Preparation of degradable and recyclable thermoset material based on 7-oxo-2, 3-diaza norbornene monomer

Through the cross-linking polymerization of 7-oxo-2,3-diazanorbornene and DCPD, the degradable thermosetting material P-MX-DCPD is formed, which solves the complex preparation process and controllable distribution problems in the existing technology, and achieves The industrial production of materials and their degradation and utilization under acidic conditions have significantly reduced costs and recycling problems.

CN118772335AActive Publication Date: 2024-10-15INST OF CHEM CHINESE ACAD OF SCI
View PDF 3 Cites 0 Cited by

Patent Information

Application Number
CN202310370258.X
Authority / Receiving Office
CN · China
Patent Type
Applications(China)
Current Assignee / Owner
Filing Date
2023-04-07
Publication Date
2024-10-15
Estimated Expiration
2043-04-07

AI Technical Summary

Technical Problem

The preparation process of existing degradable and recyclable thermoset materials is complicated, and it is difficult to achieve controllable degradable group distribution during the DCPD copolymerization process, making recycling and reuse difficult.

Method used

7-Oxo-2,3-diazanorbornene monomer and dicyclopentadiene DCPD are cross-linked and polymerized under the action of a ruthenium complex catalyst to form a degradable and recyclable thermosetting material P-MX-DCPD. Degradation occurs under acidic conditions to enable material reuse.

Benefits of technology

Industrialized production of degradable thermosetting materials has been achieved. The degraded products can be reused, significantly reducing production costs and recycling problems, and providing a more economical and efficient solution.

✦ Generated by Eureka AI based on patent content.

Smart Images

  • Figure CN118772335A_ABST
    Figure CN118772335A_ABST
Patent Text Reader

Abstract

The present invention provides a cross-linked polymer P-MX-DCPD based on the monomers MX and DCPD of 7-oxo-2, 3-diaza norbornene, and a method for preparing the cross-linked polymer P-MX-DCPD based on the monomers MX and DCPD. The obtained cross-linked polymer uses the raw materials 7-oxo-2, 3-diaza norbornene and DCPD which can be industrially produced, so that the cross-linked polymer P-MX-DCPD can also realize industrial production, and the production cost is obviously lower than that of the existing degradable and recyclable cross-linked polymer. More importantly, the cross-linked polymer provided by the invention can be degraded under an acidic condition, and a product obtained by degradation can be reused, so that the problem that the existing cross-linked polymer is difficult to degrade and recycle is obviously improved. # imgabs0 #
Need to check novelty before this filing date? Find Prior Art

Description

Technical Field

[0001] The invention belongs to the technical field of preparation of degradable polymers, and in particular relates to the synthesis of a degradable and recyclable thermosetting material based on 7-oxo-2,3-diazanorbornene. Background Art

[0002] More than 100 years since Hermann Staudinger proposed the macromolecular hypothesis, our society has benefited from the ubiquity of synthetic polymers with excellent thermal, optical, mechanical and chemical properties. Among them, thermosets are polymer materials that have a permanent shape after curing. They play a key role in the modern plastics and rubber industries, accounting for about 20% of today's polymer material manufacturing, with an annual global production of about 65 million tons. However, with the increasing production of thermosets and their inherent insoluble and infusible properties, the scrapping of thermoset waste has become a serious problem. Scientists have proposed many strategies to solve this problem, including traditional recycling, biodegradation, synthesis of polymers from biorenewable resources and various upcycling technologies. Among them, the development of degradable and recyclable thermosets has received widespread attention because the cross-linking properties of thermosets can be structurally changed from the perspective of synthetic chemistry.

[0003] Ring-opening metathesis polymerization (ROMP) has become one of the most common polymerization methods because of its mild reaction conditions and wide compatibility with functional groups. Using dicyclopentadiene (DCPD) monomer, the thermosetting cross-linked polymer material PDCPD can be directly obtained through ROMP polymerization. It has very excellent mechanical strength and is increasingly widely used as a special material in the fields of bulletproof, wind turbine blades, and automobile bumpers. However, consistent with other thermosetting materials, PDCPD is a cross-linked structure composed of C-C bonds with stable chemical properties, which poses great challenges in its recovery and reuse after service. If degradable functional groups are introduced into the monomer and the degradable monomer is copolymerized with DCPD, a degradable thermosetting PDCPD material can be obtained, which provides a new idea for the preparation of degradable and recyclable thermosetting materials. However, one of the limitations of this strategy is that it requires the use of specially designed degradable monomers, and the known degradable monomers either require multi-step synthesis, the preparation process is extremely complicated, or the monomer ring tension is insufficient, and the controllable distribution of degradable groups cannot be achieved during the DCPD copolymerization process. Summary of the invention

[0004] In order to prepare a degradable and recyclable thermosetting material, the present invention provides a cross-linked polymer based on 7-oxygen-2,3-diazanorbornene monomer, and copolymerizes the monomer 7-oxygen-2,3-diazanorbornene with dicyclopentadiene DCPD under the action of a ruthenium complex catalyst to obtain a degradable and recyclable thermosetting material.

[0005] The present invention first provides the following cross-linked polymer P-MX-DCPD based on 7-oxo-2,3-diazanorbornene monomer MX and DCPD:

[0006]

[0007] Among them, R 1 , R 2 The same or different, independently selected from C 1-12 Alkyl, C 1-12 Alkoxy chain formed by replacing 1 to 6 carbon atoms on the alkyl group with oxygen, -(CH2) p C 6-20 Aryl, p is an integer >=0.

[0008] According to an embodiment of the present invention, the cross-linked polymer P-MX-DCPD structure is shown below:

[0009]

[0010] R 1 , R 2 Having the above definition; (x+y), z are the same or different and are independently an integer of 2-200000.

[0011] According to an embodiment of the present invention, R 1 , R 2 The same or different, independently selected from C 1-6 Alkyl, C 1-6 Alkoxy chain formed by replacing 1 to 3 carbon atoms on the alkyl group with oxygen, -(CH2) p C 6-12 Aryl, p is an integer of 1-6;

[0012] (x+y), z are the same or different and are independently an integer of 10-20000, for example, an integer of 20-2000.

[0013] According to an embodiment of the present invention, R 1 , R 2 is the same and is selected from methyl, ethyl, propyl, isopropyl, benzyl, butyl, isobutyl or tert-butyl.

[0014] In one embodiment, the cross-linked polymer P-MX-DCPD has the following structure:

[0015]

[0016] wherein (x+y), z are the same or different and are independently 50, 100, 150, 200, 250, 300, 350, 400, 450, 500, 550, 600, 650, 700, 1000 or 2000.

[0017] According to an embodiment of the present invention, the cross-linked polymer P-MX-DCPD is a thermosetting material.

[0018] The present invention also provides a method for preparing the cross-linked polymer P-MX-DCPD, comprising the following steps:

[0019] 7-Oxo-2,3-diazanorbornene monomer MX and DCPD undergo cross-linking polymerization reaction under the action of ruthenium complex catalyst.

[0020] According to an embodiment of the present invention, the cross-linked polymer reaction is:

[0021]

[0022] According to an embodiment of the present invention, the ruthenium complex catalyst is a common olefin metathesis catalyst containing a ruthenium-carbene structure, wherein the most preferred catalyst is selected from one of the following G1, G2 or G3:

[0023]

[0024] According to an embodiment of the present invention, the reaction is carried out in an inert gas atmosphere, for example, in a nitrogen atmosphere.

[0025] According to an embodiment of the present invention, the molar ratio of monomer MX, DCPD to ruthenium complex catalyst is (2-200000): (2-200000): 1; when the molar ratio of monomer MX, DCPD to catalyst is 100:2000:1, a polymer with a repeating unit number z of 100 and (x+y) of 2000 is obtained; when the molar ratio of monomer MX, DCPD to catalyst is 400:2000:1, a polymer with a repeating unit number z of 400 and (x+y) of 2000 is obtained; and so on.

[0026] According to an embodiment of the present invention, the preparation method of the cross-linked polymer P-MX-DCPD is specifically operated as follows: DCPD and a certain proportion of 7-oxo-2,3-diazanorbornene monomer MX are added to a reaction bottle, and a toluene solution of the G2 catalyst is added under vigorous stirring conditions.

[0027] According to an embodiment of the present invention, during the reaction, depending on the type and proportion of monomers added, the reaction is stirred for 5-30 minutes, then transferred to a shaped mold, the reaction temperature is controlled to be below 20°C for 2-24 hours, and then reacted at high temperature for 0.5-2 hours; finally, cooled to room temperature, and the material is taken out to obtain a recyclable thermosetting material.

[0028] The present invention also provides a method for degrading the P-MX-DCPD thermosetting material as described above, comprising the following steps:

[0029] The cross-linked polymer P-MX-DCPD degrades under acidic conditions.

[0030] According to an embodiment of the present invention, the acidic condition is provided by hydrochloric acid or trifluoroacetic acid. The pH of the acidic condition is <7.0.

[0031] The present invention also provides the use of the cross-linked polymer P-MX-DCPD in preparing a high-strength thermosetting material. The high-strength thermosetting material is mainly used in the fields of construction materials, vehicles, aerospace, electronic and electrical or sports equipment.

[0032] Beneficial Effects

[0033] The present application provides a cross-linked polymer based on a class of 7-oxy-2,3-diazanorbornene and DCPD monomers. The obtained cross-linked polymer uses industrially produced raw materials 7-oxy-2,3-diazanorbornene and DCPD. Therefore, the cross-linked polymer P-MX-DCPD can also be industrially produced, and the production cost is significantly lower than that of existing degradable and recyclable cross-linked polymers. More importantly, the cross-linked polymer of the present application is degradable under acidic conditions, and the degradation product can be reused, which significantly improves the problem of difficult degradation and recycling of existing cross-linked polymers.

[0034] Definitions and explanations of terms

[0035] The term "C 1-12 “Alkyl” is understood as meaning a linear or branched, saturated, monovalent hydrocarbon radical having 1, 2, 3, 4, 5, 6, 7, 8, 9, 10, 11 or 12 carbon atoms, for example methyl, ethyl, propyl, butyl, pentyl, hexyl, isopropyl, isobutyl, sec-butyl, tert-butyl, isopentyl, 2-methylbutyl, 1-methylbutyl, 1-ethylpropyl, 1,2-dimethylpropyl, neopentyl, 1,1-dimethylpropyl, 4-methylpentyl, 3-methylpentyl, 2-methylpentyl, 1-methylpentyl, 2-ethylbutyl, 1-ethylbutyl, 3,3-dimethylbutyl, 2,2-dimethylbutyl, 1,1-dimethylbutyl, 2,3-dimethylbutyl, 1,3-dimethylbutyl or 1,2-dimethylbutyl or their isomers. In particular, the radicals have 1, 2, 3 or 4 carbon atoms (“C1-4 alkyl), for example methyl, ethyl, propyl, butyl, isopropyl, isobutyl, sec-butyl, tert-butyl, more particularly, the radical having 1, 2 or 3 carbon atoms (“C 1-3 alkyl"), for example methyl, ethyl, n-propyl or isopropyl.

[0036] The term "C 1-12 The C in the alkoxy chain formed by the substitution of 1 to 6 carbon atoms on the alkyl group by O 1-12 Alkyl has the same meaning as above. BRIEF DESCRIPTION OF THE DRAWINGS

[0037] Figure 1 For P-M1 100 -s-DCPD 1000 TGA curve of .

[0038] Figure 2 For P-M3 200 -s-DCPD 2000 TGA curve of .

[0039] Figure 3 For P-M1 400 -s-DCPD 2000 , P-M1 200 -s-DCPD 2000 , P-M1 100 -s-DCPD 2000 and P-DCPD 2000 DSC curve of .

[0040] Figure 4 For P-M1 400 -s-DCPD 2000 , P-M2 400 -s-DCPD 2000 , P-M3 400 -s-DCPD 2000 and P-M4 400 -s-DCPD 2000 DSC curve of .

[0041] Figure 5 For P-M1 200 -s-DCPD 2000 GPC of the degradation products in hydrochloric acid tetrahydrofuran solution.

[0042] Figure 6 For P-M1 200 -s-DCPD 2000 Schematic diagram of the degradation in trifluoroacetic acid in tetrahydrofuran.

[0043] Figure 7 For polymer P-M1200 -s-DCPD 2000 and P-DCPD 2000 Photos. DETAILED DESCRIPTION

[0044] The preparation method of the present invention will be described in further detail below in conjunction with specific examples. It should be understood that the following examples are only exemplary illustrations and explanations of the present invention and should not be construed as limiting the scope of protection of the present invention. All technologies implemented based on the above content of the present invention are included in the scope that the present invention is intended to protect.

[0045] Unless otherwise specified, the experimental methods used in the following examples are all conventional methods; the reagents, materials, etc. used in the following examples, unless otherwise specified, can be obtained from commercial channels.

[0046] Example 1

[0047]

[0048] Diethyl azodicarboxylate (20mmol, 3.5g) and furan (60mmol, 4.4ml) were placed in a 20ml reaction bottle equipped with a magnetron and stirred at 25°C for 2.0h until the color changed from orange-red to almost colorless. After removing the excess furan by rotary evaporation, no further purification was required, and the light yellow or colorless transparent oil obtained was the target product 7-oxo-2,3-di(ethyl azoacetate) heteronorbornene monomer M1. When the reaction is further amplified, exothermic phenomenon will occur. At the beginning of the reaction, it is necessary to cool with an ice water bath, and the prepared monomer is stored in a refrigerator at low temperature. In addition, monomers M2, M3 and M4 were also prepared. The structures of monomers M2, M3 and M4 are shown below:

[0049]

[0050] Example 2

[0051]

[0052] Under room temperature and air conditions, 26.5 g (200 mmol) of DCPD and 2.5 g (10.0 mmol) of 7-oxo-2,3-diazanorbornene monomer M1 were added to the reaction bottle, and 0.5 mL of toluene solution prepared by 73 mg of G2 catalyst was added under vigorous stirring. The reaction was stirred for 20 minutes to obtain a thermosetting polymer P-M1. 100 -s-DCPD 2000 Then transfer it to a shaped mold and react at 90℃ for 1.0h. Finally, cool it to room temperature and take out the material, which is the recyclable thermosetting material P-M1. 100 -s-DCPD 2000 .

[0053] In addition, a recyclable thermosetting material P-M1 was prepared 100 -s-DCPD 1000 The TGA test results are as follows Figure 1 shown.

[0054] Example 3

[0055] The operation method is the same as that of Example 2, using 26.5 g of DCPD and 5 g of 7-oxo-2,3-diazanorbornene monomer M1 to obtain polymer P-M1 200 -s-DCPD 2000 .

[0056] Example 4

[0057] The operation method is the same as that of Example 2, using 26.5 g DCPD and 10 g 7-oxo-2,3-diazanorbornene monomer M1 to obtain polymer P-M1 400 -s-DCPD 2000 .

[0058] Example 5

[0059] The operation method is the same as that of Example 2, using 26.5 g of DCPD and 5 g of 7-oxo-2,3-diazanorbornene monomer M2 to obtain polymer P-M2 200 -s-DCPD 2000 In addition, P-M2 was prepared by increasing the amount of monomer M2 to 10 g. 400 -s-DCPD 2000 .

[0060] Example 6

[0061] The operation method is the same as that of Example 2, using 26.5 g of DCPD and 7.5 g of 7-oxo-2,3-diazanorbornene monomer M3 to obtain polymer P-M3 200 -s-DCPD 2000 In addition, P-M3 was prepared by increasing the amount of monomer M3 to 15 g. 400 -s-DCPD 2000 .

[0062] Example 7

[0063] The operation method is the same as that of Example 2, using 26.5 g DCPD and 6.0 g 7-oxo-2,3-diazanorbornene monomer M4 to obtain polymer P-M4 400 -s-DCPD 2000 .

[0064] Comparative Example 1

[0065] Under room temperature and air conditions, 26.5 g DCPD was added to the reaction bottle, and the toluene solution of G2 catalyst was added under vigorous stirring. The reaction was continued for 2 minutes, and then transferred to a mold for finalization and reacted at 90 ° C for 1.0 h to obtain a thermosetting polymer P-DCPD. 2000 Finally, cool it to room temperature and take out the material, which is the thermosetting material P-DCPD. 2000 .

[0066] Example 8

[0067] The thermosetting polymer P-M1 obtained in Example 2 200 -s-DCPD 2000 Soaked in THF, no degradation. Soaked in THF with acid (hydrochloric acid and TFA, respectively), degraded to a soluble polymer, see Figure 5 and Figure 6 The degradation and obtained polymers were analyzed by GPC, which verified that the molecular weight and distribution of the polymer fragments after degradation were M n =2.7 kDa, PDI = 2.3. Therefore, it can be confirmed that the thermosetting polymer P-M1 200 -s-DCPD 2000 The degradation yielded P-DCPD polymer fragments.

[0068] The thermosetting polymer P-DCPD obtained in Comparative Example 1 2000 There was no degradation when immersed in the same THF and acidic THF as above.

[0069] Example 9

[0070] The polymers obtained in Examples 2-7 and Comparative Example 1 were subjected to DSC analysis, confirming that their glass transition temperatures can be regulated according to the types and amounts of the added degradable monomers M1, M2, M3 and M4 ( Figure 3 and 4 ).

[0071] The above is an explanation of the embodiments of the present invention. However, the present invention is not limited to the above embodiments. Any modification, equivalent replacement, improvement, etc. made within the spirit and principle of the present invention shall be included in the protection scope of the present invention.

Claims

1. Cross-linked polymer P-MX-DCPD based on 7-oxo-2,3-diazanorbornene monomer MX and DCPD: in, R 1 , R 2 The same or different, independently selected from C 1-12 Alkyl, C 1-12 Alkoxy chain formed by replacing 1 to 6 carbon atoms on the alkyl group with oxygen, -(CH2) p C 6-20 Aryl, p is an integer >=0.

2. The cross-linked polymer P-MX-DCPD according to claim 1, characterized in that The cross-linked polymer P-MX-DCPD structure is shown below: R 1 , R 2 It has the definition as claimed in claim 1; (x+y), z are the same or different and are independently an integer of 2-200000.

3. The cross-linked polymer P-MX-DCPD according to claim 2, characterized in that R 1 , R 2 The same or different, independently selected from C 1-6 Alkyl, C 1-6 Alkoxy chain formed by replacing 1 to 3 carbon atoms on the alkyl group with oxygen, -(CH2) p C 6-12 Aryl, p is an integer of 1-6; (x+y), z are the same or different and are independently an integer of 10-20000.

4. The cross-linked polymer P-MX-DCPD according to claim 3, characterized in that R 1 , R 2 is the same and is selected from methyl, ethyl, propyl, isopropyl, benzyl, butyl, isobutyl or tert-butyl.

5. The cross-linked polymer P-MX-DCPD according to any one of claims 1 to 4, characterized in that The cross-linked polymer P-MX-DCPD has the following structure: wherein (x+y), z are the same or different and are independently 50, 100, 150, 200, 250, 300, 350, 400, 450, 500, 550, 600, 650, 700, 1000 or 2000.

6. The method for preparing the cross-linked polymer P-MX-DCPD according to any one of claims 1 to 4, characterized in that: The steps include: 7-Oxo-2,3-diazanorbornene monomer MX and DCPD undergo cross-linking polymerization reaction under the action of ruthenium complex catalyst.

7. The preparation method according to claim 6, characterized in that: The cross-linked polymer reaction is:

8. The method for degrading the cross-linked polymer P-MX-DCPD according to any one of claims 1 to 5, characterized in that: The steps include: The cross-linked polymer P-MX-DCPD degrades under acidic conditions.

9. The degradation method according to claim 8, characterized in that: The acidic condition is provided by hydrochloric acid or trifluoroacetic acid.

10. Use of the cross-linked polymer P-MX-DCPD according to any one of claims 1 to 5 in the preparation of high-strength thermosetting materials, wherein the high-strength thermosetting materials are mainly used in the fields of construction materials, vehicles, aerospace, electrical and electronic equipment or sports equipment.

Citation Information

Patent Citations

  • Copolymerization of dicyclopentadiene with norbornene derivative and copolymers obtainable therewith

    CN1042920A

  • Norbornene-based ring-opening polymerization polymer, product of hydrogenation of norbornene-based ring-opening polymerization polymer, and processes for producing these

    CN1659205A

  • New norbornenyl and 7-oxa- or 7-aza-bicyclo(2.2.1(hept-2-enyl N-heterocyclic compounds are useful as intermediates for active materials or other organic fine chemicals and in homo- and co-polymer production

    DE10006694A1