Method for preparing 1, 5-dihydroxy-2-pentanone from furfural
By reacting furfural with a solvent and a supported catalyst under a hydrogen atmosphere, the problems of low product selectivity and waste liquid in the synthesis of 1,5-dihydroxy-2-pentanone in the existing technology are solved, and high yield and Green raw materials are used and there is no halogen-containing waste liquid discharge.
Patent Information
- Application Number
- CN202410762476.2
- Authority / Receiving Office
- CN · China
- Patent Type
- Applications(China)
- Current Assignee / Owner
- Filing Date
- 2024-06-13
- Publication Date
- 2024-10-15
AI Technical Summary
The existing synthesis method of 1,5-dihydroxy-2-pentanone has the problems of low product selectivity, low atom economy and halogen-containing waste liquid.
Mix furfural with a solvent, add a supported catalyst to react in a hydrogen atmosphere, use water or a mixed solvent of water and organic solvents, control the reaction conditions such as temperature and time, and use a metal-supported catalyst such as Pd/TiO2 for catalysis to avoid containing halogen. Generation of liquid waste.
The complete conversion of furfural is achieved, the yield of 1,5-dihydroxy-2-pentanone is increased, and there is no emission of halogen-containing waste liquid. The catalyst can be recycled and the source of raw materials is green.
Smart Images

Figure CN118771966A_ABST
Abstract
Description
Technical Field
[0001] The invention relates to the field of biomass catalytic conversion, and in particular to a method for preparing 1,5-dihydroxy-2-pentanone by utilizing furfural. Background Art
[0002] Due to the society's great concern about sustainable development and environmental issues (such as carbon dioxide and sulfur dioxide emissions), the preparation of bio-based fuels or important chemicals from renewable biomass resources can not only alleviate the crisis of increasingly depleted fossil resources, but also provide an innovative source of power for people to develop new materials based on the unique structural properties of bio-based chemicals.
[0003] Furfural is an important biomass-based platform molecule. Furfural can be converted into high value-added chemicals such as furfuryl alcohol, tetrahydrofurfuryl alcohol, 2-methylfuran and 1,5-pentanediol through catalytic conversion.
[0004] 1,5-dihydroxy-2-pentanone is an important fine chemical raw material and pharmaceutical intermediate, and is widely used in the fields of pesticides. 1,5-dihydroxy-2-pentanone can be used as an important intermediate for the synthesis of high-value chemicals such as 5-hydroxy-2-pentanone, vitamin B1 and 1,4-butanediol. The current methods for synthesizing 1,5-dihydroxy-2-pentanone include hydrolysis of 2,2-dibromo-1,5-pentanediol under acetic acid catalysis (J.Org.Chem.1962,27,5,1575) and xylose dehydration-hydrogenation method. These methods have the disadvantages of producing halogen-containing waste liquid, low atom economy and low product selectivity. Summary of the invention
[0005] In order to improve the above technical problems, the present invention provides a method for preparing 1,5-dihydroxy-2-pentanone, comprising the following steps: mixing furfural with a solvent, adding a supported catalyst, and reacting under a hydrogen atmosphere to obtain 1,5-dihydroxy-2-pentanone.
[0006] According to an embodiment of the present invention, the solvent is water or a mixed solvent of water and an organic solvent; the organic solvent can be selected from tetrahydrofuran, dioxane, 2-methyltetrahydrofuran, acetonitrile, toluene; for example, a mixed solution of water and dioxane.
[0007] According to an embodiment of the present invention, the concentration of furfural in the solvent can be 0.2-5wt%, for example 0.25-3wt%, such as 0.5wt%, 0.75wt%, 1wt%, 1.25wt%, 1.5wt%, 1.75wt%, 2wt%, 2.25wt%, 2.5wt%, 2.75wt%.
[0008] According to an embodiment of the present invention, the volume of the reaction solution in the reaction is 0.001-10L, for example 0.002-0.5L, such as 2mL, 5mL, 10mL;
[0009] According to an embodiment of the present invention, the ratio of water to organic solvent in the reaction solution is 1%-100%, for example 1%, 10%, 50%, 100%;
[0010] According to an embodiment of the present invention, the reaction temperature may be 60-180°C; for example 80-160°C, 100°C, 120°C, 140°C.
[0011] According to an embodiment of the present invention, the reaction time may be 1-16 h; for example 2-8 h, such as 2 h, 4 h, 6 h.
[0012] According to an embodiment of the present invention, the supported catalyst is an MD / support catalyst, M is a metal selected from Pd, Pt or Ru; D is a second doping metal selected from V, Nb or W; the support is selected from TiO 2 、CeO 2 , Nb 2 O 5 .
[0013] According to an embodiment of the present invention, the TiO 2 It may be selected from at least one of anatase type, P25 type or rutile type.
[0014] According to an embodiment of the present invention, the loading amount of M in the supported catalyst is 0.05wt%-15wt%, for example, 0.5wt%-5wt%, such as 1wt%, 2wt%, 3wt%, 4wt%; the loading amount of D is 0.1wt%-5wt%, for example, 0.5wt%-3wt%, such as 1wt%, 1.5wt%, 2wt%, 2.5wt%.
[0015] According to an embodiment of the present invention, the supported catalyst is selected from Pd / TiO 2 (Anatase type), Pd / TiO 2 (P25 type), Pd / TiO 2 (Rutile), Pd-V / TiO 2 (Rutile), Pd-Nb / TiO 2 (rutile type); preferably, the Pd / TiO 2 The catalyst loading is 3wt%, and the Pd-V / TiO 2 The catalyst has a palladium loading of 3wt% and a vanadium loading of 1wt%. 2The palladium loading in the catalyst is 3 wt % and the niobium loading is 1 wt %.
[0016] According to an embodiment of the present invention, the volume ratio of the mass of the supported catalyst to the solvent can be (0.001-25) g / mL, for example (0.005-10) g / mL, such as 0.002 g / mL, 0.005 g / mL, 0.008 g / mL, 0.01 g / mL, 0.015 g / mL, 0.02 g / mL, 0.05 g / mL.
[0017] According to an embodiment of the present invention, the pressure of hydrogen in the reaction may be 0.1-10 MPa; for example, 0.2-5 MPa, such as 0.5 MPa, 0.75 MPa, 1 MPa, 1.5 MPa, 2 MPa, 3 MPa, 4 MPa.
[0018] According to an embodiment of the present invention, water is present in sufficient amount in the reaction.
[0019] The present invention also provides a method for synthesizing the supported catalyst, comprising the following steps:
[0020] i) dissolving the metal precursor and potassium chloride in deionized water, adding the carrier, and stirring at room temperature for 6-12 hours;
[0021] ii) adding potassium hydroxide to the reaction solution of step i) to adjust the pH value to 10-12, and then stirring at room temperature for 6-12 hours;
[0022] iii) centrifuging the suspension obtained in step ii), washing until the pH value reaches 6-8, and then dispersing in deionized water;
[0023] iv) adding KBH to the suspension obtained in step iii) 4 or NaBH 4 The solution was stirred at room temperature for 6-12 hours;
[0024] v) centrifuging the suspension obtained in step iv), washing it and then vacuum drying it to obtain the supported catalyst.
[0025] According to an embodiment of the present invention, the metal precursor includes precursor 1 and / or precursor 2; the precursor 1 is selected from Pd salt, Pt salt or Ru salt; the precursor 2 is selected from V salt, Nb salt or W salt;
[0026] According to an embodiment of the present invention, the precursor 1 is palladium chloride, platinum chloride, or ruthenium chloride;
[0027] According to an embodiment of the present invention, the precursor 2 is selected from niobium oxalate or ammonium metavanadate.
[0028] According to an embodiment of the present invention, the carrier is selected from TiO2 、CeO 2 , Nb 2 O 5 .
[0029] According to an embodiment of the present invention, the TiO 2 It may be selected from at least one of anatase type, P25 type or rutile type.
[0030] Beneficial Effects
[0031] Compared with the prior art for synthesizing 1,5-dihydroxy-2-pentanone, the method of the present invention uses furfural as a raw material, has the advantages of green raw material source, high yield of target product, no halogen-containing waste liquid discharge, and catalyst recyclability. In the method of the present invention, furfural can be completely converted, and the yield of 1,5-dihydroxy-2-pentanone can reach up to 36.0%. BRIEF DESCRIPTION OF THE DRAWINGS
[0032] Figure 1 The supported catalyst (Pd-Nb / TiO 2 (Rutile type)) scanning transmission electron microscopy image.
[0033] Figure 2 The catalyst of Example 1 of the present invention is Pd / TiO 2 Gas chromatograms of 1,5-dihydroxy-2-pentanone, tetrahydrofurfuryl alcohol and 5-hydroxy-2-pentanone obtained when (anatase type) was used. DETAILED DESCRIPTION
[0034] The technical solution of the present disclosure will be further described in detail below in conjunction with specific embodiments. It should be understood that the following embodiments are only exemplary illustrations and explanations of the present disclosure and should not be construed as limiting the scope of protection of the present disclosure. All technologies implemented based on the above content of the present disclosure are included in the scope of protection intended by the present disclosure.
[0035] Unless otherwise specified, the raw materials and reagents used in the following examples are commercially available or can be prepared by known methods.
[0036] In the following examples, the raw materials and products were detected by centrifuging the reaction solution and the catalyst, adding a certain amount of γ-valerolactone ethanol solution as an internal standard, mixing the internal standard with the reaction clear solution, and performing gas phase analysis and quantification (Agilent 7890B; split flow injection port; separation column: HP-INNOWAX (0.32 mm×30 m); hydrogen ion flame detector)
[0037] Catalyst Preparation Example 1:
[0038] Synthesis of Pd-Nb / TiO 2(rutile type) catalyst, comprising the steps of:
[0039] i) dissolving palladium chloride, niobium oxalate and potassium chloride in deionized water, adding rutile titanium dioxide, and stirring at room temperature for 6-12 hours;
[0040] ii) adding potassium hydroxide to the reaction solution of step i) to adjust the pH value to 10, and stirring at room temperature for 12 hours;
[0041] iii) centrifuging the suspension obtained in step ii), washing until the pH reaches 7, and then dispersing in deionized water;
[0042] iv) adding KBH to the suspension obtained in step iii) 4 The solution was stirred at room temperature for 12 h.
[0043] v) centrifuging the suspension obtained in step iv), washing it and then vacuum drying it to obtain Pd-Nb / TiO 2 (Rutile) catalyst.
[0044] The other catalysts used below were prepared by referring to the above steps to obtain Pd / TiO 2 (Anatase type) catalyst, Pd / TiO 2 (Anatase type) catalyst, Pd / TiO 2 (P25 type) catalyst, Pd / TiO 2 (Rutile type) catalyst, Pd-V / TiO 2 (Rutile) catalyst.
[0045] Embodiment 1:
[0046] 2 mL of furfural aqueous solution with a mass fraction of 2.5 wt% was placed in a reactor, and 0.01 g of Pd / TiO with a loading of 3% was added. 2 (anatase type) catalyst. After replacing the air in the reactor three times, H 2 The pressure in the reactor was set to 1 MPa at room temperature, and the reactor was sealed and heated to 120°C, and stirred for 2 hours. The reaction liquid and the catalyst were separated by centrifugation, and the upper clear layer was analyzed for gas phase.
[0047] The results showed that the furfural conversion rate was 100%, the yield of 1,5-dihydroxy-2-pentanone was 11.6%, and other products included tetrahydrofurfuryl alcohol, 5-hydroxy-2-pentanone, etc.
[0048]
[0049] Embodiment 2:
[0050] The concentration and volume of the furfural aqueous solution used were the same as those in Example 1 of the present invention, and 0.01 g of Pd / TiO with a loading of 3% was added. 2 (P25 type) catalyst. After replacing the air in the reactor three times, H 2 The pressure in the reactor was set to 1 MPa at room temperature, and the reactor was sealed and heated to 120°C, and stirred for 2 hours. The reaction liquid and the catalyst were separated by centrifugation, and the upper clear layer was analyzed for gas phase.
[0051] The results showed that the furfural conversion rate was 100%, the yield of 1,5-dihydroxy-2-pentanone was 34.9%, and other products included tetrahydrofurfuryl alcohol, 5-hydroxy-2-pentanone, etc.
[0052] Embodiment 3:
[0053] 10 mL of furfural aqueous solution with a mass fraction of 0.25 wt% was placed in a reactor, and 0.05 g of Pd / TiO with a loading of 3% was added. 2 (Rutile type) catalyst. After replacing the air in the reactor three times, fill it with H 2 The pressure in the reactor was set to 0.75 MPa at room temperature, and the reactor was sealed and heated to 100°C, and stirred for 4 hours. The reaction liquid and the catalyst were separated by centrifugation, and the upper clear layer was analyzed for gas phase.
[0054] The results showed that the furfural conversion rate was 100%, the yield of 1,5-dihydroxy-2-pentanone was 29.3%, and other products included tetrahydrofurfuryl alcohol, tetrahydrofurfural, etc.
[0055] Embodiment 4:
[0056] The concentration and volume of the furfural aqueous solution used were the same as those in Example 1 of the present invention, and 0.01 g of Pd-V / TiO with a palladium loading of 3% and a vanadium loading of 1% was added. 2 (Rutile type) catalyst. After replacing the air in the reactor three times, fill it with H 2 The pressure in the reactor was set to 1 MPa at room temperature, and the reactor was sealed and heated to 120°C, and stirred for 2 hours. The reaction liquid and the catalyst were separated by centrifugation, and the upper clear layer was analyzed for gas phase.
[0057] The results showed that the furfural conversion rate was 100%, the yield of 1,5-dihydroxy-2-pentanone was 36.0%, and other products included tetrahydrofurfuryl alcohol, 5-hydroxy-2-pentanone, etc.
[0058] Embodiment 5:
[0059] The concentration and volume of the furfural aqueous solution used were the same as those in Example 1 of the present invention, and 0.01 g of Pd-Nb / TiO with a palladium loading of 3% and a niobium loading of 1% was added. 2(Rutile type) catalyst. After replacing the air in the reactor three times, fill it with H 2 The pressure in the reactor was set to 1 MPa at room temperature, and the reactor was sealed and heated to 120°C, and stirred for 2 hours. The reaction liquid and the catalyst were separated by centrifugation, and the upper clear layer was analyzed for gas phase.
[0060] The results showed that the furfural conversion rate was 100%, the yield of 1,5-dihydroxy-2-pentanone was 25.0%, and other products included tetrahydrofurfuryl alcohol, 5-hydroxy-2-pentanone, etc.
[0061] Embodiment 6:
[0062] The catalyst after the reaction in the above Example 5 is recovered through washing and drying steps.
[0063] The concentration and volume of the furfural aqueous solution used were the same as those in Example 1 of the present invention, and the Pd-Nb / TiO 2 (Rutile type) catalyst. After replacing the air in the reactor three times, fill it with H 2 The pressure in the reactor was set to 1 MPa at room temperature, and the reactor was sealed and heated to 120°C, and stirred for 2 hours. The reaction liquid and the catalyst were separated by centrifugation, and the upper clear layer was analyzed for gas phase.
[0064] The results showed that the furfural conversion rate was 100%, the yield of 1,5-dihydroxy-2-pentanone was 24.8%, and other products included tetrahydrofurfuryl alcohol, 5-hydroxy-2-pentanone, etc.
[0065] Comparative Example 1:
[0066] The concentration and volume of the furfural aqueous solution used were the same as those in Example 1 of the present invention, and 0.01 g of a 3% Pd / MgO catalyst was added. The air in the reactor was replaced three times and H 2 The pressure in the reactor was set to 1 MPa at room temperature, and the reactor was sealed and heated to 100°C, and stirred for 2 hours. The reaction liquid and the catalyst were separated by centrifugation, and the upper clear layer was analyzed for gas phase.
[0067] The results showed that the furfural conversion rate was 100%, and the products in the reaction supernatant included tetrahydrofurfuryl alcohol, tetrahydrofurfural, etc., and no 1,5-dihydroxy-2-pentanone was detected.
[0068] The above is an exemplary description of the implementation of the technical solution of the present disclosure. It should be understood that the protection scope of the present disclosure is not limited to the above-mentioned implementation. Any modification, equivalent substitution, improvement, etc. made by those skilled in the art within the spirit and principle of the present disclosure shall be included in the protection scope of the claims of this application.
Claims
1. A method for preparing 1,5-dihydroxy-2-pentanone, comprising the following steps: mixing furfural with a solvent, adding a supported catalyst, and reacting under a hydrogen atmosphere to obtain 1,5-dihydroxy-2-pentanone; The solvent is water or a mixed solvent of water and an organic solvent; the organic solvent can be selected from tetrahydrofuran, dioxane, 2-methyltetrahydrofuran, acetonitrile, toluene; for example, a mixed solution of water and dioxane.
2. The method according to claim 1, characterized in that The concentration of furfural in the solvent may be 0.2-5 wt%, such as 0.25-3 wt%.
3. The method according to claim 1 or 2, characterized in that: The volume of the reaction solution in the reaction is 0.001-10 L, for example 0.002-0.5 L; Preferably, the ratio of water to organic solvent in the reaction solution is 1%-100%, such as 5%-90%.
4. The method according to any one of claims 1 to 3, characterized in that: The reaction temperature may be 60-180°C; for example 80-160°C; Preferably, the reaction time may be 1-16 h; for example 2-8 h.
5. The method according to any one of claims 1 to 4, characterized in that: The supported catalyst is a MD / carrier catalyst, M is a metal selected from Pd, Pt or Ru; D is a second doping metal selected from V, Nb or W; the carrier is selected from TiO2, CeO2, Nb2O5; Preferably, the TiO2 can be selected from at least one of anatase type, P25 type or rutile type.
6. The method according to claim 5, characterized in that The loading amount of M in the supported catalyst is 0.05wt%-15wt%, for example 0.5wt%-5wt%; Preferably, the loading amount of D is 0.1 wt%-5 wt%, such as 0.5 wt%-3 wt%.
7. The method according to any one of claims 1 to 6, characterized in that: The supported catalyst is, for example, selected from Pd / TiO2 (anatase type), Pd / TiO2 (P25 type), Pd / TiO2 (rutile type), Pd-V / TiO2 (rutile type), Pd-Nb / TiO2 (rutile type); Preferably, the loading amount of the Pd / TiO2 catalyst is 3wt%, the loading amount of palladium in the Pd-V / TiO2 catalyst is 3wt%, and the loading amount of vanadium is 1wt%, and the loading amount of palladium in the Pd-Nb / TiO2 catalyst is 3wt%, and the loading amount of niobium is 1wt%.
8. The method according to any one of claims 1 to 7, characterized in that: The mass ratio of the supported catalyst to the volume ratio of the solvent may be (0.001-25) g / mL, for example (0.005-10) g / mL; Preferably, the pressure of hydrogen in the reaction may be 0.1-10 MPa; for example 0.2-5 MPa; Preferably, water is present in sufficient amount in the reaction.
9. The method according to any one of claims 1 to 7, characterized in that: The method for synthesizing the supported catalyst comprises the following steps: i) dissolving the metal precursor and potassium chloride in deionized water, adding the carrier, and stirring at room temperature for 6-12 hours; ii) adding potassium hydroxide to the reaction solution of step i) to adjust the pH value to 10-12, and then stirring at room temperature for 6-12 hours; iii) centrifuging the suspension obtained in step ii), washing until the pH value reaches 6-8, and then dispersing in deionized water; iv) adding KBH4 or NaBH4 solution to the suspension obtained in step iii) and continuing stirring at room temperature for 6-12 hours; v) centrifuging the suspension obtained in step iv), washing it and then vacuum drying it to obtain the supported catalyst.
10. The method according to claim 9, characterized in that The metal precursor includes precursor 1 and / or precursor 2; the precursor 1 is selected from Pd salt, Pt salt or Ru salt; the precursor 2 is selected from V salt, Nb salt or W salt; Preferably, the precursor 1 is palladium chloride, platinum chloride, or ruthenium chloride; Preferably, the precursor 2 is selected from niobium oxalate or ammonium metavanadate; Preferably, the carrier is selected from TiO2, CeO2, Nb2O5; Preferably, the TiO2 can be selected from at least one of anatase type, P25 type or rutile type.