a scanning electron microscope image of the electrode sheet of the sodium oxyvanadium fluorophosphate composite microsphere supported by the three-dimensional network skeleton constructed by one-dimensional carbon nanotubes in Example 2 of the present invention before and after cycling 9000 times at a current density of 50°C. DETAILED DESCRIPTION
[0025] In order to better understand the present invention, the content of the present invention is further explained below in conjunction with the embodiments, but the content of the present invention is not limited to the following embodiments.
[0026] The preparation of sodium vanadyl fluorophosphate comprises the following steps: 1) Weigh 0.5303 g of vanadyl acetylacetonate and add it to 40 mL of anhydrous ethanol, stirring until it is completely dissolved; slowly add a certain amount of phosphoric acid and stir for 30 min to obtain a brown solution; 2) Weigh a certain amount of polyethylene glycol and add it to 30 mL of water. Stir for a certain period of time until it is completely dissolved. Slowly add 0.91332 g of sodium oleate and stir to obtain a colorless and transparent solution. 3) The solution of step 2) and the solution of step 1) were mixed and stirred for 3 h to obtain a uniform dark green solution; 4) Slowly add 10 mL of the 3.707 g L ‒1 The ammonium fluoride solution is stirred for a certain period of time to obtain a grass green transparent solution; 5) Transfer the solution from step 4) to a 100 mL reactor and hydroheat at 180 °C for 24 h; 6) After the reaction in step 5), the reactor was cooled to room temperature, the supernatant was poured out, the green precipitate at the bottom was taken out, and it was washed alternately with water and anhydrous ethanol for 6 times. The centrifuged product was dried in a vacuum oven at 60°C for 24 hours to obtain the sodium vanadium fluorophosphate nanoplate sample used in the present invention. The applicant believes that the sodium vanadium fluorophosphate nanoparticles prepared by other methods can also achieve the following technical solutions of the present invention.
[0027] Example 1 A method for preparing sodium vanadyl fluorophosphate composite microspheres supported by a three-dimensional network skeleton constructed by one-dimensional carbon nanotubes comprises the following steps: (1) Disperse a certain amount of sodium vanadyl fluorophosphate in deionized water to prepare 1.28 mmol L ‒1 After the dispersion is completely dispersed, 15% hydroxylated multi-walled carbon nanotubes by weight of sodium fluorovanadium phosphate are slowly added under continuous stirring, and stirred for 30 min, and then transferred to an ultrasonic machine and ultrasonicated in a water bath at room temperature for 30 min; (2) The solution obtained in step (1) was transferred to a spray drying device, and a precursor powder sample was obtained through processes such as droplet refinement, water evaporation and cyclone recovery. The spray drying panel parameters were set as follows: the temperature in the drying chamber was 170 °C, the air inlet volume (Aspirator) was 95%, the injection rate (Pump) was 15%, and the number of nozzles (Nozzle) was 2 times / min.
[0028] (3) The precursor powder sample obtained in step (2) is placed in a tube furnace and calcined at a high temperature to obtain a composite material of sodium vanadium fluorophosphate and carbon nanotubes; the heating rate is 2 °C min ‒1 The calcination temperature is 450 ℃ and the calcination time is 3 h; the calcination atmosphere is a hydrogen-argon mixture.
[0029] The scanning electron microscopy (SEM) results of the sodium vanadium fluorophosphate composite microspheres supported by the three-dimensional network skeleton constructed by one-dimensional carbon nanotubes prepared in this example are as follows: Figure 1As shown, due to the short ultrasonic dispersion treatment time and the water temperature being overheated due to the mechanical energy converted into heat energy by the machine vibration during the ultrasonic process, the carbon nanotubes self-aggregated and failed to obtain a precursor solution in which the carbon nanotubes and sodium vanadyl fluorophosphate were evenly dispersed. As a result, the multi-walled carbon nanotubes and sodium vanadyl fluorophosphate nanoparticles in the powder sample obtained after spray drying tended to self-aggregate, and the sodium vanadyl fluorophosphate composite microspheres supported by a three-dimensional network skeleton constructed by uniform one-dimensional carbon nanotubes could not be obtained.
[0030] The sodium vanadium fluorophosphate composite microspheres supported by a three-dimensional network skeleton constructed by one-dimensional carbon nanotubes prepared by the present invention are used as the positive electrode active material of the sodium ion battery. The remaining steps of the assembly method of the sodium ion battery are the same as the usual assembly method. The preparation method of the positive electrode sheet is as follows: sodium vanadium fluorophosphate composite microspheres supported by a three-dimensional network skeleton constructed by one-dimensional carbon nanotubes are used as the active material, acetylene black is used as the conductive agent, and polyvinylidene fluoride is used as the binder. The mass ratio of the active material, acetylene black, and polyvinylidene fluoride is 70:20:10; the active material and acetylene black are weighed in proportion and ground for 30 minutes, and then polyvinylidene fluoride and a small amount of N-methylpyrrolidone in a corresponding proportion are added, ground into a uniform slurry, and then scraped on an aluminum foil; after drying, a positive electrode sheet with a diameter of 1 cm is engraved with a hole punching machine, and placed in an oven at 70°C for further drying for 12 hours before use. A button-type sodium-ion battery was assembled with 1M NaClO4 dissolved in propylene carbonate (PC) and 5% fluoroethylene carbonate (FEC) as the electrolyte, metallic sodium as the negative electrode, a glass fiber membrane as the separator, and a CR2016 stainless steel battery casing for electrochemical performance testing.
[0031] Taking the sodium vanadium fluorophosphate composite microspheres supported by the three-dimensional network skeleton constructed by one-dimensional carbon nanotubes prepared in this embodiment as the positive electrode active material of the sodium ion battery as an example, at a current density of 0.2 C, the initial capacity can reach 102.9 mAh g ‒1 After 100 cycles, the capacity remains at 102.6 mAh g ‒1 The capacity retention rate is 99.7%. At a high current density of 50 C, the first discharge capacity can reach 65.5 mAh g ‒1 After 9000 cycles, the capacity can still reach 40.8 mAh g ‒1 , the capacity retention rate is 62.3%.
[0032] Example 2 A method for preparing sodium vanadium fluorophosphate composite microspheres supported by a three-dimensional network skeleton constructed by one-dimensional carbon nanotubes: (1) Disperse a certain amount of sodium vanadyl fluorophosphate in deionized water to prepare 1.28 mmol L ‒1After the dispersion is completely dispersed, 15% hydroxylated multi-walled carbon nanotubes by weight of sodium fluorovanadium phosphate are slowly added under continuous stirring, stirred for 30 min, and then transferred to an ultrasonic machine and ultrasonicated in an ice water bath for 3 h; (2) The solution obtained in step (1) was transferred to a spray drying device, and a spherical precursor powder sample was obtained through processes such as droplet refinement, water evaporation and cyclone recovery. The spray drying panel parameters were set as follows: the temperature in the drying chamber was 170 °C, the air inlet volume (Aspirator) was 95%, the injection rate (Pump) was 15%, and the number of nozzles (Nozzle) was 3 times / min.
[0033] (3) The precursor powder sample obtained in step (2) is placed in a tube furnace and calcined at high temperature to obtain sodium vanadium fluorophosphate composite microspheres supported by a three-dimensional network skeleton composed of one-dimensional carbon nanotubes; the heating rate is 2 °C min ‒1 The calcination temperature is 450 ℃ and the calcination time is 3 h; the calcination atmosphere is a hydrogen-argon mixture.
[0034] Taking the sodium vanadium oxyfluorophosphate composite microspheres supported by a three-dimensional network skeleton constructed by one-dimensional carbon nanotubes as an example, its structure was determined by an X-ray diffractometer. Figure 2 As shown, the X-ray diffraction pattern (XRD) shows that the sodium vanadium fluorophosphate composite microspheres supported by the three-dimensional network skeleton constructed by the one-dimensional carbon nanotubes are Na3V2O2(PO4)2F phase (PDF card number is 04-011-1042), the space group is I4 / mmm, and there is no other impurity phase. Figure 3 As shown in the figure, the results of scanning electron microscopy (SEM) show that the structure of the composite microsphere is composed of a carbon nanotube conductive network interwoven with sodium vanadium fluorophosphate nanoparticles. The diameter of the composite microsphere is 0.8-1.8 microns, and the size of the nanoparticles is 150-300 nanometers. Figure 4 As shown, transmission electron microscopy (TEM) and high-resolution transmission electron microscopy (HRTEM) tests indicate that the composite microsphere has a good crystal structure, and the nanoparticles are uniformly wrapped in a three-dimensional conductive network structure constructed by one-dimensional carbon nanotubes.
[0035] Taking the sodium vanadium fluorophosphate composite microspheres supported by the three-dimensional network skeleton constructed by the one-dimensional carbon nanotubes prepared in this embodiment as the positive electrode active material of the sodium ion battery as an example, Figure 5 As shown in Figure 2, at a current density of 0.2 C, the first discharge capacity can reach 110.7 mAh g ‒1 After 100 cycles, the capacity remains at 110 mAh g ‒1 The capacity retention rate is 100%. Figure 6 As shown in Figure 2, at a high current density of 50 C, the first discharge capacity can reach 87.7 mAh g‒1 After 9000 cycles, the capacity can still reach 70.4 mAh g ‒1 , the capacity retention rate is 80.3%. Figure 7 The scanning electron microscope (SEM) results of the initial electrode sheet and the electrode sheet after 9000 cycles at a high current density of 50 C show that after 9000 high current cycles, the NVOPF-CNTs microsphere composite with regular morphology can still be clearly observed in the electrode sheet. This result shows that the three-dimensional network skeleton constructed by one-dimensional carbon nanotubes exhibits a good self-buffering effect, which can effectively alleviate the structural stress caused by sodium ion deintercalation during high current charging and discharging, and help the composite microsphere material to obtain excellent long-cycle stability and high-rate characteristics.
[0036] Example 3 A method for preparing sodium vanadyl fluorophosphate composite microspheres supported by a three-dimensional network skeleton constructed by one-dimensional carbon nanotubes comprises the following steps: (1) Disperse a certain amount of sodium vanadyl fluorophosphate in deionized water to prepare 1.28 mmol L ‒1 After the dispersion is completely dispersed, 10% hydroxylated multi-walled carbon nanotubes by weight of sodium fluorovanadium phosphate are slowly added under continuous stirring, and stirred for 30 min. Then, the mixture is transferred to an ultrasonic machine and ultrasonicated in an ice water bath for 3 h. (2) The solution obtained in step (1) was transferred to a spray drying device, and a spherical precursor powder sample was obtained through processes such as droplet refinement, water evaporation and cyclone recovery. The spray drying panel parameters were set as follows: the temperature in the drying chamber was 170 °C, the air inlet volume (Aspirator) was 95%, the injection rate (Pump) was 15%, and the number of impact samples (Nozzle) was 2 times / min.
[0037] (3) The precursor powder sample obtained in step (2) is placed in a tube furnace and calcined at a high temperature to obtain a composite material of sodium vanadium fluorophosphate and carbon nanotubes; the heating rate is 2 °C min ‒1 The calcination temperature is 450 ℃ and the calcination time is 3 h; the calcination atmosphere is a hydrogen-argon mixture.
[0038] Taking the sodium vanadium fluorophosphate composite microspheres supported by the three-dimensional network skeleton constructed by one-dimensional carbon nanotubes prepared in this example as the positive electrode active material of sodium ion battery, the first discharge specific capacity can reach 107.5 mAh g at a current density of 0.2 C. ‒1 After 100 cycles, the remaining capacity is 104.9 mAh g ‒1 The capacity retention rate is 97.6%. At a high current density of 50 C, the first discharge capacity can reach 67.7 mAh g ‒1After 9000 cycles, the capacity can still reach 46.5 mAh g ‒1 , the capacity retention rate is 68.7%.
[0039] Example 4 The preparation method of sodium vanadyl fluorophosphate microspheres comprises the following steps: (1) Disperse a certain amount of sodium vanadyl fluorophosphate in deionized water to prepare 1.28 mmol L ‒1 The dispersion was stirred for 30 min to make it completely dispersed.
[0040] (2) The solution obtained in step (1) was transferred to a spray drying device, and a spherical precursor powder sample was obtained through processes such as droplet refinement, water evaporation and cyclone recovery. The spray drying panel parameters were set as follows: the temperature in the drying chamber was 170 °C, the air inlet volume (Aspirator) was 95%, the injection rate (Pump) was 15%, and the number of impact samples (Nozzle) was 2 times / min.
[0041] (3) Collect the powder sample obtained in step (2) to obtain a sodium vanadyl fluorophosphate microsphere sample. Taking the sodium vanadyl fluorophosphate composite microspheres prepared in this example as the positive electrode active material of the sodium ion battery as an example, at a current density of 0.2 C, the initial capacity can reach 74.9 mAh g ‒1 After 100 cycles, the remaining capacity is 37.21 mAh g ‒1 , the capacity retention rate is 49.7%.
Claims
1. A method for preparing composite microspheres of sodium vanadyl fluorophosphate supported by a three-dimensional network skeleton composed of one-dimensional carbon nanotubes. It is characterized in that The composite microsphere is prepared by the following method: (1) dispersing sodium vanadyl fluorophosphate in water, adding hydroxylated multi-walled carbon nanotubes under continuous stirring, and ultrasonically dispersing in an ice-water bath to obtain solution A; (2) spray drying the solution A obtained in step (1) to obtain a spherical powder sample; (3) The spherical powder sample obtained in step (2) is subjected to high temperature calcination to obtain sodium vanadyl fluorophosphate composite microspheres supported by a three-dimensional network skeleton composed of one-dimensional carbon nanotubes.
2. The method for preparing the composite microspheres of sodium vanadyl fluorophosphate supported by a three-dimensional network skeleton composed of one-dimensional carbon nanotubes according to claim 1, It is characterized in that The sodium vanadyl fluorophosphate is a product obtained by mixing a solution formed by a vanadium source, a phosphorus source, a sodium source and a fluorine source and then subjecting the solution to a hydrothermal reaction.
3. The method for preparing the composite microspheres of sodium vanadyl fluorophosphate supported by a three-dimensional network skeleton composed of one-dimensional carbon nanotubes according to claim 2, It is characterized in that The vanadium source is one or more of ammonium metavanadate, vanadyl sulfate, vanadium trichloride, vanadium acetylacetonate, vanadyl acetylacetonate, vanadium pentoxide, vanadium dioxide, vanadium trioxide, sodium metavanadate and sodium vanadate; the phosphorus source is one or more of phosphoric acid, ammonium dihydrogen phosphate, diammonium hydrogen phosphate, sodium dihydrogen phosphate, disodium hydrogen phosphate, sodium phosphate and ammonium phosphate; the sodium source is at least one of sodium oleate, sodium carbonate, sodium bicarbonate, sodium acetate, sodium dihydrogen phosphate and disodium hydrogen phosphate; the fluorine source is at least one of ammonium fluoride, sodium fluoride, hydrogen fluoride, magnesium fluoride or potassium fluoride.
4. The method for preparing the composite microspheres of sodium vanadyl fluorophosphate supported by a three-dimensional network skeleton composed of one-dimensional carbon nanotubes according to claim 1, It is characterized in that The specifications of the hydroxylated multi-walled carbon nanotubes are: particle size 10-30 μm, and the added amount is 10-15% of the mass of sodium vanadyl fluorophosphate.
5. The method for preparing the composite microspheres of sodium vanadyl fluorophosphate supported by a three-dimensional network skeleton composed of one-dimensional carbon nanotubes according to claim 1, It is characterized in that In step (1), ultrasonic dispersion is performed in an ice-water bath for 3-5 h.
6. The method for preparing the composite microspheres of sodium vanadyl fluorophosphate supported by a three-dimensional network skeleton composed of one-dimensional carbon nanotubes according to claim 1, It is characterized in that The spraying conditions described in step (2) are as follows: the temperature in the drying chamber is 160-190°C, the air volume (Aspirator) is 85-95%, the injection rate (Pump) is 10-18%, and the number of impact samples (Nozzle) is 1-2 times / min.
7. The method for preparing composite microspheres of sodium vanadyl fluorophosphate supported by a three-dimensional network skeleton composed of one-dimensional carbon nanotubes according to claim 6, It is characterized in that The spray conditions described in step (2) are as follows: the temperature in the drying chamber is 170°C, the air volume (Aspirator) is 95%, the injection rate (Pump) is 15%, and the number of nozzles is 2 times / min.
8. The method for preparing the composite microspheres of sodium vanadyl fluorophosphate supported by a three-dimensional network skeleton composed of one-dimensional carbon nanotubes according to claim 1, It is characterized in that High temperature calcination system: heating rate is 1-5 ℃ min ‒1 The calcination temperature is 400-600℃, the calcination time is 1-3 h, and the calcination atmosphere is a hydrogen-argon mixture.
9. Use of sodium vanadyl fluorophosphate composite microspheres supported by a three-dimensional network skeleton constructed by one-dimensional carbon nanotubes prepared by the preparation method according to any one of claims 1 to 8 as positive electrode active materials for sodium ion batteries.
Citation Information
Patent Citations
Method for controllably preparing vanadium sodium fluorophosphate positive electrode material
CN108682855A
Porous single-crystal sodium vanadyl fluorophosphate positive electrode material as well as preparation method and application thereof
CN115084474A
Sodium ion positive electrode material, preparation method thereof and sodium ion battery
CN115275187A
Cathode active material of calcium ion battery as well as preparation method and application of cathode active material
CN115939405A
Surface-doped and coated sodium ion battery positive electrode material as well as preparation and application thereof
CN118173732A
Cited By
Electrode material, positive electrode film and preparation method and application thereof
CN120914236A