Method for preparing 4N quartz through efficient separation of high-silicon iron ore waste

By optimizing process parameters through desliming-magnetic separation, atmospheric leaching, high-temperature hot-press leaching and heat treatment steps, the problems of low utilization rate and environmental pollution of traditional high-silica iron ore waste have been solved, and efficient iron recovery and preparation of 4N high-silicon iron ore have been achieved. Pure quartz, significantly improving the purity and resource utilization of quartz.

CN118771397AActive Publication Date: 2024-10-15CENT SOUTH UNIV
View PDF 8 Cites 0 Cited by

Patent Information

Application Number
CN202411005541.3
Authority / Receiving Office
CN · China
Patent Type
Applications(China)
Current Assignee / Owner
Filing Date
2024-07-25
Publication Date
2024-10-15
Estimated Expiration
2044-07-25

AI Technical Summary

Technical Problem

Traditional high-silicon iron ore waste utilization methods have problems such as low utilization rate, environmental pollution, high energy consumption and insufficient purity. It is difficult to efficiently recover iron and prepare high-purity silica.

Method used

Using desliming-magnetic separation, atmospheric pressure leaching, high-temperature hot-press leaching and heat treatment steps, through multi-stage magnetic separation, ternary mixed acid pickling and heat treatment, process parameters are optimized to improve the separation efficiency of iron and silicon to prepare 4N high-purity quartz , and reduce environmental impact by recycling acid and water.

Benefits of technology

It achieves efficient resource utilization, improves the recovery efficiency of iron and silicon, significantly improves the purity of quartz, reduces impurity content and environmental pollution, and is simple, efficient, environmentally friendly, and low-cost.

✦ Generated by Eureka AI based on patent content.

Smart Images

  • Figure CN118771397A_ABST
    Figure CN118771397A_ABST
Patent Text Reader

Abstract

The invention provides a novel method for preparing 4N quartz through efficient separation of high-silicon iron ore waste. According to the method, an innovative multi-stage strong magnetic separation and two-stage ternary pickling process is adopted, so that the grade of the iron ore concentrate is improved to 60%, and meanwhile, 99.99% high-purity quartz is prepared. Compared with the prior art, the method has the advantages that the technological process is optimized, the environmental pollution and the operation cost are remarkably reduced, the utilization efficiency of useful components in the high-silicon iron ore waste is improved, and the challenge of shortage of high-quality quartz resources is effectively handled. Particularly in a sulfuric acid-phosphoric acid-hydrofluoric acid ternary pickling link, the technology shows remarkable advantages in the aspects of purification effect, environmental protection performance and cost control, and a more environment-friendly and economic solution is provided for resource utilization of the high-silicon iron ore waste.
Need to check novelty before this filing date? Find Prior Art

Description

Technical Field

[0001] The invention belongs to the field of secondary utilization of mineral resources and relates to a method for efficiently separating and preparing 4N quartz by utilizing high-silicon iron ore waste. Background Art

[0002] High silicon iron ore waste is a by-product produced in the process of iron ore refining, and its main components are quartz, silicate minerals and hematite. High silicon iron ore waste is rich in silicon and has certain economic value. However, traditional utilization methods have problems such as low utilization rate and environmental pollution. Therefore, it is of great significance to develop a new resource utilization method for high silicon iron ore waste. In modern industrial production, steel is widely used in casting, construction, aerospace and other fields as an important material. In the production process from iron ore to steel, a large amount of tailings will be produced. These tailings have high silicon content and low iron content, and have potential application value. However, traditional utilization methods have problems such as low utilization rate and environmental pollution. Although traditional methods such as magnetization roasting, acid leaching, alkali leaching, and hydrothermal method have achieved iron recovery and silicon extraction to some extent, these methods usually face problems such as high energy consumption, large environmental pollution, large equipment investment, and insufficient purity.

[0003] Therefore, it is of great practical significance to develop a method for efficiently recovering iron and preparing high-purity silica for the special resource of high-silicon iron ore waste. Summary of the invention

[0004] In view of the above problems existing in the prior art, the purpose of the present invention is to provide a method for efficiently separating and preparing 4N quartz using high-silicon iron ore waste. The method can efficiently realize the resource utilization of high-silicon iron ore waste. It can not only realize the recovery of iron in the high-silicon iron ore waste to obtain high-quality iron concentrate, but also can separate and recover silicon concentrate. The silicon concentrate can be used as a raw material to prepare 4N high-purity quartz, and the acid generated in the entire pickling process can be recycled.

[0005] In order to achieve the above object, the present invention provides a method for preparing 4N quartz by efficiently separating high-silicon iron ore waste, which improves the resource utilization rate of high-silicon iron ore waste and increases the added value of products.

[0006] The present invention discloses a method for efficiently separating and preparing 4N quartz by using high-silicon iron ore waste, comprising the following steps:

[0007] (1) Desliming-magnetic separation: The high-silicon iron ore waste is first deslimed and then subjected to multi-stage magnetic separation. The first stage of strong magnetic separation is 1.8-2.1T. After magnetic separation, the first iron concentrate and silicon concentrate are obtained. The first iron concentrate is then subjected to the second stage of magnetic separation. The magnetic field strength is 1.5-1.6T to obtain the second iron concentrate.

[0008] (2) Normal pressure leaching: ball-milling the silicon concentrate obtained in step (1) to a predetermined fineness, performing normal pressure leaching using a ternary mixed acid, washing the leached product to neutrality, and drying to obtain a first high-purity quartz;

[0009] (3) High-temperature hot-pressing leaching: ball-milling the first high-purity quartz to a set fineness, and performing high-temperature hot-pressing leaching on the ball-milled first high-purity quartz using a ternary mixed acid to obtain an acid-washed product;

[0010] (4) Heat treatment: The acid-washed product obtained in step (3) is washed to neutrality, dried and then heat-treated to obtain the second high-purity quartz, i.e., the 4N quartz product;

[0011] The ternary mixed acid is a mixed acid of sulfuric acid, phosphoric acid and hydrofluoric acid, and the volume ratio is 1-3:1-3:1.

[0012] In a preferred embodiment, in step (1), a wet high intensity magnetic separator or a high gradient magnetic separator is used for magnetic separation.

[0013] In a preferred embodiment, in step (1), the magnetic field strength of the first stage of high-intensity magnetic separation is 1.8 to 2.1 T, and the pulp ratio is 1:5 to 10. This process optimizes the separation efficiency of iron and silicon, reduces the silicon content in the iron concentrate, and provides a purer silicon source for the subsequent preparation of high-purity SiO2.

[0014] In a preferred solution, in step (1), the magnetic field strength of the second magnetic separation is 1.2 to 1.6 T, and the pulp ratio is 1:5 to 10. The magnetic separation stage of the present invention is different in that no flotation treatment is required, and the iron concentrate obtained after magnetic separation has a high grade.

[0015] Further preferably, the second stage magnetic separation is to perform one or more magnetic separations on the first iron concentrate.

[0016] In a preferred embodiment, in step (2), the atmospheric pressure leaching process is specifically as follows: the acid concentration is 9-10 mol / L, the atmospheric pressure leaching time is 5-6 h, the reaction temperature is 90-100° C., and the liquid-to-solid ratio is 4-5:1 (mL:g).

[0017] In a preferred embodiment, in step (2), the drying temperature is 100-105° C. and the drying time is 3-8 h. After initial purification, the first high-purity quartz is obtained, and the total impurities are 500-900 mg / kg, i.e., a 3N-3N5 high-purity quartz product.

[0018] In a preferred embodiment, in steps (2) and (3), during the ball milling process, zirconium balls are used as the grinding medium and a nylon screen is used as the sieve.

[0019] In a preferred embodiment, in step (3), the high temperature hot acid leaching process is specifically as follows: the acid concentration is 9-10 mol / L, the leaching time is 5-8 hours, the reaction temperature is 180-200°C, and the liquid-solid ratio is 4-5:1 (mL:g). Through the hot acid leaching treatment, this purification process significantly improves the purity of SiO2 and reduces the impurity content.

[0020] In a preferred embodiment, in step (3), the pickling equipment used for high-temperature hot-pressure leaching is a reactor, and the reactor used can withstand high temperature and high pressure conditions to ensure leaching efficiency and safety.

[0021] In a preferred embodiment, in step (4), the drying temperature is 100 to 105° C. and the drying time is 3 to 8 hours.

[0022] In a preferred solution, in step (4), the heat treatment process is specifically: high temperature treatment at 900-1000°C in a tube furnace for 3-5 hours. After primary purification-repurification-heat treatment, the second high-purity quartz is obtained, and the total impurities can be reduced to below 100 mg / kg, that is, a 4N high-purity quartz product.

[0023] In the preferred solution, after the waste liquid is treated by evaporation and crystallization, sulfuric acid and hydrofluoric acid are recovered for recycling, which significantly reduces chemical consumption and environmental impact, meets environmental protection requirements, and improves the economy and sustainability of the entire process.

[0024] The preferred solution is to use ultrapure water to wash multiple times after pickling, and the material of the washing equipment is all polytetrafluoro material, and glass material cannot be used.

[0025] The present invention adopts a mixed acid of sulfuric acid, phosphoric acid and hydrofluoric acid. Sulfuric acid has strong acidity and can effectively dissolve metal impurities such as iron, aluminum, calcium and the like in quartz, promote the dissolution of impurities, and thus improve the purity of quartz. Hydrofluoric acid is the only acid that can effectively dissolve silicates, and can efficiently dissolve silicate minerals in quartz and reduce their content; the presence of hydrofluoric acid can significantly improve the leaching efficiency of the pickling process, and can effectively open inclusions, release impurities for leaching, and ensure that the silicon content in quartz meets high purity requirements. Phosphoric acid can form a stable complex with certain metal ions, such as W, to prevent impurities from reprecipitating during the pickling process; phosphoric acid can cooperate with the effects of sulfuric acid and hydrofluoric acid in the mixed acid, improve the pickling effect, and further improve the purity of quartz.

[0026] The innovative features of the present invention are as follows:

[0027] The free SiO2 content of high-silicon iron ore waste is 65-78%, the iron content is 8-15%, and the -200 mesh content is 10-24%. This precise raw material selection standard is based on a large amount of experimental and practical data, and is more conducive to the subsequent high-purity SiO2 preparation compared with existing technologies.

[0028] The first stage of strong magnetic separation obtains the first iron concentrate and silicon concentrate. The grade of the first iron concentrate is above 40-45%, and the SiO2 content of the silicon concentrate is above 90-95%. This process optimizes the separation efficiency of iron and silicon, reduces the silicon content in the iron concentrate, and provides a purer silicon source for the subsequent preparation of high-purity SiO2. The first iron concentrate is magnetically separated with a magnetic field strength of 1.2-1.6T and a pulp ratio of 1:5-10 to obtain a second iron concentrate with an iron grade of 57-60% or more.

[0029] In the desludging-multi-stage strong magnetic separation process, the present invention achieves more efficient separation of iron and silicon by precisely controlling the parameters of the multi-stage strong magnetic separation. Compared with the prior art, the present invention uses a wet strong magnetic separator or a high gradient magnetic separator, and sets the magnetic separation intensity at 1.2T to 2.1T. This improvement significantly improves the grade of iron concentrate and silicon concentrate, and provides a purer silicon source for the subsequent preparation of high-purity SiO2.

[0030] The two-stage pickling process (primary purification and re-purification) adopted by the present invention shows significant advantages in purification effect, environmental performance and cost control. By carefully controlling the pickling conditions (such as total acid concentration, leaching time, reaction temperature and liquid-solid ratio), compared with the prior art, the method of the present invention not only achieves higher purity SiO2, but also significantly reduces environmental pollution.

[0031] The heat treatment process of the present invention includes drying in a vacuum drying oven and high temperature treatment in a tube furnace. By precisely controlling the temperature and time, the present invention not only removes the gas-liquid inclusions and lattice impurities in the silicon concentrate, but also ensures the structural stability and high purity of the SiO2 product, which is difficult to achieve with other patented technologies.

[0032] Compared with the prior art, the beneficial technical effects of the present invention are:

[0033] The method proposed in the present invention not only improves the recovery efficiency of iron and silicon by optimizing process parameters and processing procedures, but also realizes the preparation of 4N high-purity silicon dioxide, solves the problems existing in traditional methods, and has the characteristics of simplicity, high efficiency, environmental protection, and low cost.

[0034] The present invention achieves a more efficient separation and purification process by optimizing process parameters and processing procedures. For example, the present invention uses a wet high-intensity magnetic separator or a high-gradient magnetic separator, and the multi-stage magnetic separation intensity is 1.2T to 2.1T, eliminating the flotation process, thereby improving the grade of the iron ore concentrate. During the pickling process, the present invention accurately controls the parameters of the pickling equipment and the ratio of the ternary mixed acid to maximize the removal rate of impurities. In addition, after the waste liquid is evaporated and crystallized, sulfuric acid and hydrofluoric acid can be recycled, which significantly reduces chemical consumption and environmental impact, and improves the economy and sustainability of the entire process.

[0035] These innovative process parameters and process flow improvements have enabled the product purity of the present invention to reach a level that other patents cannot reach, ensuring the production of high-purity SiO2 products. Compared with inventions CN 108636591 B and CN116159666A, the purity of quartz has increased by 2 grades, and the iron concentrate has also reached 60% iron grade. BRIEF DESCRIPTION OF THE DRAWINGS

[0036] Figure 1 is a process flow chart of the present invention;

[0037] Figure 2 This is the XRD diagram of iron concentrate 1 in Example 1. DETAILED DESCRIPTION

[0038] In order to better explain the present invention, the present invention is described in detail below through specific implementation modes in conjunction with the accompanying drawings, but the following embodiments do not limit the protection scope of the claims.

[0039] The components of high-silicon iron ore waste are: free SiO2 content is 65-78%, iron grade is 8-15%, and -200 mesh content accounts for 10-24%.

[0040] Unless otherwise specified, the chemical reagents used in the following examples are all commercial reagents.

[0041] Example 1

[0042] A method for efficiently separating and preparing 4N quartz by using high-silicon iron ore waste comprises the following steps:

[0043] (1) Desliming-magnetic separation: 100g of high-silicon iron ore waste (less mud, SiO2 content of 78%, iron grade of 8-10%) was mixed with 500ml of water, and a silicon concentrate 1 with a grade of 95.45% and an iron concentrate 1 with a grade of 58.8% were obtained under the condition of a 1.8T wet high-intensity magnetic separator. 100g of iron concentrate 1 was mixed with 500g of water, and an iron concentrate 2 with an iron grade of 61.56% was obtained under the condition of a 1.5T wet high-intensity magnetic separator.

[0044] (2) Normal pressure leaching: The silicon concentrate 1 is ball milled with a planetary ball mill. The ball mill jar and the ball mill medium are made of 95 zirconia and the particle size is ground to less than -200 mesh. Pickling initial purification process: The silicon concentrate 1 is pickled with sulfuric acid-phosphoric acid-hydrofluoric acid ternary pickling (pickling conditions: liquid-solid ratio of 6:1, acid concentration of 8 mol / L, sulfuric acid: phosphoric acid: hydrofluoric acid volume ratio of 2:2:1, reaction temperature of 100°C, reaction time of 3h). After the pickling, the pH value of ultrapure water cleaning is neutral. Then it is dried in a vacuum drying oven at 105°C for 3h to obtain high-purity quartz 1 of more than 3N.

[0045] (3) High-temperature hot-pressing leaching: A planetary ball mill was used to ball-mill the high-purity quartz 1. The ball mill jar and the ball mill medium were both made of 95 zirconia. The particle size was ground to below -5000 mesh. The silicon concentrate 1 was hot-pressed and pickled with sulfuric acid-phosphoric acid-hydrofluoric acid ternary acid. The leaching conditions were as follows: the total acid concentration was 12 mol / L, the ratio of sulfuric acid-phosphoric acid-hydrofluoric acid ternary acid was 2:2:1 (the ratio was by volume), the high-pressure leaching time was 6 h, the reaction temperature was 200 °C, and the liquid-solid ratio was 6:1 (mL:g), and the pickling product was obtained.

[0046] (4) Heat treatment: After acid washing, the product was washed with ultrapure water to a neutral pH value. It was then dried in a vacuum drying oven at 105°C for 3 hours, and then treated at 900°C in a rotary tube furnace for 3 hours. The product was then sealed in a vacuum package to obtain high-purity quartz 2. Figure 1 .

[0047] Table 1 Chemical composition of high purity quartz 2 in Example 1 / mg / kg

[0048]

[0049] Example 2

[0050] A method for efficiently separating and preparing 4N quartz by using high-silicon iron ore waste comprises the following steps:

[0051] (1) Desliming-magnetic separation: 100g of raw material was mixed with 500ml of water, and under the condition of 1.8T wet high-intensity magnetic separator, a silicon concentrate 1 with a grade of 95.45% and an iron concentrate 1 with a grade of 58.8% were obtained. 100g of iron concentrate 1 was mixed with 500g of water, and then passed through a 1.5T wet high-intensity magnetic separator to obtain iron concentrate 2 and silicon concentrate 2 with an iron grade of 60.56%. Ball milling: Silicon concentrate 1 was ball milled using a planetary ball mill, and the ball milling jar and ball milling medium were both made of 95 zirconia, and the particle size was ground to less than -200 mesh.

[0052] (2) Normal pressure leaching: The silicon concentrate 1 was pickled by sulfuric acid-phosphoric acid-hydrofluoric acid ternary pickling (pickling conditions: liquid-solid ratio of 5:1, acid concentration of 10 mol / L, sulfuric acid:phosphoric acid:hydrofluoric acid volume ratio of 2:2:1, reaction temperature of 100°C, reaction time of 3 h). After pickling, the pH value of ultrapure water washing was neutral. Then it was dried in a vacuum drying oven at 105°C for 3 h to obtain high-purity quartz 1 of more than 3N.

[0053] (3) High-temperature hot-pressing leaching: A planetary ball mill was used to ball-mill the high-purity quartz 1. The ball mill jar and the ball mill medium were both made of 95 zirconia. The particle size was ground to below -5000 mesh. The silicon concentrate 1 was hot-pressed and pickled with sulfuric acid-phosphoric acid-hydrofluoric acid ternary acid. The leaching conditions were as follows: the total acid concentration was 10 mol / L, the ratio of sulfuric acid-phosphoric acid-hydrofluoric acid ternary acid was 2:2:1 (the ratio was by volume), the high-pressure leaching time was 8 h, the reaction temperature was 200 °C, and the liquid-solid ratio was 5:1 (mL:g), and the pickling product was obtained.

[0054] (4) Heat treatment: After the acid wash, the product is washed with ultrapure water to a neutral pH value, dried in a vacuum drying oven at 105°C for 3 h, and then treated in a rotary tube furnace at 1000°C for 3 h, and then sealed in a vacuum package to obtain the product high-purity quartz 2.

[0055] Table 2 Chemical composition of high purity quartz 2 of Example 2 / mg / kg

[0056]

[0057] Example 3

[0058] A method for efficiently separating and preparing 4N quartz by using high-silicon iron ore waste comprises the following steps:

[0059] (1) Desliming-magnetic separation: 100g of raw material was mixed with 500ml of water, and under the condition of 1.8T wet high-intensity magnetic separator, a silicon concentrate 1 with a grade of 95.45% and an iron concentrate 1 with a grade of 58.8% were obtained. 100g of iron concentrate 1 was mixed with 500g of water, and then passed through a 1.5T wet high-intensity magnetic separator to obtain iron concentrate 2 and silicon concentrate 2 with an iron grade of 60.56%. Ball milling: Silicon concentrate 1 was ball milled using a planetary ball mill, and the ball milling jar and ball milling medium were both made of 95 zirconia, and the particle size was ground to less than -200 mesh.

[0060] (2) Normal pressure leaching: The silicon concentrate 1 was pickled by sulfuric acid-phosphoric acid-hydrofluoric acid ternary pickling (pickling conditions: liquid-solid ratio of 5:1, acid concentration of 10 mol / L, sulfuric acid:phosphoric acid:hydrofluoric acid volume ratio of 3:3:1, reaction temperature of 100°C, reaction time of 3 h). After pickling, the pH value of ultrapure water washing was neutral. Then it was dried in a vacuum drying oven at 105°C for 3 h to obtain high-purity quartz 1 of more than 3N.

[0061] (3) High-temperature hot-pressing leaching: A planetary ball mill was used to ball-mill the high-purity quartz 1. The ball mill jar and the ball mill medium were both made of 95 zirconia. The particle size was ground to below -5000 mesh. The silicon concentrate 1 was hot-pressed and pickled with sulfuric acid-phosphoric acid-hydrofluoric acid ternary acid. The leaching conditions were as follows: the total acid concentration was 10 mol / L, the ratio of sulfuric acid-phosphoric acid-hydrofluoric acid ternary acid was 3:3:1 (the ratio was by volume), the high-pressure leaching time was 8 h, the reaction temperature was 200 °C, and the liquid-solid ratio was 5:1 (mL:g), and the pickling product was obtained.

[0062] (4) Heat treatment: After the acid wash, the product is washed with ultrapure water to a neutral pH value, dried in a vacuum drying oven at 105°C for 3 h, and then treated in a rotary tube furnace at 1000°C for 3 h, and then sealed in a vacuum package to obtain the product high-purity quartz 2.

[0063] Table 3 Chemical composition of high purity quartz 2 of Example 3 / mg / kg

[0064]

[0065] Comparative Example 1

[0066] For comparison, in Comparative Example 1, a mixed acid of sulfuric acid and hydrofluoric acid (volume ratio of 2:1) was added, and the remaining preparation steps and process parameters were the same as those in Example 1 to obtain product quartz.

[0067] Table 4 Quartz chemical composition of comparative example 1 / mg / kg

[0068]

[0069] Figure 2 is the XRD diagram of iron concentrate 1 in Example 1, from Figure 2 It can be seen that the peak values ​​of Fe2O3 and FeO(OH) in iron concentrate 1 are also significantly increased, indicating that the grade of the iron concentrate is significantly improved after magnetic separation.

[0070] The present invention is not limited to the above-mentioned embodiments, and various changes can be made within the knowledge scope of ordinary technicians in this field without departing from the purpose of the present invention.

Claims

1. A method for efficiently separating and preparing 4N quartz using high-silicon iron ore waste, characterized in that: The following steps are involved: (1) Desliming-magnetic separation: The high-silicon iron ore waste is first deslimed and then subjected to multi-stage magnetic separation. The first stage of strong magnetic separation is 1.8-2.1T. After magnetic separation, the first iron concentrate and silicon concentrate are obtained. The first iron concentrate is then subjected to the second stage of magnetic separation. The magnetic field strength is 1.5-1.6T to obtain the second iron concentrate. (2) Normal pressure leaching: ball-milling the silicon concentrate obtained in step (1) to a predetermined fineness, performing normal pressure leaching using a ternary mixed acid, washing the leached product to neutrality, and drying to obtain a first high-purity quartz; (3) High-temperature hot-pressing leaching: ball-milling the first high-purity quartz to a set fineness, and performing high-temperature hot-pressing leaching on the ball-milled first high-purity quartz using a ternary mixed acid to obtain an acid-washed product; (4) Heat treatment: The acid-washed product obtained in step (3) is washed to neutrality, dried and then heat-treated to obtain the second high-purity quartz, i.e., the 4N quartz product; The ternary mixed acid is a mixed acid of sulfuric acid, phosphoric acid and hydrofluoric acid, and the volume ratio is 1-3:1-3:

1.

2. A method for efficiently separating and preparing 4N quartz by using high-silicon iron ore waste according to claim 1, characterized in that: In step (1), a wet high-intensity magnetic separator or a high-gradient magnetic separator is used for magnetic separation.

3. A method for efficiently separating and preparing 4N quartz by using high-silicon iron ore waste according to claim 1, characterized in that: In step (1), the pulp ratio of the first stage of high intensity magnetic separation is 1:5-10.

4. A method for efficiently separating and preparing 4N quartz using high-silicon iron ore waste according to claim 1, characterized in that: In step (1), the pulp ratio of the second stage magnetic separation is 1:5-10.

5. A method for efficiently separating and preparing 4N quartz by using high-silicon iron ore waste according to claim 1, characterized in that: In step (2), the atmospheric pressure leaching process is: the acid concentration is 9-10 mol / L, the atmospheric pressure leaching time is 5-6 hours, the reaction temperature is 90-100° C., and the liquid-solid ratio is 4-5:1 (mL:g).

6. A method for efficiently separating and preparing 4N quartz using high-silicon iron ore waste according to claim 1, characterized in that: In steps (2) and (3), during the ball milling process, zirconium balls are used as grinding media and nylon screens are used as sieves.

7. The method for preparing 4N quartz by efficiently separating high-silicon iron ore waste according to claim 1, characterized in that: In step (3), the high temperature hot pressure leaching process: the acid concentration is 9-10 mol / L, the leaching time is 5-8 hours, the reaction temperature is 180-200° C., and the liquid-to-solid ratio is 4-5:1 (mL:g).

8. The method for preparing 4N quartz by efficiently separating high-silicon iron ore waste according to claim 1, characterized in that: In step (4), the heat treatment process is specifically: high temperature treatment at 900-1000° C. in a tubular furnace for 3-5 hours.

9. The method for preparing 4N quartz by efficiently separating high-silicon iron ore waste according to claim 1, characterized in that: The second stage magnetic separation is to perform one or more magnetic separations on the first iron concentrate.

Citation Information

Patent Citations

  • Method for purifying vein quartz under non-pickling condition

    CN102126727A

  • Natural powder quartz purification method, high-purity powder quartz and quartz product

    CN109019609A

  • Green and efficient method for preparing high-purity quartz

    CN116654944A

  • Method for refining high-purity quartz sand by using common quartz sand

    CN117303376A

  • Method for preparing high-purity quartz sand through ultrasonic-assisted pickling