Metal mask plate, manufacturing method and testing method thereof, and OLED packaging layer forming method
By optimizing the etching depth and film-forming air pressure on the metal mask, the problems of large shadow areas at the packaging layer boundary and thickening of the film layer in OLED packaging technology are solved, extending the service life of the mask and improving the packaging of OLED panels. quality.
Patent Information
- Application Number
- CN202410807891.5
- Authority / Receiving Office
- CN · China
- Patent Type
- Applications(China)
- Current Assignee / Owner
- Filing Date
- 2024-06-20
- Publication Date
- 2024-10-15
AI Technical Summary
In OLED thin film packaging technology, existing metal masks have problems such as large shadow areas at the boundary of the packaging layer, abnormal thickening of the film layer in the TP terminal part, and early peeling of the insulating film layer during use, which affects the quality of the packaging layer and the mask. The service life of the board.
By optimizing the manufacturing method of the metal mask, including forming half-grooves on the mesh surface and coating, adjusting the etching depth and film-forming air pressure, the shadow area at the boundary of the packaging layer and the thickness of the TP terminal film are reduced, and the insulation film is improved. The bonding strength and service life of the layers.
It effectively reduces the shadow area at the boundary of the packaging layer, extends the service life of the mask, reduces the cost, and improves the packaging quality and process margin of the OLED panel.
Smart Images

Figure CN118773570A_ABST
Abstract
Description
Technical Field
[0001] The present disclosure relates to the technical field of OLED manufacturing, and in particular to a metal mask plate and a manufacturing method and a testing method thereof, and a method for forming an OLED encapsulation layer. Background Art
[0002] In OLED Thin Film Encapsulation (TFE) technology, using Chemical Vapor Deposition (CVD) to form an encapsulation layer is a sophisticated process. Its main purpose is to form one or more protective films on the surface of the OLED device to prevent moisture and oxygen from penetrating, thereby protecting the organic light-emitting layer from the external environment.
[0003] In the aforementioned TFE process, a metal mask plate, namely a CVD metal mask plate (CVD Mask), is required as a mask to limit the boundary of the formed encapsulation layer. However, during the production process, it was found that the encapsulation film of the TP terminal part was abnormally thickened, and the shadow area (shadow) of the encapsulation layer boundary was large. It was further found that the above phenomenon would become more serious when the mask plate was used repeatedly. At the same time, it was observed that along with the above phenomenon, the insulating film layer of the mask plate would peel off earlier than the preset lifespan. Summary of the invention
[0004] The present disclosure provides a method for manufacturing a metal mask plate, a metal mask plate formed by the aforementioned method, and a method for manufacturing an OLED encapsulation layer using the metal mask plate, aiming to at least improve or solve the problems in the aforementioned prior art.
[0005] According to a first aspect of an embodiment of the present disclosure, a method for manufacturing a metal mask is provided, the method specifically comprising:
[0006] A frame and a mesh are provided, wherein the mesh includes a plurality of mask strips and a plurality of openings surrounded by the plurality of mask strips; the thickness of the mesh is 80 μm to 250 μm;
[0007] Forming a half groove, etching part or all of the plurality of mask strips to form a half groove facing the back of the metal mask plate, the etching direction is the mesh thickness direction, and the etching depth is 10% to 40% of the thickness of the etched mask strip; wherein the distance between the side edge of the half groove and the side edge of the mask strip is 0.2 mm to 6 mm;
[0008] Stretching the mesh, stretching the mesh surface and fixing it in the frame to form a mask plate substrate;
[0009] Coating is performed to form an insulating film layer on the surface of the mask substrate, and the thickness of the insulating film layer is 1μm to 3.5μm.
[0010] The aforementioned technical solution, in particular, optimizes the etching depth of the half groove, and in conjunction with the limitation of the film thickness and the width of the solid material area, can effectively reduce the shadow area at the boundary of the packaging layer, alleviate the thickening of the film layer in the TP terminal part, and improve the bonding strength of the insulating film layer.
[0011] In the aforementioned etching depth range of 10% to 40%, for example, a 150μm substrate is selected and a 50μm half groove is etched, the etching depth is 33.3%, and with a specific film-forming gas pressure, the service life can reach about 7000half, the shadow area is about 200μm, which is better than the 250μm in the prior art, and the TP terminal film thickness is within 1000A. In the bending experiment that reflects the bonding strength of the film layer, with a specific film-forming gas pressure, no delamination occurs in at least 50 bends. Only when the etching depth is 50%, that is, about 75μm, a slight solid material section appears.
[0012] Optionally, the nominal thickness of the mesh surface is 150 μm, and the etching depth of the half groove is 15 μm to 50 μm.
[0013] Optionally, the etching depth of the half groove is 20 μm±5 μm.
[0014] In the above-mentioned optional scheme, the half-groove etching depth is specially optimized for the commonly used thickness specification of the mask plate, 150μm. In the bending test, with the specific film-forming gas pressure, no delamination phenomenon occurs after at least 50 bends, which makes the mask plate have an excellent service life. In the use scenario, the shadow area is small and the TP terminal film thickness is effectively controlled, which helps to compress the OLED panel frame.
[0015] In particular, when the etching depth of the half groove is about 20μm, with a specific film-forming gas pressure, the service life can reach 9000 half, which is much higher than the 4000 / 5000 half of the existing products. Under ideal conditions, it can save nearly 50% of the mask cost.
[0016] In addition, when the etching depth of the half groove is about 20μm, the shadow area can be controlled within 150μm, contributing about 50-100μm to the narrow border of the OLED product, that is, the OLED panel border can be compressed by 50-100μm.
[0017] In terms of TP terminal film thickness, the etching depth is about 20μm, and the TP terminal film thickness is within 700A (angstroms), which is significantly optimized compared to the existing technology of about 1400A, providing a larger process margin for OLED panels.
[0018] Optionally, the nominal thickness of the mesh is 100μm and the etching depth of the half groove is 10μm to 30μm
[0019] Optionally, the insulating film layer is an aluminum oxide coating;
[0020] The substrate material is selected from: Invar36 alloy, Super Invar32 alloy, SUS304 or SUS420;
[0021] During the coating step, the pressure in the film forming chamber is set at 2*10 -1 ~5*10 -1 MPa range.
[0022] Optional, using 2*10 -1 ~3*10 -1 MPa film forming gas pressure.
[0023] In the above optional scheme, the setting of the gas pressure in the film forming chamber can improve the winding quality of the insulating film layer, and the film layer quality is relatively good. At least 50 bending tests will not cause delamination at the crease, solid material section, or half-cut section. Combined with the above-mentioned half-cut groove depth characteristics, it helps to further improve the product life.
[0024] Optionally, the aluminum oxide layer has a thickness of 2.4 μm to 2.8 μm.
[0025] Optionally, the aluminum oxide layer has a nominal thickness of 2.5 μm.
[0026] Optionally, the aluminum oxide layer has a nominal thickness of 2.7 μm.
[0027] The resistivity, uniformity and bonding strength of the aforementioned coating thickness all meet the requirements of the TFE process.
[0028] Preferably, the distance between the side edge of the half-groove and the side edge of the mask strip is 0.2 mm to 4 mm.
[0029] Preferably, the distance between the side edge of the half-groove and the side edge of the mask strip is 0.2 mm to 2 mm.
[0030] Preferably, the distance between the side edge of the half-groove and the side edge of the mask strip is 0.2 mm to 1.4 mm.
[0031] Preferably, the distance between the side edge of the half-groove and the side edge of the mask strip is 0.3 mm to 0.5 mm.
[0032] Optionally, the distance between the side of the half groove and the side of the mask strip, that is, the width of the solid material area, is 0.4 mm ± 0.05 mm, which can significantly reduce the scratching of the mask plate on the packaging layer.
[0033] Optionally, the multiple mask strips specifically include multiple first mask strips and multiple second mask strips; the first mask strips are perpendicular to the second mask strips and are wider than the second mask strips; the half-grooves are formed in the first mask strips and / or the second mask strips; the half-grooves are segmented grooves or through grooves.
[0034] Optionally, the width of the first mask strip is 20 mm±0.05 mm, and the width of the second mask strip is less than or equal to 10 mm.
[0035] According to a second aspect of the embodiments of the present disclosure, a metal mask plate is provided, wherein the metal mask plate is manufactured by adopting the manufacturing method of the technical solution of the first aspect and any optional solution thereof.
[0036] A third aspect of the embodiments of the present disclosure provides a method for testing the film bonding strength of the aforementioned metal mask, comprising:
[0037] In the coating step of the metal mask plate, a co-plating sheet is provided;
[0038] Periodically bending the two ends of the accompanying plating sheet until the accompanying plating sheet has film layer delamination, a solid material section or a half-engraved section, and recording the number of periodic bending;
[0039] The accompanying plating sheet and the mask plate substrate are made of the same material and are provided with half grooves of the same depth.
[0040] According to a fourth aspect of the embodiments of the present disclosure, a method for forming an OLED encapsulation layer is provided, wherein the method uses the metal mask plate according to the technical solution of the second aspect as a mask, and forms one or more encapsulation layers on the surface of the target device by a chemical vapor deposition method. The encapsulation layer formed by the method has a small shadow area, a thin TP terminal film thickness, a good process margin, a good film quality, and a small number of scratches per unit area.
[0041] In summary, the metal mask plate manufacturing method provided by the embodiment of the present disclosure, and the mask plate formed therefrom, can significantly optimize the service life, reduce the cost of use, improve the quality of the formed encapsulation layer, and provide a larger process margin and more reliable encapsulation quality for the OLED panel. BRIEF DESCRIPTION OF THE DRAWINGS
[0042] In order to more clearly illustrate the technical solutions in the embodiments of the present invention or the background technology, the drawings required for use in the embodiments of the present invention or the background technology will be described below.
[0043] Figure 1 The overall structure diagram of the metal mask plate involved in the present disclosure is shown;
[0044] Figure 2 A partial enlarged view of a half-groove in the manufacturing method disclosed in the present invention, the view showing the width T1 of the solid material area;
[0045] Figure 3 is a schematic cross-sectional view of a mask strip in a metal mask plate involved in the present disclosure;
[0046] Figure 4An embodiment of etching a through half groove on a first mask strip in the present disclosure is shown;
[0047] Figure 5 An embodiment of etching a segmented half groove on a first mask strip in the present disclosure is shown;
[0048] Figure 6 An embodiment of etching a through half groove on a second mask strip in the present disclosure is shown;
[0049] Figure 7 An embodiment of etching a segmented half groove on a second mask strip in the present disclosure is shown;
[0050] Figure 8 An embodiment of the present disclosure for etching through half-grooves on all mask strips at the same time is shown;
[0051] Fig. 9 An embodiment of etching segmented half grooves on all mask strips simultaneously in the present disclosure is shown;
[0052] Fig.10 is a schematic diagram of an existing mask coating process as a comparative example;
[0053] Fig.11 is a schematic diagram of coating a mask plate in the manufacturing method disclosed in the present invention;
[0054] Fig.12 It shows the process of processing a metal mask plate from a sheet to a finished product, and the production line usage flow chart;
[0055] Fig.13 The effect of half-grooves of different depths on edge shadows in the process of forming a packaging layer is shown;
[0056] Fig.14 The improvement effect of the embodiment of the present disclosure on the shadow area is shown;
[0057] Fig.15 The improvement effect of the embodiment of the present disclosure on the film thickness of the TP terminal is shown;
[0058] Fig.16 A schematic diagram of a film layer bonding strength testing method in an embodiment of the present disclosure is shown.
[0059] Note in the figure:
[0060] 1 frame, 2 mesh surfaces;
[0061] 20 opening; 21 mask strip;
[0062] 210 is a half groove, 211 is a first mask strip, and 212 is a second mask strip. DETAILED DESCRIPTION
[0063] The present disclosure will now be described more fully below with reference to the accompanying drawings, however, the present disclosure can be implemented in many different ways and should not be construed as being limited to the embodiments set forth herein. On the contrary, providing these embodiments herein will make the present disclosure more detailed and complete, and fully convey the scope of the present disclosure to those skilled in the art. The same reference numerals throughout the text represent the same objects.
[0064] In view of the phenomenon in the prior art that the insulating film layer of the mask plate peels off earlier than the preset lifespan, the inventors of the present disclosure have conducted in-depth research and do not wish to be bound by any theory. The inventors of the present disclosure believe that the cause of this phenomenon is that when the mask plate is in use, the temperature in the equipment chamber rises, causing the flatness of the mask strip (the mask rib is used to form the mask plate mesh surface and surround the opening for limiting the vapor deposition area) of the mask plate to deteriorate. After the use process, the temperature drops to room temperature, and the flatness of the mask rib gradually recovers to its original state. Therefore, when the mask plate is repeatedly used, the flatness of the mask rib will periodically deteriorate and recover, and the insulating coating on the surface of the mask plate will bend and recover accordingly. Over time, the surface coating will peel due to the stress of repeated bending.
[0065] Usually, the rib area on the back side of the mask plate (i.e., the side facing the substrate during the CVD process) is etched to improve the flatness of the mask plate. The inventors further investigated and realized that such etching has an adverse effect under the aforementioned temperature cycle conditions. Specifically, the etching depth in the prior art is more than 50% of the plate thickness. The inventors realized that reducing the etching depth helps alleviate the aforementioned peeling phenomenon.
[0066] Without wishing to be bound by any theory, the inventors of the present disclosure also recognize that optimizing the gas pressure in the film-forming chamber for forming the insulating coating while adjusting the aforementioned etching depth can further increase the life of the film layer.
[0067] In addition, the existing mask plates often have abnormal thickening of the packaging film of the TP terminal part, and the shadow area (shadow) at the boundary of the packaging layer is large. After research, the inventors realized that the cause is also related to the current etching depth of more than 50%. Although the existing mask plates meet the flatness standards at room temperature, the disadvantage of reduced local strength caused by large etching depth is magnified under elevated temperature conditions. Similar to the aforementioned discussion on the peeling phenomenon, under elevated temperature conditions, the rib area and the substrate are poorly bonded, and gaps appear at the edges, resulting in increased shadow & TP terminal film thickness.
[0068] The metal mask plate in the prior art, for example, uses the type with an etching depth of more than 50%, and the shadow area (shadow) of the generated packaging layer is about 250μm, the TP terminal film thickness is within 1400A, and the mask life is 4000 / 5000half. The embodiments of the present disclosure aim to improve the above-mentioned indicators in the existing mask plate by optimizing the etching depth and optimizing parameters such as the film-forming gas pressure.
[0069] The present disclosure first provides an embodiment of a method for manufacturing a metal mask.
[0070] In an embodiment, the method specifically comprises:
[0071] like Figure 1 As shown, a frame 1 and a mesh surface 2 are provided.
[0072] like Figure 2 and Figure 3 As shown, the mesh surface 2 specifically includes a plurality of mask strips 21 and a plurality of openings 20 surrounded by the plurality of mask strips.
[0073] The mesh thickness is 80 μm to 250 μm; optionally, the mesh nominal thickness is 250 μm, or 150 μm, or 100 μm, or 80 μm, or 60 μm.
[0074] The frame 1 and the mesh surface 2 are preferably made of a low expansion alloy, or may be made of materials such as SUS304 or SUS420.
[0075] The frame 1 and the mesh surface 2 are preferably made of Invar 36 (Invar alloy, Invar steel, 4J36) alloy, the chemical composition of which includes: about 36% nickel (Ni), about 63% iron (Fe), and may also contain trace amounts of cobalt (Co), silicon (Si), manganese (Mn), phosphorus (P), sulfur (S) and carbon (C), wherein the carbon content is generally ≤0.05%, manganese ≤0.5%, silicon ≤0.3%, and phosphorus and sulfur are both ≤0.02%.
[0076] The frame 1 and the mesh surface 2 are preferably made of Super-Invar 32 alloy (4J32 or 4J5), which is formed by replacing nickel (Ni) with cobalt (Co) on the basis of Invar alloy, for example, containing 31-33% nickel (Ni), 4-6% cobalt (Co), and the remainder iron (Fe).
[0077] like Figure 3 As shown, a half groove 210 is formed. Specifically, part or all of the multiple mask strips are etched to form a half groove 210 facing the back of the metal mask plate. The etching direction is the mesh thickness direction, and the etching depth is 10% to 40% of the thickness of the etched mask strip.
[0078] It should be understood that the back side of the metal mask is the side facing the substrate during the CVD process.
[0079] Usually, the multiple mask strips (rib areas) of the mask plate include multiple horizontal and vertical mask strips, which are perpendicular to each other and cross each other to form multiple openings 20 for limiting the vapor deposition area. In the embodiment, the half grooves 210 can be formed in the horizontal mask strips, or in the vertical mask strips, or in both. Specifically, according to the actual situation of the mask plate, in combination with experiments / model simulation and other methods, a suitable setting position of the half grooves 210 can be selected, for example Figure 4 , Figure 6 and Figure 8 Examples of forming half grooves on transverse mask strips, longitudinal mask strips, and all mask strips are shown respectively.
[0080] In addition, the present embodiment also optimizes the width of the solid material area. Explanatoryally, the solid material area refers to the area on the rib area that has not been etched, that is, the area on the mesh surface that is neither an opening nor a half-groove.
[0081] exist Figure 2 The width indicated by T1 in the partial enlarged view is the width of the solid material area.
[0082] In the embodiment, the distance T1 between the solid material area, i.e., the side edge of the half-groove and the side edge of the mask strip is in the range of 0.2 mm to 6 mm;
[0083] After the aforementioned frame, mesh and the half grooves thereon are prepared, the mesh is stretched and fixed in the frame to form a mask plate substrate; in other words, the mesh is prestressed and tightened to ensure its flatness, and in this state the mesh is fixed in the frame by, for example, welding.
[0084] After the net is fixed, the mask substrate is plated, that is, an insulating film layer is formed on the surface of the mask substrate, and the thickness of the insulating film layer is 1 μm to 3.5 μm.
[0085] Explanatory note, since the mask plate in the embodiment is made of metal material and is conductive, this will cause the gas phase material to be mistakenly deposited on the mask plate during the process of forming the packaging layer. Therefore, the mask plate in the embodiment is provided with an insulating coating layer as a whole.
[0086] The overall manufacturing process of the CVD metal mask plate and the cleaning process during use are the same as those in the prior art except for the parts disclosed in this embodiment. Fig.12 The process flow diagram is shown.
[0087] Optionally, the material of the insulating coating layer may be aluminum oxide, aluminum nitride, zirconium oxide, yttrium oxide, aluminum oxynitride, silicon nitride or silicon oxide, etc.
[0088] The aforementioned technical solution, in particular, optimizes the etching depth of the half groove, and in conjunction with the limitation of the film thickness and the width of the solid material area, can effectively reduce the shadow area at the boundary of the packaging layer, alleviate the thickening of the film layer in the TP terminal part, and improve the bonding strength of the insulating film layer.
[0089] On the basis of the above-mentioned embodiment, in a further preferred embodiment, the half-groove etching depth is further limited, wherein the etching depth has different optimization schemes depending on the thickness of the plate.
[0090] For typical technical specifications, in a scheme where the nominal thickness of the mesh is 150 μm, the etching depth of the half groove is 15 μm to 60 μm, that is, the etching depth is 10% to 40% of the thickness of the mesh (foil), and more preferably, the etching depth can be selected from 15 μm to 50 μm.
[0091] In a typical embodiment, the half-groove is etched to a depth of 20 μm.
[0092] In a typical embodiment, the half-groove is etched to a depth of 50 μm.
[0093] As a comparative example, the etching depth of the half groove is set to 75μm. In this example, the etching depth reaches 50%. After experiments, obvious film layer delamination appeared after 50 bends (Table 1). At the same time, the warping was about 50μm, which was significantly greater than the 30μm of the 40% etching depth (Table 3). It can be seen that the 10% to 40% in the disclosed embodiment is significantly better than the etching depth of 50% and above.
[0094] In another embodiment, the etching depth of the half groove is 10 μm to 30 μm.
[0095] For typical technical specifications, the etching depth of the half groove is 10μm to 30μm for a nominal mesh thickness of 100μm.
[0096] In a typical embodiment, the half-groove is etched to a depth of 20 μm.
[0097] In the experiment, the pressure in the film-forming chamber was controlled by the conventional pressure parameters of the existing process. For the invar mesh with a nominal thickness of 150μm, half-groove etching was performed at a depth of 70% to 10%, and then 10, 30 and 50 bending tests were performed to observe the delamination and record whether the material section and half-groove section appeared. The film layer was aluminum oxide. The experimental results are as follows:
[0098] Table 1 Bending experiments at different etching depths
[0099]
[0100] The experimental results show that when the half-engraving depth is in the range of 10%-40% of the plate thickness, the film layer bonding strength is optimal; within this depth range, during the aluminum oxide coating process, it is less affected by temperature changes, the deformation of the invar plate is smaller, the gap with the substrate frame is smaller, the wrap-around plating phenomenon is improved more significantly, and ultimately the aluminum oxide film layer bonding strength is greatly improved.
[0101] On the contrary, the deeper the half-engraving depth, the weaker the local strength of the mask. During use, SiN x O x The film layer is deposited on the surface of the mask plate. The thermal expansion coefficient of the invar raw material is smaller than that of alumina. Before and after use, the temperature of the mask plate changes significantly. The deformation of alumina is greater than that of the invar raw material, which makes it easier to fall off. The deeper the etching depth, the greater the initial deformation of the invar plate, which leads to greater internal stress of the alumina film layer, making it easier to peel off during use.
[0102] It can be seen that when the etching depth is reduced to below 40%, the stratification and cross-section show a qualitative improvement. In particular, the wrap-around plating phenomenon is improved, which ultimately greatly enhances the unexpected effect of the aluminum oxide film bonding strength.
[0103] Explanatory, the wrap-around plating refers to the movement of aluminum oxide molecules to the back of the plate surface when the front side of the film mask is plated to form a film layer (refer to Fig.10 and Fig.11 ), usually, the quality of the winding coating layer is poor, and the peeling caused by bending often starts from the winding coating layer on the back. The above-mentioned improvement in etching depth surprisingly significantly improves the quality of the winding coating layer, especially when the etching depth is reduced to less than 40%, the quality of the winding coating layer is significantly improved, and the film bonding strength is greatly improved.
[0104] The inventors noticed the influence of the coating quality on the life of the mask plate. In view of this, they conducted in-depth research on the improvement of coating, adjusted and experimented with the pressure setting value of the film forming chamber, and noticed that when the pressure setting value of the film forming chamber was 2*10 -1 ~5*10 -1 Within the MPa range, the film quality is significantly improved. In the experiment, samples with an etching depth of 50% were selected, and the experimental data are as follows:
[0105] Table 2 Effect of film forming chamber air pressure on film quality
[0106]
[0107]
[0108] It can be seen that for the sample with an etching depth of 50%, the obvious delamination that originally appeared after 50 bends has changed after 5*10-1 MPa pressure, the serious solid material section also becomes mild. As the chamber pressure is further reduced, at 2*10 -1 MPa to 3*10 - 1 MPa, the crease, solid section and half-cut section are significantly improved. -1 MPa, the crease, solid section and half-engraved section deteriorate, and the bonding strength of the film layer tends to weaken.
[0109] Through the above experiments, it can be seen that in 2*10 -1 ~5*10 -1 MPa pressure range, the original obvious delamination in the sample became mild, and the original serious solid material end surface also became mild. Surprisingly, within 2*10 -1 ~3*10 -1 MPa, the sample problem was further corrected, and it is reasonable to believe that 2*10 -1 ~5*10 -1 MPa, or more preferably 2*10 -1 ~3*10 -1 MPa film-forming chamber pressure combined with the 10% to 40% etching depth in the aforementioned embodiment can more significantly optimize the film quality.
[0110] Therefore, the present disclosure provides an embodiment for improving the quality of winding plating.
[0111] In the embodiment, the insulating film layer is an aluminum oxide coating;
[0112] The substrate material is selected from: Invar36 alloy, Super Invar32 alloy, SUS304 or SUS420;
[0113] In the coating step, the pressure setting value of the film forming chamber is 2*10 -1 ~5*10 -1 MPa.
[0114] Preferably, the film forming chamber pressure setting value is 2*10 -1 ~3*10 -1 MPa.
[0115] In a preferred embodiment, the setting of the gas pressure in the film forming chamber can improve the winding quality of the insulating film layer, and the film layer quality is relatively good, and at least 50 bending tests will not cause delamination at the crease, solid material section, or half-engraved section. This allows the mask plate film layer to withstand repeated deformation caused by more cycles of temperature cycling, thereby increasing the life of the mask plate.
[0116] At the same time, combined with the aforementioned half-groove depth feature, it helps to further improve product life.
[0117] In a typical embodiment, under the condition of a nominal mesh thickness of 150 μm, 2*10 -1 ~3*10 -1 MPa of film-forming chamber pressure, combined with a half-groove etching depth of 20μm±5μm, can effectively improve the film layer bonding degree. As expected, the life of the mask plate is significantly improved.
[0118] The above embodiments describe the influence of etching depth and film forming parameters on film layer bonding strength and plating quality. On this basis, the inventors further studied the relationship between etching depth and plate warping degree. The experiment used a 150 μm substrate and controlled other variables, that is, the film forming chamber pressure setting value was 2.5*10 -1 MPa, the results are as follows:
[0119] Table 3 Analysis of half-engraving depth and plate warping degree
[0120]
[0121] It can be seen that the critical point of the change in the warping degree is between 50% and 40% of the half-engraving depth.
[0122] Combined with the above data, the film forming chamber pressure is 2.5*10 -1 MPa, and the half-engraving depth is in the range of 10%-40% of the plate thickness. The local deformation of the CVD mask plate is small, and it fits better with the substrate frame, and it is not easy to produce poor plating. The film bonding strength of the CVD mask plate aluminum oxide film is significantly improved, and the aluminum oxide film is not easy to peel off.
[0123] The optimization method for etching depth proposed in the above embodiments has specific effects on Invar plates with different nominal thicknesses. The inventors conducted experiments to verify the influence of plates with different thicknesses on the bonding strength and life of the mask film layer. The conventional film-forming chamber gas pressure parameters of the existing process were used in the experiment. It was found that there was no difference in life when the plate thickness was 100μm-250μm. In the case of 80μm, the deeper the etching depth, the lower the strength of the mask plate, resulting in a decrease in life. In the case of 60μm depth, deeper etching will cause the plate to break. It is believed that the factor affecting the bonding strength of the film layer is mainly the etching depth, which has little to do with the plate thickness.
[0124] In the case of 10%-40% etching depth, the plate thickness is more reasonable between 80-250μm, and the film layer bonding force and the plate strength itself can meet the use requirements;
[0125] The experimental data are as follows:
[0126] Table 4 Effect of different plate thickness on CVD Mask film bonding strength and life
[0127]
[0128]
[0129]
[0130] The present disclosure further provides an embodiment for optimizing the thickness of the aluminum oxide film layer.
[0131] In the process of testing the thickness of the aluminum oxide film, it was found that the coating thickness was in the range of 1-3.5μm, which met the requirements for the use of CVD Mask (resistivity>10 11 &Film thickness uniformity <8%,), when the thickness is 0.5μm, the resistivity requirement is not up to standard, and when it is 4μm, the film thickness uniformity is not up to standard, so the CVD Mask aluminum oxide coating thickness is required to be in the range of 1-3.5μm; in the experiment, a 150μm mesh surface and an etching depth of 20μm were selected, and the film forming pressure was 2.5*10 -1 MPa, the experimental results are as follows:
[0132] Table 5 Effect of aluminum oxide film thickness on resistivity & film bonding strength
[0133]
[0134] Therefore, the thickness of the insulating film layer can be selected to be 1 μm to 3.5 μm. After further verification, in combination with the aforementioned half-groove etching depth characteristics, the thickness of the aluminum oxide layer is 2.4 μm to 2.8 μm, which has no adverse effect on the film layer bonding strength.
[0135] In a typical embodiment, the aluminum oxide layer has a nominal thickness of 2.5 μm.
[0136] In a typical embodiment, the aluminum oxide layer has a nominal thickness of 2.7 μm.
[0137] In the above-mentioned embodiments, the resistivity, uniformity and bonding strength of the coating thickness all meet the requirements of the TFE process.
[0138] The present disclosure further provides an embodiment for optimizing the width of the solid material area.
[0139] like Figure 2 As shown, the width T1 of the solid material area is the distance between the side of the half groove and the side of the mask strip. The purpose of this embodiment is to explore the influence of the width of the solid material area on the number of substrate scratches and product life.
[0140] The test found that the width of the solid material area is within the range of 0.2mm-6mm, which can control the number of scratches on the single-chip substrate to meet the process requirements. Combined with the aforementioned half-groove etching depth characteristics, the warping of the rib area can be further reduced, so that under the condition of temperature cycling, the deformation under the same conditions is reduced, which also helps to increase the product life.
[0141] Preferably, the distance between the side edge of the half-grooved groove and the side edge of the mask strip is 0.2 mm to 4 mm. Further preferably, the distance between the side edge of the half-grooved groove and the side edge of the mask strip is 0.2 mm to 2 mm.
[0142] When the width of the solid material area does not exceed 1.4mm, that is, when the distance between the side of the half-groove and the side of the mask strip is 0.2mm to 1.4mm, the average number of scratches on the tested single-chip substrate can be controlled within 10, and the scratch risk (number) is significantly improved, with unexpected effects.
[0143] Preferably, the distance between the side edge of the half-groove and the side edge of the mask strip is 0.3 mm to 0.5 mm.
[0144] Under the condition of 0.4mm±0.05mm width, the number of scratches is small, and the average number of scratches is rounded to 2, which is significantly better than the process requirements. At the same time, it can improve the quality of the packaging film, so that the final product has high reliability and good life.
[0145] Take a single-chip substrate of unit size and conduct ten experiments with CVD masks of different solid material area widths. Take the average value of the number of scratches and round it up. The verification data is as follows:
[0146] Table 6 Verification of the scratch condition of the single-chip substrate by the width of the solid material area
[0147]
[0148]
[0149] In addition, the effects of the dual optimization of the film forming chamber pressure and the half-engraving depth on the life of the mask product are verified in the embodiment, and the experimental data are as follows:
[0150] Table 7 CVD Mask life verification
[0151]
[0152] It can be seen from the above experimental data that the use of 2*10 -1 ~3*10 -1 When the gas pressure parameters of the film-forming chamber are within the MPa range and the etching depth is within the range of 10% to 20%, for example, when the etching depth is 20 μm, the life is optimal and can reach about 9000 half years.
[0153] The present disclosure further provides embodiments of various different half-engraved designs.
[0154] like Figures 4 to 9 As shown, multiple mask strips specifically include multiple first mask strips 211 and multiple second mask strips 212; the first mask strips 211 are perpendicular to the second mask strips 212 and are wider than the second mask strips 212; the half-grooves 210 are formed in the first mask strips and / or the second mask strips; the half-grooves are segmented grooves or through grooves.
[0155] like Figure 4 As shown, the half-groove 210 is only formed on the first mask strip 211 .
[0156] like Figure 5 As shown, the half-groove 210 is only formed on the first mask strip 211, and the half-groove 210 is segmented, and is segmented at the intersection of the first mask strip and the second mask strip.
[0157] like Figure 6 As shown, the half-groove 210 is only formed on the second mask strip 212 .
[0158] like Figure 7 As shown, the half groove 210 is only formed on the second mask strip 212, and the half groove 210 is segmented, which is segmented at the intersection of the first mask strip and the second mask strip.
[0159] like Figure 8 As shown, the half-grooves 210 are formed on the first mask strip and the second mask strip at the same time.
[0160] like Fig. 9 As described above, the half-grooved groove 210 is formed on the first mask strip and the second mask strip at the same time, and the half-grooved groove 210 is segmented, and is segmented at the intersection of the first mask strip and the second mask strip.
[0161] The aforementioned half-grooving forms have no significant effect on the bonding strength of the film layer, and the verification data are as follows.
[0162] Table 8 CVD Mask half-engraving design verification
[0163]
[0164]
[0165]
[0166] In Table 8, howling refers to the first mask strip in the embodiment, and rib refers to the second mask strip described in the embodiment.
[0167] In a preferred embodiment, the width of the first mask strip is 20 mm ± 0.05 mm, and the width of the second mask strip is less than or equal to 10 mm. This width design, combined with the aforementioned half-groove etching depth feature, can reduce the warpage of the rib area, so that under the condition of temperature cycling, the deformation under the same conditions is reduced, which also helps to increase the product life.
[0168] In a preferred embodiment, the tolerance range of the width of the first mask strip can be further reduced, for example, to 20 mm±0.05 mm, which helps to improve product consistency.
[0169] In addition, for a 150μm thick sheet, the effects of different etching depths on the flatness of the rib area are as follows:
[0170] Table 9 Etching depth & rib flatness analysis (mean)
[0171] Etching depth Rib flatness 20μm 15μm 50μm 30μm 75μm 40μm 90μm 50μm
[0172] In the embodiment of the present disclosure, the depth setting of the half groove can affect the shadow area size of the packaging film formed by the mask plate and the film thickness of the TP terminal. Fig.14 and Fig.15 shown.
[0173] Taking the thickness of 150μm plate as an example, the shadow area size produced by using the mask plate formed by 20μm half engraving, 50μm half engraving and 75μm half engraving is as follows: Fig.13 As shown, it can be seen that the shadow area of the 20μm half-mark is smaller in size.
[0174] Based on the solutions in the above embodiments, within the above etching depth range of 10% to 40%, for example, a 150 μm substrate is selected and a 50 μm half-groove is etched, the etching depth is 33.3%, and a specific film forming gas pressure such as 2*10 -1 ~5*10 -1 MPa, the width of the solid material area is 0.4mm, the service life can reach about 7000half, the shadow area is about 200μm, which is better than the 250μm in the existing technology, and the TP terminal film thickness is within 1000A. In the bending experiment that reflects the bonding strength of the film layer, no delamination occurs in at least 50 bends. Only when the etching depth is 40%, that is, about 60μm, a slight solid material end face appears.
[0175] In the above-mentioned optional scheme, the half-groove etching depth is specially optimized for the commonly used thickness specification of the mask plate, 150μm. In the bending test, no delamination phenomenon occurs after at least 50 bends, which makes the mask plate have an excellent service life. With the specific film-forming gas pressure, in the use scenario, the shadow area is small and the TP terminal film thickness is effectively controlled, which helps to compress the OLED panel frame.
[0176] In particular, when the etching depth of the half-groove is about 20 μm, with a specific film forming pressure such as 2*10 -1 ~3*10 -1 MPa, the width of the solid material area is 0.4mm, the thickness of the aluminum oxide layer is 2.4μm to 2.8μm, and the service life can reach 9000half, which is much higher than the 4000 / 5000half of the existing products. Under ideal conditions, it can save nearly 50% of the mask cost.
[0177] In addition, when the etching depth of the half groove is about 20μm, the shadow area can be controlled within 150μm, contributing about 50-100μm to the narrow border of the OLED product, that is, the OLED panel border can be compressed by 50-100μm.
[0178] In terms of TP terminal film thickness, the etching depth is about 20μm, and the TP terminal film thickness is within 700A, which is significantly optimized compared to the existing technology of about 1400A, providing a larger process margin for OLED panels.
[0179] The present disclosure provides an embodiment of a metal mask.
[0180] The metal mask plate is manufactured by adopting the manufacturing method in the aforementioned embodiment and any preferred embodiment thereof.
[0181] In view of the experiment on the film layer bonding strength in the aforementioned embodiment, the embodiment of the present disclosure provides a method for testing the film layer bonding strength of a metal mask plate. In the coating step of the tested metal mask plate, a co-plating sheet is provided.
[0182] After the coating is formed on the accompanying plate, Fig.16 As shown, the middle part of the accompanying plating sheet is restricted by clamping or similar means to maintain its original shape, and then the two ends of the accompanying plating sheet are periodically bent until the accompanying plating sheet shows film layer stratification, solid material section or half-engraved section, and the number of periodic bending is recorded; in recording the number of bending times, one action cycle, that is, bending up and down, is recorded as one bending.
[0183] The accompanying plating sheet is made of the same material as the mask substrate and is provided with a half groove of the same depth. In addition, in an optional embodiment, the accompanying plating sheet can also be provided with the same parameters as the mask such as the width of the solid material area.
[0184] The present disclosure provides an embodiment of a method for forming an OLED encapsulation layer.
[0185] The method uses the metal mask plate described in the above embodiment as a mask, and forms one or more packaging layers on the surface of the target device by chemical vapor deposition. The packaging layer formed by the method has a smaller shadow area, a thinner TP terminal film thickness, a good process margin, a good film quality, and a small number of scratches per unit area.
[0186] In summary, the metal mask plate manufacturing method provided by the embodiment of the present disclosure, and the mask plate formed therefrom, can significantly optimize the service life, reduce the cost of use, improve the quality of the formed encapsulation layer, and provide a larger process margin and more reliable encapsulation quality for the OLED panel.
[0187] The above is only a specific implementation of the embodiment of the present invention, but the protection scope of the embodiment of the present invention is not limited thereto. Any technician familiar with the technical field can easily think of changes or substitutions within the technical scope disclosed in the embodiment of the present invention, which should be included in the protection scope of the embodiment of the present invention. Therefore, the protection scope of the embodiment of the present invention should be based on the protection scope of the claims.
Claims
1. A method for manufacturing a metal mask, characterized in that: include: Providing a frame and a mesh surface, wherein the mesh surface includes a plurality of mask strips and a plurality of openings surrounded by the plurality of mask strips; The mesh surface thickness is 80 μm to 250 μm; Forming a half groove, etching part or all of the plurality of mask strips to form a half groove facing the back of the metal mask plate, wherein the etching direction is the thickness direction of the mesh surface, and the etching depth is 10% to 40% of the thickness of the etched mask strip; wherein the distance between the side edge of the half groove and the side edge of the mask strip is 0.2 mm to 6 mm; Stretching the mesh, stretching the mesh surface and fixing it in the frame to form a mask plate substrate; Film coating is performed to form an insulating film layer on the surface of the mask substrate, wherein the thickness of the insulating film layer is 1 μm to 3.5 μm.
2. The method according to claim 1, characterized in that: The nominal thickness of the mesh surface is 150 μm, and the etching depth of the half-groove is 15 μm to 50 μm.
3. The method according to claim 2, characterized in that: The etching depth of the half groove is 20 μm±5 μm.
4. The method according to claim 1, characterized in that: The nominal thickness of the mesh surface is 100 μm, and the etching depth of the half-groove is 10 μm to 30 μm.
5. The method according to claim 1, characterized in that: The insulating film layer is an aluminum oxide coating; The substrate material is selected from: Invar36 alloy, Super Invar32 alloy, SUS304 or SUS420; In the coating step, the pressure setting value of the film forming chamber is 2*10 -1 ~5*10 -1 MPa.
6. The method according to claim 4, characterized in that: The aluminum oxide layer has a thickness of 2.4 μm to 2.8 μm.
7. The manufacturing method according to claim 1, characterized in that: The distance between the side edge of the half-groove and the side edge of the mask strip is 0.4 mm±0.05 mm.
8. The production method according to any one of claims 1 to 7, characterized in that: The plurality of mask strips include a plurality of first mask strips and a plurality of second mask strips; the first mask strips are perpendicular to the second mask strips and are wider than the second mask strips; The half-engraved groove is formed on the first mask strip and / or the second mask strip; the half-engraved groove is a segmented groove or a through groove.
9. The manufacturing method according to claim 7, characterized in that: The width of the first mask strip is 20 mm±0.05 mm, and the width of the second mask strip is less than or equal to 10 mm.
10. A metal mask, characterized in that: The metal mask is manufactured by the manufacturing method according to any one of claims 1 to 9.
11. A method for testing the film bonding strength of a metal mask as claimed in claim 10, characterized in that: include: In the coating step of the metal mask plate, a co-plating sheet is provided; Periodically bending the two ends of the accompanying plating sheet until the accompanying plating sheet has film layer delamination, a solid material section or a half-engraved section, and recording the number of periodic bendings; The accompanying plating sheet is made of the same material as the mask plate substrate and is provided with half grooves of the same depth.
12. A method for forming an OLED encapsulation layer, characterized in that: The metal mask plate according to claim 10 is used as a mask, and one or more packaging layers are formed on the surface of the target device by a chemical vapor deposition method.