Composite conductive adhesive as well as preparation method and application thereof

By using a combination of conductive particles and a resin matrix with inorganic additives, carbon black, coupling agents and dispersants in the composite conductive adhesive, the problems of insufficient conductivity and weather resistance in the existing technology are solved and high conductivity is achieved , low-cost and low-curing temperature composite conductive adhesive, suitable for low-temperature ceramic chip packaging.

CN118772803APending Publication Date: 2024-10-15SHANGHAI XINTAO MICRO NEW MATERIALS CO LTD
View PDF 0 Cites 1 Cited by

Patent Information

Application Number
CN202411043866.0
Authority / Receiving Office
CN · China
Patent Type
Applications(China)
Current Assignee / Owner
Filing Date
2024-07-31
Publication Date
2024-10-15

AI Technical Summary

Technical Problem

It is difficult to develop a composite conductive adhesive with good conductivity, simple preparation process, low cost and excellent weather resistance and corrosion resistance with the existing technology.

Method used

It adopts a combination of resin matrix and conductive particles. The conductive particles are made of inorganic additives, carbon black, coupling agent and dispersant through spray granulation to ensure the uniform dispersion of carbon black and control the proportion of components to achieve high conductivity and adhesion. properties while lowering the curing temperature.

Benefits of technology

A composite conductive adhesive with good conductivity, strong adhesion, low cost and can be cured below 300°C has been realized. It has excellent weather resistance and corrosion resistance and is suitable for low-temperature ceramic chip packaging technology.

✦ Generated by Eureka AI based on patent content.

Smart Images

  • Figure BDA0004973003550000131
    Figure BDA0004973003550000131
  • Figure BDA0004973003550000141
    Figure BDA0004973003550000141
Patent Text Reader

Abstract

The invention provides a composite conductive adhesive as well as a preparation method and application thereof. The composite conductive adhesive comprises a resin matrix and conductive particles, the conductive particles comprise the following components in percentage by mass: 68%-95% of an inorganic additive, 3%-30% of carbon black, 0.5%-2% of a coupling agent and 0.5%-1.5% of a dispersing agent; the conductive particles are prepared by spray granulation of a suspension with a particle size of 100-300 nm. The composite conductive adhesive provided by the invention is good in conductivity, good in cohesiveness, low in preparation cost, low in curing temperature and excellent in weather resistance and corrosion resistance.
Need to check novelty before this filing date? Find Prior Art

Description

Technical Field

[0001] The invention belongs to the technical field of conductive adhesives, and in particular relates to a composite conductive adhesive and a preparation method and application thereof. Background Art

[0002] Composite conductive adhesives are mainly composed of main components, conductive fillers, toughening agents, solvents and other additives. Among them, conductive fillers are the key to achieving conductive properties of conductive adhesives. Common conductive fillers include precious metal conductive powders such as gold and silver. Cheap metal conductive powders such as copper, aluminum, and iron are rarely used in conductive adhesives due to their instability. Carbon materials such as carbon black are very excellent conductive materials with stable properties, but due to their light weight and difficulty in dispersion, they are rarely used as conductive fillers in conductive adhesives.

[0003] CN102079847A discloses a photosensitive silver paste conductive adhesive and a preparation method thereof. The photosensitive silver paste conductive adhesive is composed of a photosensitive resin, conductive particles, a dispersant, a photoinitiator, an antioxidant, and a defoaming agent. Isobornyl acrylate is used as a dispersant, and micron silver powder, nano silver powder and silver-plated glass powder are used as conductive particles; a silane coupling agent is used as a nano silver dispersant; benzoin ether is used as a photoinitiator; p-hydroxyanisole is used as an antioxidant, and dibutyl phosphate is used as a defoaming agent. The weight percentage of photosensitive resin, conductive particles, dispersant, photoinitiator, antioxidant and defoaming agent is as follows: 15-30 parts of photosensitive resin, 60-80 parts of conductive particles, 0.1-2 parts of dispersant, 0.5-2.0 parts of photoinitiator, 0.1-1.0 parts of antioxidant and 0.5-5 parts of defoaming agent. The photosensitive silver paste conductive adhesive provided by the technical solution has good UV curing performance and has the advantages of low resistivity and good mechanical properties compared with traditional conductive adhesives. However, the micron silver powder and nano silver powder used are expensive.

[0004] CN109517562A discloses a ceramic conductive adhesive for electronic packaging and a preparation method thereof, wherein the ceramic conductive adhesive for electronic packaging uses titanium diboride ceramic powder as the main conductive filler of the conductive adhesive, prepares a composite hydrogel by cross-linking hydroxylated titanium diboride and carboxylated graphene oxide, reduces the graphene oxide, freeze-dries to obtain a composite aerogel powder, and then coats the aerogel powder with succinic acid-modified silver nanowires, and finally mixes evenly with bisphenol A epoxy resin, dimethyl phthalate, acetone, nano titanium dioxide, 2-methylimidazole, and liquid silicone rubber to obtain a ceramic conductive adhesive. This technical solution significantly reduces the volume resistivity of the titanium diboride ceramic conductive adhesive and improves the conductivity by cross-linking and coating modification of titanium diboride, but the preparation process is complicated.

[0005] Therefore, it is necessary to develop a composite conductive adhesive with good conductivity, simple preparation process, low cost, and excellent weather resistance and corrosion resistance. Summary of the invention

[0006] In view of the shortcomings of the prior art, the present invention aims to provide a composite conductive adhesive and its preparation method and application. The composite conductive adhesive has good conductivity, good adhesion, low preparation cost, low curing temperature, and excellent weather resistance and corrosion resistance.

[0007] To achieve this object, the present invention adopts the following technical solutions:

[0008] In a first aspect, the present invention provides a composite conductive adhesive, the composite conductive adhesive comprising a resin matrix and conductive particles;

[0009] The conductive particles include the following components by mass percentage: 68%-95% (e.g., 70%, 73%, 76%, 79%, 82%, 85%, 88%, 91% or 94%) of inorganic additives, 3%-30% (e.g., 6%, 9%, 12%, 15%, 18%, 21%, 24% or 27%) of carbon black, 0.5%-2% (e.g., 0.7%, 0.9%, 1.1%, 1.3%, 1.5%, 1.7% or 1.9%) of coupling agents and 0.5%-1.5% (e.g., 0.6%, 0.7%, 0.8%, 0.9%, 1.0%, 1.1%, 1.2%, 1.3% or 1.4%) of dispersants.

[0010] The conductive particles are prepared by spray granulation of a suspension with a particle size of 100-300 nm (eg, 120 nm, 140 nm, 160 nm, 180 nm, 200 nm, 220 nm, 240 nm, 260 nm or 280 nm, etc.).

[0011] The present invention adds carbon black with stable performance and excellent conductive effect into the composite conductive adhesive, and prepares conductive particles by combining inorganic additives, carbon black, coupling agent and dispersant, and then mixes the conductive particles with components such as resin matrix, thereby overcoming the characteristic that carbon black is not easy to disperse, achieving uniform dispersion of carbon black in the composite conductive adhesive, and preparing a composite conductive adhesive with good conductivity, low preparation cost, low curing temperature, curing below 300°C, excellent weather resistance and corrosion resistance, and stable properties.

[0012] In the present invention, the inorganic additives adhere to the conductive carbon black by micro-melting during the granulation process, the coupling agent and the dispersant are conducive to the uniform dispersion of the carbon black and the inorganic additives during the mixing process, and the prepared composite conductive adhesive has high strength, weather resistance and conductivity by controlling the mass percentage of each component in the conductive particles within a specific range. If the mass percentage of carbon black is too small, the conductivity of the prepared composite conductive adhesive is extremely low; if the mass percentage of carbon black is too large, the bonding force of the prepared composite conductive adhesive is seriously reduced.

[0013] In the present invention, the particle size of the suspension refers to the average particle size of particles contained in the suspension.

[0014] Preferably, the inorganic additive includes lead oxide.

[0015] Preferably, the inorganic additive further comprises any one of potassium oxide, boron oxide, sodium oxide, silicon oxide or gypsum powder, or a combination of at least two thereof.

[0016] Preferably, the inorganic additives include the following components in parts by mass: 100 parts of lead oxide, 0-90 parts of potassium oxide (for example, 15 parts, 25 parts, 35 parts, 45 parts, 55 parts, 65 parts, 75 parts or 85 parts, etc.), 0-80 parts of boron oxide (for example, 5 parts, 15 parts, 25 parts, 35 parts, 45 parts, 55 parts, 65 parts or 75 parts, etc.), 0-80 parts of sodium oxide (for example, 5 parts, 15 parts, 25 parts, 35 parts, 45 parts, 55 parts, 65 parts or 75 parts, etc.), 0-60 parts of silicon oxide (for example, 5 parts, 15 parts, 25 parts, 35 parts, 45 parts or 55 parts, etc.) and 0-30 parts of gypsum powder (for example, 3 parts, 6 parts, 9 parts, 12 parts, 15 parts, 17 parts, 20 parts, 23 parts, 25 parts or 28 parts, etc.).

[0017] Preferably, the inorganic additives include the following components in parts by mass: 100 parts of lead oxide, 60-80 parts of potassium oxide (for example, 63 parts, 66 parts, 69 parts, 72 parts, 75 parts or 78 parts, etc.), 50-60 parts of boron oxide (for example, 52 parts, 54 parts, 56 parts, 58 parts or 59 parts, etc.), 40-50 parts of sodium oxide (for example, 42 parts, 44 parts, 46 parts, 48 ​​parts or 49 parts, etc.), 10-20 parts of silicon oxide (for example, 12 parts, 14 parts, 16 parts, 18 parts or 19 parts, etc.) and 10-20 parts of gypsum powder (for example, 12 parts, 14 parts, 16 parts, 18 parts or 19 parts, etc.).

[0018] Preferably, the coupling agent comprises a silane coupling agent.

[0019] Preferably, the silane coupling agent includes vinyltriethoxysilane.

[0020] Preferably, the dispersant comprises an anionic dispersant and / or a nonionic dispersant.

[0021] Preferably, the anionic dispersant comprises sodium dodecylbenzenesulfonate and / or dodecylamine acetate.

[0022] Preferably, the nonionic dispersant comprises alkylphenol polyoxyethylene ether and / or fatty acid polyoxyethylene ester.

[0023] Preferably, the raw materials for preparing the resin matrix include epoxy-modified acrylic resin, methyl phenyl silicone resin and phenyl POSS.

[0024] Preferably, the raw materials for preparing the resin matrix include the following components in parts by mass: 100 parts of epoxy-modified acrylic resin, 50-90 parts of methylphenyl silicone resin (for example, 55 parts, 60 parts, 65 parts, 70 parts, 75 parts, 80 parts or 85 parts, etc.) and 30-60 parts of phenyl POSS (for example, 33 parts, 36 parts, 39 parts, 42 parts, 45 parts, 48 ​​parts, 51 parts, 54 parts or 57 parts, etc.).

[0025] Preferably, the resin matrix is ​​prepared by the following method: epoxy-modified acrylic resin, methylphenyl silicone resin and phenyl POSS are mixed at 65-75°C (for example, 66°C, 67°C, 68°C, 69°C, 70°C, 71°C, 72°C, 73°C or 74°C, etc.) for 0.5-3h (for example, 0.8h, 1h, 1.5h, 2h, 2.5h or 2.8h, etc.) to obtain the resin matrix.

[0026] Preferably, the composite conductive adhesive further includes a diluent, a curing agent and a curing accelerator.

[0027] Preferably, the diluent comprises styrene.

[0028] Preferably, the curing agent comprises methyl ethyl ketone peroxide.

[0029] Preferably, the curing accelerator is silica sol.

[0030] Preferably, the composite conductive adhesive includes the following components in parts by mass: 100 parts of a resin matrix, 30-50 parts of conductive particles (for example, 32 parts, 34 parts, 36 parts, 38 parts, 40 parts, 42 parts, 44 parts, 46 parts or 48 parts, etc.), 10-20 parts of a diluent (for example, 11 parts, 12 parts, 13 parts, 14 parts, 15 parts, 16 parts, 17 parts, 18 parts or 19 parts, etc.), 5-10 parts of a curing agent (for example, 5.5 parts, 6 parts, 6.5 parts, 7 parts, 7.5 parts, 8 parts, 8.5 parts, 9 parts or 9.5 parts, etc.) and 2-5 parts of a curing accelerator (for example, 2.3 parts, 2.6 parts, 2.9 parts, 3.2 parts, 3.5 parts, 3.8 parts, 4.1 parts, 4.4 parts or 4.7 parts, etc.).

[0031] In the present invention, by controlling the mass fraction of the conductive particles in the composite conductive adhesive within a specific range, the prepared composite conductive adhesive has higher strength and conductivity.

[0032] In a second aspect, the present invention provides a method for preparing the composite conductive adhesive as described in the first aspect, the preparation method comprising the following steps:

[0033] (1) mixing an inorganic additive, carbon black, a coupling agent and a dispersant, grinding to form a suspension having a particle size of 100-300 nm, and spraying granulation to obtain conductive particles;

[0034] (2) Mixing the resin matrix and the conductive particles obtained in step (1) to obtain the composite conductive adhesive.

[0035] Preferably, the step (1) specifically comprises the following steps:

[0036] (I) Lead oxide, potassium oxide, boron oxide, sodium oxide, silicon oxide and gypsum powder are mixed to obtain an inorganic additive.

[0037] (II) Carbon black is mixed with an aqueous solution containing a coupling agent and a dispersant to obtain a suspension A.

[0038] (III) The inorganic additive prepared in step (I) and the suspension A prepared in step (II) are mixed to obtain a suspension B.

[0039] (IV) Grinding the suspension B obtained in step (III) to obtain a suspension with a particle size of 100-300 nm.

[0040] (V) spraying and granulating the suspension with a particle size of 100-300 nm obtained in step (IV) to obtain the conductive particles.

[0041] The step (I) and step (II) are carried out step by step in no particular order, or simultaneously.

[0042] In the present invention, carbon black and other components are prepared into a suspension and ground to form a suspension with a particle size of 100-300nm, and then spray granulated to form conductive particles, thereby increasing the uniformity of carbon black dispersion and achieving uniform dispersion of carbon black in the composite conductive adhesive.

[0043] Preferably, the spray granulation is carried out in a centrifugal spray granulator, and the nozzle temperature of the centrifugal spray granulator is 100-150°C, for example, 105°C, 110°C, 115°C, 120°C, 125°C, 130°C, 135°C, 140°C or 145°C, etc.

[0044] Preferably, the mixing in step (2) further includes mixing with a diluent, a curing agent and a curing accelerator.

[0045] In a third aspect, the present invention provides a use of the composite conductive adhesive as described in the first aspect in preparing chip packaging.

[0046] Compared with the prior art, the present invention has the following beneficial effects:

[0047] In the present invention, carbon black with stable performance and excellent conductive effect is added to the composite conductive adhesive, and conductive particles are prepared by combining inorganic additives, carbon black, coupling agent, dispersant and glass powder, and then mixed with components such as resin matrix, thereby overcoming the characteristic that carbon black is not easy to disperse, achieving uniform dispersion of carbon black in the composite conductive adhesive, and preparing a composite conductive adhesive with good conductivity, surface resistivity of 12 to 2458Ω / □, good adhesion, low preparation cost, low curing temperature, curing below 300°C, excellent weather resistance and corrosion resistance, and stable properties. The composite conductive adhesive can meet the needs of low-temperature ceramic chip packaging technology. DETAILED DESCRIPTION

[0048] The technical solution of the present invention is further described below by specific implementation methods. It should be understood by those skilled in the art that the embodiments are only to help understand the present invention and should not be regarded as specific limitations of the present invention.

[0049] Some of the raw materials in the embodiments and comparative examples are derived from the following sources:

[0050] Silica sol, manufacturer: Yantai Hengxin Chemical Technology Co., Ltd., brand S-S30 silica sol;

[0051] Epoxy modified acrylic resin, manufacturer: Yingxin Laboratory, brand acrylic resin SS-22;

[0052] Methyl phenyl silicone resin, manufacturer: Japan Shin-Etsu, brand KR-112;

[0053] Phenyl POSS, manufacturer: Shanghai Yuanye Biotechnology Co., Ltd., brand number S47904.

[0054] Example 1

[0055] The present embodiment provides a composite conductive adhesive and a preparation method thereof, wherein the composite conductive adhesive includes the following components in parts by mass: 100 parts of a resin matrix, 30 parts of conductive particles, 10 parts of a diluent (styrene), 5 parts of a curing agent (methyl ethyl ketone peroxide), and 2 parts of a curing accelerator (silica sol).

[0056] The conductive particles include the following components by mass percentage: 92% of inorganic additives, 6% of carbon black, 1% of coupling agent (vinyl triethoxysilane) and 1% of dispersant (sodium dodecylbenzene sulfonate).

[0057] The inorganic additives include the following components by mass: 100 parts of lead oxide, 80 parts of potassium oxide, 50 parts of boron oxide, 50 parts of sodium oxide, 10 parts of silicon oxide and 10 parts of gypsum powder.

[0058] The resin matrix is ​​prepared by mixing 100 parts of epoxy-modified acrylic resin, 70 parts of methylphenyl silicone resin and 45 parts of phenyl POSS at 70° C. for 0.5 h.

[0059] The preparation method of the composite conductive adhesive is as follows:

[0060] (1) mixing lead oxide, potassium oxide, boron oxide, sodium oxide, silicon oxide and gypsum powder to obtain an inorganic additive;

[0061] A coupling agent, a dispersant and water are mixed (the ratio of the total mass of the dispersant and the coupling agent to the mass of water is 1:60) to form an aqueous solution of the coupling agent and the dispersant, and carbon black is mixed with the aqueous solution containing the coupling agent and the dispersant to obtain a suspension A;

[0062] The inorganic additive is mixed with the suspension A to obtain a suspension B;

[0063] The suspension B is ground to control the particle size at 135 nm to obtain a suspension with a particle size of 135 nm;

[0064] The suspension with a particle size of 135 nm was sprayed and granulated by a centrifugal spray granulator with a nozzle temperature of 130° C. to obtain the conductive particles.

[0065] (2) Mixing a resin matrix, the conductive particles obtained in step (1), a diluent, a curing agent and a curing accelerator to obtain the composite conductive adhesive.

[0066] Example 2

[0067] The present embodiment provides a composite conductive adhesive and a preparation method thereof, wherein the composite conductive adhesive includes the following components in parts by mass: 100 parts of a resin matrix, 50 parts of conductive particles, 20 parts of a diluent (styrene), 10 parts of a curing agent (methyl ethyl ketone peroxide), and 5 parts of a curing accelerator (silica sol).

[0068] The conductive particles include the following components by mass percentage: 91.5% of inorganic additives, 6% of carbon black, 2% of coupling agent (vinyl triethoxysilane) and 0.5% of dispersant (alkylphenol polyoxyethylene ether).

[0069] The inorganic additives include the following components by mass: 100 parts of lead oxide, 70 parts of potassium oxide, 55 parts of boron oxide, 45 parts of sodium oxide, 15 parts of silicon oxide and 15 parts of gypsum powder.

[0070] The resin matrix is ​​prepared by mixing 100 parts of epoxy-modified acrylic resin, 50 parts of methylphenyl silicone resin and 60 parts of phenyl POSS at 70° C. for 1 hour.

[0071] The preparation method of the composite conductive adhesive is as follows:

[0072] (1) mixing lead oxide, potassium oxide, boron oxide, sodium oxide, silicon oxide and gypsum powder to obtain an inorganic additive;

[0073] A coupling agent, a dispersant and water are mixed (the ratio of the total mass of the dispersant and the coupling agent to the mass of water is 1:100) to form an aqueous solution of the coupling agent and the dispersant, and carbon black is mixed with the aqueous solution containing the coupling agent and the dispersant to obtain a suspension A;

[0074] The inorganic additive is mixed with the suspension A to obtain a suspension B;

[0075] The suspension B is ground to control the particle size at 135 nm to obtain a suspension with a particle size of 135 nm;

[0076] The suspension with a particle size of 135 nm was sprayed and granulated by a centrifugal spray granulator with a nozzle temperature of 100° C. to obtain the conductive particles.

[0077] (2) Mixing a resin matrix, the conductive particles obtained in step (1), a diluent, a curing agent and a curing accelerator to obtain the composite conductive adhesive.

[0078] Example 3

[0079] The present embodiment provides a composite conductive adhesive and a preparation method thereof, wherein the composite conductive adhesive includes the following components in parts by mass: 100 parts of a resin matrix, 35 parts of conductive particles, 12 parts of a diluent (styrene), 6 parts of a curing agent (methyl ethyl ketone peroxide), and 3 parts of a curing accelerator (silica sol).

[0080] The conductive particles include the following components by mass percentage: 92% of inorganic additives, 6% of carbon black, 0.5% of coupling agent (vinyl triethoxysilane) and 1.5% of dispersant (sodium dodecylbenzene sulfonate).

[0081] The inorganic additives include the following components by mass: 100 parts of lead oxide, 60 parts of potassium oxide, 60 parts of boron oxide, 40 parts of sodium oxide, 20 parts of silicon oxide and 20 parts of gypsum powder.

[0082] The resin matrix is ​​prepared by mixing 100 parts of epoxy-modified acrylic resin, 90 parts of methylphenyl silicone resin and 30 parts of phenyl POSS at 70° C. for 3 hours.

[0083] The preparation method of the composite conductive adhesive is as follows:

[0084] (1) mixing lead oxide, potassium oxide, boron oxide, sodium oxide, silicon oxide and gypsum powder to obtain an inorganic additive;

[0085] A coupling agent, a dispersant and water are mixed (the ratio of the total mass of the dispersant and the coupling agent to the mass of water is 1:70) to form an aqueous solution of the coupling agent and the dispersant, and carbon black is mixed with the aqueous solution containing the coupling agent and the dispersant to obtain a suspension A;

[0086] The inorganic additive is mixed with the suspension A to obtain a suspension B;

[0087] The suspension B is ground to control the particle size at 135 nm to obtain a suspension with a particle size of 135 nm;

[0088] The suspension with a particle size of 135 nm was sprayed and granulated by a centrifugal spray granulator with a nozzle temperature of 150° C. to obtain the conductive particles.

[0089] (2) Mixing a resin matrix, the conductive particles obtained in step (1), a diluent, a curing agent and a curing accelerator to obtain the composite conductive adhesive.

[0090] Example 4

[0091] This embodiment provides a composite conductive adhesive and a preparation method thereof. The only difference between the present embodiment and the embodiment 1 is that the components of the inorganic additives are adjusted as follows. The inorganic additives include the following components by mass: 100 parts of lead oxide, 90 parts of potassium oxide, 40 parts of boron oxide, 35 parts of sodium oxide, 60 parts of silicon oxide or 30 parts of gypsum powder. Other conditions are the same as those in the embodiment 1.

[0092] Example 5

[0093] This embodiment provides a composite conductive adhesive and a preparation method thereof, which differs from Embodiment 1 only in that the composition of the inorganic additive is adjusted as follows, and the inorganic additive includes the following components by mass: 100 parts of lead oxide, 55 parts of potassium oxide, 80 parts of boron oxide and 80 parts of sodium oxide; in step (1), lead oxide, potassium oxide and boron oxide are mixed to obtain the inorganic additive, and other conditions are the same as those in Embodiment 1.

[0094] Example 6

[0095] This embodiment provides a composite conductive adhesive and a preparation method thereof. The difference between this embodiment and embodiment 1 is that the mass percentage of carbon black is adjusted to 3%, and other conditions are the same as those in embodiment 1.

[0096] Example 7

[0097] This embodiment provides a composite conductive adhesive and a preparation method thereof. The difference between this embodiment and embodiment 1 is that the mass percentage of carbon black is adjusted to 10%, and other conditions are the same as those in embodiment 1.

[0098] Example 8

[0099] This embodiment provides a composite conductive adhesive and a preparation method thereof. The difference between this embodiment and embodiment 1 is that the mass percentage of carbon black is adjusted to 30%, and other conditions are the same as those in embodiment 1.

[0100] Example 9

[0101] This embodiment provides a composite conductive adhesive and a preparation method thereof, which differs from Embodiment 1 only in that the grinding in step (1) is performed to control the particle size of the suspension C to 100 nm to obtain a suspension with a particle size of 100 nm, and other conditions are the same as those in Embodiment 1.

[0102] Example 10

[0103] This embodiment provides a composite conductive adhesive and a preparation method thereof, which differs from Embodiment 1 only in that the grinding in step (1) is performed to control the particle size of the suspension C to 300 nm, thereby obtaining a suspension with a particle size of 300 nm, and other conditions are the same as those in Embodiment 1.

[0104] Comparative Example 1

[0105] This comparative example provides a composite conductive adhesive and a preparation method thereof, which differs from Example 1 only in that the grinding step is not included in step (1), and the suspension B is sprayed and granulated by a centrifugal spray granulator, and other conditions are the same as those in Example 1.

[0106] Comparative Example 2

[0107] This comparative example provides a composite conductive adhesive and a preparation method thereof, which is different from Example 1 only in that the preparation method of the composite conductive adhesive is adjusted as follows:

[0108] (1) mixing lead oxide, potassium oxide, boron oxide, sodium oxide, silicon oxide and gypsum powder to obtain an inorganic additive;

[0109] The coupling agent, the dispersant and water are mixed (the ratio of the total mass of the dispersant and the coupling agent to the mass of water is 1:60) to form an aqueous solution of the coupling agent and the dispersant.

[0110] (2) Mixing a resin matrix, the inorganic additive obtained in step (1), an aqueous solution of a coupling agent and a dispersant obtained in step (1), carbon black, a diluent, a curing agent and a curing accelerator to obtain the composite conductive adhesive.

[0111] Other conditions are the same as in Example 1.

[0112] Comparative Example 3

[0113] This comparative example provides a composite conductive adhesive and a preparation method thereof, which is different from Example 1 only in that the carbon black is replaced with copper powder of the same mass, and the rest is the same as Example 1.

[0114] Comparative Example 4

[0115] This comparative example provides a composite conductive adhesive and a preparation method thereof, which is different from Example 1 only in that the mass percentage of carbon black is adjusted to 2%, and other conditions are the same as those of Example 1.

[0116] Comparative Example 5

[0117] This comparative example provides a composite conductive adhesive and a preparation method thereof, which is different from Example 1 only in that the mass percentage of carbon black is adjusted to 35%, and other conditions are the same as those of Example 1.

[0118] Comparative Example 6

[0119] This comparative example provides a composite conductive adhesive and a preparation method thereof, which differs from Example 1 only in that the grinding in step (1) is performed to control the particle size of the suspension C to 350 nm to obtain a suspension with a particle size of 350 nm, and other conditions are the same as those in Example 1.

[0120] The performance of the composite conductive adhesive provided in the above embodiments and comparative examples was tested, and the specific testing method is as follows:

[0121] Conductivity: The composite conductive adhesive was coated on a glass sheet and cured at 280°C for 60 minutes to make a sample. The plane resistance of the cured composite conductive adhesive was tested with a four-probe tester. Using a constant current source and a voltmeter, four microprobes were set on the surface of the sample, a constant current was passed, and the voltage value was measured to calculate the surface resistivity.

[0122] Bond strength: The bond strength of the adhesive is evaluated by applying a tensile force at a rate of 5 mm / min. The specific operations include: a. Prepare the test sample: evenly apply the composite conductive adhesive on the contact surface of two specimens (alumina ceramic plates) and cure them at 280°C for 60 minutes to bond the two specimens. b. Fix one end of the two specimens bonded together and apply a tensile force to the other end. c. Calculate the bond strength of the composite conductive adhesive by measuring the maximum value of the applied tensile force.

[0123] Weather resistance: a. Prepare the test sample: evenly apply the composite conductive adhesive on the contact surface of two samples (alumina ceramic plates) and cure at 280℃ for 60 minutes to bond the two samples; b. Place the test sample in a reactor, add deionized water to cover the sample, and boil the reactor at 120℃ for 24 hours. c. Take out the sample, dry it, and then conduct a conductivity test. If the resistance change before and after boiling is ≤10%, it is passed, otherwise it is failed; then conduct an adhesion test. If the adhesion is ≥30Mpa, it is passed, otherwise it is failed. If both the conductivity test and the adhesion strength test are passed, the weather resistance test result is passed, otherwise it is failed.

[0124] The test results of the composite conductive adhesives provided in the above embodiments and comparative examples are shown in Table 1 below.

[0125] Table 1

[0126]

[0127]

[0128] According to the test results in Table 1, the surface resistivity of the composite conductive adhesive provided in Examples 1-10 is 12-2458Ω / □, and has excellent weather resistance.

[0129] Compared with Example 1, the bonding force of the composite conductive adhesives obtained in Example 4 and Example 5 is reduced, which shows that the inorganic additives include the following components in parts by mass: 100 parts of lead oxide, 60-80 parts of potassium oxide, 50-60 parts of boron oxide, 40-50 parts of sodium oxide, 10-20 parts of silicon oxide and 10-20 parts of gypsum powder, and the obtained composite conductive adhesive has better performance.

[0130] Compared with Example 1, if step (1) does not include the grinding step (Comparative Example 1), the weather resistance test cannot be passed.

[0131] Compared with Example 1, if carbon black is directly mixed with components such as the resin matrix (Comparative Example 2), the conductivity is extremely poor and the weather resistance test cannot be passed.

[0132] Compared with Example 1, if the carbon black is replaced with the same mass of copper powder (Comparative Example 3), the conductivity is seriously reduced.

[0133] Compared with Example 1, if the mass percentage of carbon black is too small (Comparative Example 4), the conductivity will drop sharply; if the mass percentage of carbon black is too large (Comparative Example 5), the weather resistance test cannot be passed. It can be seen that the composite conductive adhesive obtained by controlling the mass percentage of carbon black within a specific range has better performance.

[0134] Comparing Example 1 with Comparative Example 6, if the ground particle size is too large, the particle size of the obtained conductive particles is too large, and the weather resistance test cannot be passed. It can be seen that the composite conductive adhesive obtained by making conductive particles from a suspension with a particle size of 100-300nm has better performance.

[0135] The applicant declares that the present invention uses the above-mentioned embodiments to illustrate a composite conductive adhesive and its preparation method and application, but the present invention is not limited to the above-mentioned embodiments, that is, it does not mean that the present invention must rely on the above-mentioned embodiments to be implemented. Those skilled in the art should understand that any improvement of the present invention, equivalent replacement of various raw materials of the product of the present invention, addition of auxiliary components, selection of specific methods, etc., all fall within the protection scope and disclosure scope of the present invention.

Claims

1. A composite conductive adhesive, It is characterized in that The composite conductive adhesive comprises a resin matrix and conductive particles; The conductive particles include the following components by mass percentage: 68%-95% of inorganic additives, 3%-30% of carbon black, 0.5%-2% of coupling agent and 0.5%-1.5% of dispersant; The conductive particles are prepared by spraying granulation of a suspension with a particle size of 100-300nm.

2. The composite conductive adhesive according to claim 1, It is characterized in that The inorganic additive includes lead oxide; Preferably, the inorganic additive further comprises any one or a combination of at least two of potassium oxide, boron oxide, sodium oxide, silicon oxide or gypsum powder; Preferably, the inorganic additives include the following components by mass: 100 parts of lead oxide, 0-90 parts of potassium oxide, 0-80 parts of boron oxide, 0-80 parts of sodium oxide, 0-60 parts of silicon oxide and 0-30 parts of gypsum powder.

3. The composite conductive adhesive according to claim 1 or 2, It is characterized in that The inorganic additives include the following components by mass: 100 parts of lead oxide, 60-80 parts of potassium oxide, 50-60 parts of boron oxide, 40-50 parts of sodium oxide, 10-20 parts of silicon oxide and 10-20 parts of gypsum powder; Preferably, the coupling agent comprises a silane coupling agent; Preferably, the silane coupling agent comprises vinyltriethoxysilane; Preferably, the dispersant comprises an anionic dispersant and / or a nonionic dispersant; Preferably, the anionic dispersant comprises sodium dodecylbenzenesulfonate and / or dodecyl acetate; Preferably, the nonionic dispersant comprises alkylphenol polyoxyethylene ether and / or fatty acid polyoxyethylene ester.

4. The composite conductive adhesive according to any one of claims 1 to 3, It is characterized in that The raw materials for preparing the resin matrix include epoxy modified acrylic resin, methyl phenyl silicone resin and phenyl POSS; Preferably, the raw materials for preparing the resin matrix include the following components by mass: 100 parts of epoxy-modified acrylic resin, 50-90 parts of methylphenyl silicone resin and 30-60 parts of phenyl POSS; Preferably, the resin matrix is ​​prepared by the following method: epoxy-modified acrylic resin, methylphenyl silicone resin and phenyl POSS are mixed at 65-75° C. for 0.5-3 h to obtain the resin matrix.

5. The composite conductive adhesive according to any one of claims 1 to 4, It is characterized in that The composite conductive adhesive also includes a diluent, a curing agent and a curing accelerator.

6. The composite conductive adhesive according to claim 5, It is characterized in that The diluent includes styrene; Preferably, the curing agent comprises methyl ethyl ketone peroxide; Preferably, the curing accelerator is silica sol.

7. The composite conductive adhesive according to any one of claims 1 to 6, It is characterized in that The composite conductive adhesive comprises the following components by mass: 100 parts of a resin matrix, 30-50 parts of conductive particles, 10-20 parts of a diluent, 5-10 parts of a curing agent and 2-5 parts of a curing accelerator.

8. A method for preparing the composite conductive adhesive according to any one of claims 1 to 7, It is characterized in that The preparation method comprises the following steps: (1) mixing an inorganic additive, carbon black, a coupling agent and a dispersant, grinding to form a suspension having a particle size of 100-300 nm, and spraying granulation to obtain conductive particles; (2) Mixing the resin matrix and the conductive particles obtained in step (1) to obtain the composite conductive adhesive.

9. The preparation method according to claim 8, It is characterized in that The step (1) specifically comprises the following steps: (I) mixing lead oxide, potassium oxide, boron oxide, sodium oxide, silicon oxide and gypsum powder to obtain an inorganic additive; (II) mixing carbon black with an aqueous solution containing a coupling agent and a dispersant to obtain a suspension A; (III) mixing the inorganic additive obtained in step (I) and the suspension A obtained in step (II) to obtain a suspension B; (IV) grinding the suspension B obtained in step (III) to obtain a suspension having a particle size of 100-300 nm; (V) spraying and granulating the suspension with a particle size of 100-300 nm obtained in step (IV) to obtain the conductive particles; The step (I) and step (II) are carried out in no particular order, or simultaneously; Preferably, the spray granulation is carried out in a centrifugal spray granulator, and the nozzle temperature of the centrifugal spray granulator is 100-150°C; Preferably, the mixing in step (2) further includes mixing with a diluent, a curing agent and a curing accelerator.

10. Use of the composite conductive adhesive according to any one of claims 1 to 7 in preparing chip packaging.

Citation Information

Cited By

  • Environment-friendly epoxy resin adhesive and preparation method thereof

    CN121914658A