Surface-porous degradable composite microsphere and preparation method thereof
By combining bioactive glass with materials such as polylactic acid, surface porous degradable composite microspheres are prepared, which solves the acidic environment problem caused by the rapid degradation of polylactic acid materials, promotes tissue regeneration and cell adhesion, and expands its application in biology. Applications in the medical field.
Patent Information
- Application Number
- CN202411009837.2
- Authority / Receiving Office
- CN · China
- Patent Type
- Applications(China)
- Current Assignee / Owner
- Filing Date
- 2024-07-26
- Publication Date
- 2024-10-15
- Estimated Expiration
- Not applicable · inactive patent
AI Technical Summary
The rapid degradation of polylactic acid and its derivative materials in the biomedical field results in a local acidic microenvironment, which affects cell activity and tissue regeneration and repair, and its insufficient cell adhesion limits its application.
Bioactive glass is combined with degradable polymer materials, and surface porous degradable composite microspheres are prepared through stirring and freeze-drying methods. The bioactive glass neutralizes the acidic environment and promotes tissue regeneration, while improving cell adhesion.
It effectively neutralizes the acidic environment produced by the degradation of degradable polymer materials, promotes tissue regeneration, improves cell adhesion and migration conditions, and expands the application scope of composite microspheres.
Smart Images

Figure CN118772449A_ABST
Abstract
Description
Technical Field
[0001] The present invention relates to the technical field of biomedical materials, and more particularly to a porous and degradable composite microsphere and a preparation method thereof. Background Art
[0002] Polylactic acid and its derivatives are biodegradable polymer materials with good biocompatibility, which are widely used in the biomedical field. For example, it is used as a scaffold material in the field of tissue engineering to provide support and guidance for the generation of new tissues, and has application research in the fields of skin, bones and blood vessels. Another example is that it is used in the field of medical beauty filling as a core component of injectable fillers, which stimulates the regeneration of collagen to provide a lasting filling effect and improve skin sagging and wrinkles. In surgical sutures, its absorbable and degradable properties are used to avoid the pain caused to patients by secondary suture removal.
[0003] Although polylactic acid and its derivative materials have shown application diversity and potential in the biomedical field, the local acidic microenvironment caused by their rapid degradation may irritate surrounding tissues, affect cell activity, and may even cause long-term inflammatory responses, which is not conducive to tissue regeneration and repair.
[0004] Therefore, how to develop a surface porous degradable composite microsphere and a preparation method thereof to solve the acidic microenvironment caused by excessive degradation of polylactic acid and its derivative materials while improving cell adhesion is an urgent problem to be solved by those skilled in the art. Summary of the invention
[0005] In view of this, the present invention provides a surface porous degradable composite microsphere and a preparation method thereof.
[0006] In order to achieve the above object, the present invention adopts the following technical solution:
[0007] A method for preparing surface porous and degradable composite microspheres comprises the following steps:
[0008] (1) dissolving polyvinyl alcohol (PVA) in pure water to obtain an aqueous solution;
[0009] (2) adding the degradable polymer material and the bioactive glass into dichloromethane in sequence to obtain an oil phase solution;
[0010] (3) adding the oil phase solution into the water phase solution under stirring conditions, stirring sufficiently, washing with pure water, and freeze-drying to obtain surface porous and degradable composite microspheres.
[0011] Beneficial effects of the present invention: The present invention prepares surface porous degradable composite microspheres by introducing bioactive glass, a degradable material with good biological activity, into degradable polymer materials. The bioactive glass provides an alkaline environment to neutralize the acidic microenvironment produced by the degradation of the degradable polymer materials, thereby providing good conditions for tissue regeneration. At the same time, active ions such as silicon, calcium, and phosphorus released by the bioactive glass also help promote tissue regeneration. On the other hand, the porous structure of the surface of the surface porous degradable composite microspheres prepared by the present invention provides favorable conditions for the adhesion and migration of tissue cells. At the same time, the microspheres provide the possibility of developing injection products, further expanding the application scope of the surface porous degradable composite microspheres.
[0012] Furthermore, in step (1), the mass ratio of polyvinyl alcohol to water in the aqueous phase solution is (0.5-1):100.
[0013] The beneficial effect of adopting the above further technical solution is: through the surfactant effect of polyvinyl alcohol, the oil phase microspheres are stably present in the aqueous phase solution, and the generated surface porous and degradable composite microspheres have better dispersibility.
[0014] Furthermore, in step (2), the degradable polymer material is polylactic acid or / and polylactic acid-glycolic acid copolymer, the molecular weight range of the degradable polymer material is 3 to 10 KDa, and the mass ratio of the degradable polymer material to dichloromethane in the oil phase solution is (5 to 10):100.
[0015] The beneficial effect of adopting the above further technical solution is that the degradable polymer material is dissolved in the oil phase solution to form the main material of the porous and degradable composite microspheres.
[0016] Furthermore, in step (2), the bioactive glass is composed of a ternary system of SiO2-CaO-P2O5, with the mass percentage contents being 56% to 62%, 27% to 33%, and 5% to 12%, respectively, and the particle size range is D10>1μm, D50=2 to 6μm, and D90<10μm. The amount of bioactive glass added is 2% to 10% of the mass of the degradable polymer material.
[0017] The beneficial effects of adopting the above further technical solution are: realizing the construction of a porous structure on the surface of the composite microspheres, and neutralizing the acidic environment generated by the degradation of the degradable polymer material.
[0018] Furthermore, the mass ratio of the oil phase solution to the water phase solution is 1:(5-7).
[0019] The beneficial effect of adopting the above further technical solution is that the prepared surface porous degradable composite microspheres have a higher roundness.
[0020] Furthermore, in step (3), the stirring speed is 200 to 800 rpm.
[0021] The beneficial effect of adopting the above further technical solution is that the particle size of the prepared surface porous degradable composite microspheres is less than 300 μm.
[0022] Furthermore, in step (3), the vacuum degree of freeze drying is <5 Pa, the temperature of freeze drying is -45°C, and the time of freeze drying is 48 hours.
[0023] The beneficial effect of adopting the above further technical solution is that the prepared surface porous degradable composite microspheres have better dispersibility.
[0024] The present invention also provides a surface porous degradable composite microsphere prepared by the above method, characterized in that the particle size of the surface porous degradable composite microsphere is less than 300 μm, the surface has a porous structure, and the pore size range is 1 to 10 μm.
[0025] Beneficial effects of the present invention: The present invention uses bioactive glass as one of the components of the composite microspheres, which neutralizes the local acidic environment caused by excessive degradation of degradable polymer materials and provides more favorable conditions for tissue regeneration.
[0026] Another purpose of the present invention is to add bioactive glass materials and utilize the tissue regeneration and repair effect brought about by the ion release thereof, so as to be more conducive to tissue regeneration.
[0027] The present invention also constructs composite microspheres with a porous surface structure by adding bioactive glass materials. The porous surface structure is conducive to cell adhesion and migration, and has a promoting effect on tissue regeneration. The microspheres are conducive to expanding the application range of composite materials. BRIEF DESCRIPTION OF THE DRAWINGS
[0028] In order to more clearly illustrate the embodiments of the present invention or the technical solutions in the prior art, the drawings required for use in the embodiments or the description of the prior art will be briefly introduced below. Obviously, the drawings described below are only embodiments of the present invention. For ordinary technicians in this field, other drawings can be obtained based on the provided drawings without paying creative work.
[0029] Figure 1 The particle size distribution diagram of the bioactive glass used in Examples 1-3 of the present invention;
[0030] Figure 2 This is a particle size distribution diagram of the surface porous and degradable composite microspheres prepared in Example 1 of the present invention;
[0031] Figure 3Fourier transform infrared absorption spectrum of the surface porous and degradable composite microspheres prepared in Example 2 of the present invention;
[0032] Figure 4 This is a scanning electron microscope image of the surface porous and degradable composite microspheres prepared in Example 2 of the present invention.
[0033] Figure 5 This is a thermogravimetric curve of the surface porous and degradable composite microspheres prepared in Example 3 of the present invention.
[0034] Figure 6 This is a scanning electron microscope image of the smooth-surfaced polylactic acid microspheres prepared in Comparative Example 1 of the present invention. DETAILED DESCRIPTION
[0035] The following will be combined with the drawings in the embodiments of the present invention to clearly and completely describe the technical solutions in the embodiments of the present invention. Obviously, the described embodiments are only part of the embodiments of the present invention, not all of the embodiments. Based on the embodiments of the present invention, all other embodiments obtained by ordinary technicians in this field without creative work are within the scope of protection of the present invention.
[0036] Example 1
[0037] The method for preparing surface porous degradable composite microspheres comprises the following steps:
[0038] (1) dissolving 1.5 g of polyvinyl alcohol in 300 g of pure water to obtain an aqueous phase solution;
[0039] (2) adding 1 g of polylactic acid having a molecular weight of 3 to 5.5 KDa to 10 g of dichloromethane, stirring to completely dissolve it, and then adding 0.1 g of bioactive glass having a particle size range of D10 = 1.62 μm, D50 = 3.77 μm, and D90 = 6.39 μm, wherein the bioactive glass is composed of a SiO2-CaO-P2O5 ternary system, and the mass percentage contents are SiO2 = 62%, CaO = 33%, and P2O5 = 5%, respectively; stirring to fully disperse it, and obtaining an oil phase solution;
[0040] (3) Add 10 g of the oil phase solution to 70 g of the water phase solution under stirring conditions, continue stirring for 24 h, the stirring speed is 800 rpm, repeatedly wash with pure water, and freeze-dry for 48 h. The vacuum degree of freeze-drying is <5 Pa and the freeze-drying temperature is -45°C to obtain surface porous degradable composite microspheres with a particle size of <300 μm and a porous structure on the surface with a pore size range of 1 to 10 μm.
[0041] Example 2
[0042] The method for preparing surface porous degradable composite microspheres comprises the following steps:
[0043] (1) dissolving 9 g of polyvinyl alcohol in 900 g of pure water to obtain an aqueous phase solution;
[0044] (2) adding 7.5 g of polylactic acid with a molecular weight range of 5 to 10 KDa to 150 g of dichloromethane, stirring to completely dissolve it, and then adding 0.15 g of bioactive glass with a particle size range of D10 = 1.05 μm, D50 = 4.77 μm, and D90 = 8.55 μm, wherein the bioactive glass is composed of a SiO2-CaO-P2O5 ternary system, and the mass percentage contents are SiO2 = 56%, CaO = 32%, and P2O5 = 12% respectively; stirring to fully disperse it to obtain an oil phase solution;
[0045] (3) Add 12 g of the oil phase solution to 60 g of the water phase solution under stirring conditions, continue stirring for 24 h, the stirring speed is 400 rpm, repeatedly wash with pure water, and freeze-dry for 48 h. The vacuum degree of freeze-drying is <5 Pa and the freeze-drying temperature is -45°C to obtain surface porous biodegradable composite microspheres with a particle size of <300 μm and a porous structure on the surface with a pore size range of 1 to 10 μm.
[0046] Example 3
[0047] The method for preparing surface porous degradable composite microspheres comprises the following steps:
[0048] (1) dissolving 27.6 g of polyvinyl alcohol in 4.6 kg of pure water to obtain an aqueous phase solution;
[0049] (2) adding 56 g of polylactic acid-glycolic acid copolymer with a molecular weight range of 3 to 8 KDa to 750 g of dichloromethane, stirring to completely dissolve it, and then adding 4.48 g of bioactive glass with a particle size range of D10 = 1.62 μm, D50 = 3.77 μm, and D90 = 6.39 μm, wherein the bioactive glass is composed of a SiO2-CaO-P2O5 ternary system, and the mass percentage contents are SiO2 = 62%, CaO = 27%, and P2O5 = 11% respectively; stirring to fully disperse it to obtain an oil phase solution;
[0050] (3) Add 800 g of the oil phase solution to 4 kg of the water phase solution under stirring conditions, continue stirring for 24 hours, the stirring speed is 200 rpm, repeatedly wash with pure water, and freeze-dry for 48 hours. The vacuum degree of freeze-drying is <5 Pa and the freeze-drying temperature is -45°C to obtain surface porous degradable composite microspheres with a particle size of <300 μm and a porous structure on the surface with a pore size range of 1 to 10 μm.
[0051] Comparative Example 1
[0052] In order to demonstrate the technical effects of the preparation method of the present invention and the prepared surface porous degradable composite microspheres, in this comparative example, the existing polylactic acid preparation technology is used to prepare polylactic acid microspheres, including the following steps:
[0053] (1) dissolving 0.6 g of polyvinyl alcohol in 100 g of pure water to obtain an aqueous solution;
[0054] (2) adding 1.5 g of polylactic acid having a molecular weight range of 3 to 5 kDa into 20 g of dichloromethane and stirring to completely dissolve the polylactic acid to obtain an oil phase solution;
[0055] (3) Add 10 g of the oil phase solution to 60 g of the water phase solution under stirring conditions, continue stirring for 24 h, and the stirring speed is 600 rpm. Repeatedly wash with pure water and dry at 35° C. for 48 h to obtain polylactic acid microspheres with a particle size of less than 300 μm and a smooth surface.
[0056] The above description of the disclosed embodiments enables one skilled in the art to implement or use the present invention. Various modifications to these embodiments will be apparent to one skilled in the art, and the general principles defined herein may be implemented in other embodiments without departing from the spirit or scope of the present invention. Therefore, the present invention will not be limited to the embodiments shown herein, but rather to the widest scope consistent with the principles and novel features disclosed herein.
Claims
1. A method for preparing surface porous and degradable composite microspheres, characterized in that: The following steps are involved: (1) dissolving polyvinyl alcohol in pure water to obtain an aqueous solution; (2) adding the degradable polymer material and the bioactive glass into dichloromethane in sequence to obtain an oil phase solution; (3) adding the oil phase solution into the water phase solution under stirring conditions, stirring sufficiently, washing with pure water, and freeze-drying to obtain surface porous and degradable composite microspheres.
2. The method for preparing a surface porous and degradable composite microsphere according to claim 1, characterized in that: In step (1), the mass ratio of polyvinyl alcohol to water in the aqueous phase solution is (0.5-1):
100.
3. The method for preparing a surface porous and degradable composite microsphere according to claim 1, characterized in that: In step (2), the degradable polymer material is polylactic acid or / and polylactic acid-glycolic acid copolymer, the molecular weight range of the degradable polymer material is 3 to 10 KDa, and the mass ratio of the degradable polymer material to dichloromethane in the oil phase solution is (5 to 10):
100.
4. The method for preparing a surface porous and degradable composite microsphere according to claim 1, characterized in that: In step (2), the bioactive glass is composed of a ternary system of SiO2-CaO-P2O5, with the mass percentage contents being 56% to 62%, 27% to 33%, and 5% to 12% respectively, and the particle size range is D10>1μm, D50=2 to 6μm, and D90<10μm. The amount of bioactive glass added is 2% to 10% of the mass of the degradable polymer material.
5. The method for preparing a surface porous and degradable composite microsphere according to claim 1, characterized in that: The mass ratio of the oil phase solution to the water phase solution is 1:(5-7).
6. The method for preparing a surface porous and degradable composite microsphere according to claim 1, characterized in that: In step (3), the stirring speed is 200 to 800 rpm.
7. The method for preparing a surface porous and degradable composite microsphere according to claim 1, characterized in that: In step (3), the vacuum degree of freeze drying is <5 Pa, the temperature of freeze drying is -45°C, and the time of freeze drying is 48 hours.
8. A surface porous and degradable composite microsphere prepared by the method according to any one of claims 1 to 7, characterized in that: The particle size of the surface porous degradable composite microsphere is less than 300 μm, and the surface has a porous structure with a pore size ranging from 1 to 10 μm.