Foamed aluminum wall thermal insulation material and preparation method thereof
By using the chemical vapor deposition method to generate a core-shell structure additive for the aluminum oxide shell in the preparation of aluminum foam, the problem of floating and breaking bubbles is solved, the thermal insulation performance and thermal conductivity of aluminum foam are improved, and the preparation process is simplified.
Patent Information
- Application Number
- CN202410747266.6
- Authority / Receiving Office
- CN · China
- Patent Type
- Applications(China)
- Current Assignee / Owner
- Filing Date
- 2024-06-11
- Publication Date
- 2024-10-15
AI Technical Summary
In the existing aluminum foam preparation method, titanium hydride reacts quickly, causing bubbles to float and break, affecting the thermal insulation performance.
The chemical vapor deposition method is used to deposit an aluminum oxide shell layer on the surface of calcium carbonate to form a core-shell structure additive. When added to the aluminum melt, the calcium carbonate decomposes to generate bubbles, and the alumina shell layer limits the bubbles from floating up, forming a multi-level pore structure and reducing the thermal conductivity.
The thermal insulation performance of aluminum foam is improved, the thermal conductivity is reduced, and the use of tackifiers is avoided through the viscosity-increasing effect of alumina, simplifying the preparation process.
Smart Images

Figure CN118773574A_ABST
Abstract
Description
Technical Field
[0001] The invention belongs to the technical field of thermal insulation materials, and specifically relates to a foam aluminum wall thermal insulation material and a preparation method thereof. Background Art
[0002] At present, there are many kinds of wall insulation materials, such as aerated blocks, hollow blocks, gypsum hollow blocks, porous clay bricks, aerated fly ash bricks, GRC wall panels, reinforced fiber cement boards, sandwich panels, fly ash aerated wall panels, etc. Although there are many kinds, there is no category with particularly outstanding performance. For wall insulation materials, it is not only necessary to have excellent thermal insulation performance, but also high mechanical strength. Foamed aluminum is a material composed of a metal matrix and pores. Compared with traditional wall insulation materials, it has the advantages of high strength and light weight. According to the different ways of connecting the pores, foamed aluminum can be divided into open foamed aluminum and closed-cell foamed aluminum. The pores of open foamed aluminum are in an open form, which is conducive to the transfer of heat, so it has better heat dissipation performance, while the pores in closed-cell foamed aluminum are closed, which makes the material have good thermal insulation performance, and the thermal conductivity of closed-cell foamed aluminum decreases with the increase of porosity, so increasing the closed-cell porosity in foamed aluminum is a strategy to improve its thermal insulation performance.
[0003] At present, the most commonly used method for producing aluminum foam is the melt foaming method, which specifically refers to adding a foaming agent, titanium hydride, to an aluminum melt with a certain viscosity. During the heating process, titanium hydride generates hydrogen that remains in the system and forms an aluminum foam material after solidification. However, due to the fast reaction rate of titanium hydride, the rapidly generated bubbles easily float to the surface of the melt, and the bubbles are easily broken and merged, resulting in coarse and broken pores in the final formation, which affects the thermal insulation performance of the aluminum foam. Summary of the invention
[0004] In order to solve the above technical problems, the present invention provides a foam aluminum wall insulation material and a preparation method thereof. In the prepared foam aluminum composite material, the generated bubbles are not easy to float up and rupture, the pore quality is high, and the thermal conductivity of the composite material is reduced, so that the composite material has excellent thermal insulation performance.
[0005] The present invention is specifically achieved through the following technical solutions.
[0006] The first object of the present invention is to provide a method for preparing a foam aluminum wall insulation material, comprising the following steps:
[0007] An aluminum oxide shell layer is deposited on the surface of calcium carbonate by chemical vapor deposition to prepare an additive with a core-shell structure;
[0008] Aluminum is heated and melted to prepare an aluminum melt; the additive is added to the aluminum melt, stirred evenly, and then the temperature is increased to decompose the calcium carbonate in the additive to perform foaming treatment, and then the mixture is placed in a mold to be cooled to prepare a foamed aluminum wall insulation material.
[0009] The mechanism of the present invention is as follows: the present invention uses chemical vapor deposition to generate aluminum oxide on the surface of calcium carbonate, and prepares a core-shell structure additive with a core of calcium carbonate and an outer shell of aluminum oxide. In the additive, calcium carbonate is used as a foaming agent. After the additive is added to the aluminum melt, since the melting point of Al is 660.4°C, the decomposition temperature of calcium carbonate is (898-910°C), and the melting point of aluminum oxide is 2054°C, when the temperature is raised to the decomposition of calcium carbonate, aluminum oxide will not be destroyed. When the temperature is raised to the decomposition of calcium carbonate to generate bubbles, since there is an aluminum oxide shell layer on the outside of the calcium carbonate, the generated bubbles are restricted, and the bubbles are not easy to float. In addition, compared with the bubbles, the shell layer and the reaction products in the shell have a higher density, so they will not float in the aluminum melt, ensuring the uniform distribution of the bubbles in the system. After the calcium carbonate is decomposed, there are two pore structures in the system. On the one hand, there is an aluminum oxide shell generated after the decomposition of the calcium carbonate core, which is a cavity structure; on the other hand, there are tiny bubbles generated in the cavity structure. Therefore, there is a multi-level bubble structure in the prepared composite material, and the bubbles are independent of each other, which improves the bubble quality and thus reduces the thermal conductivity of the composite material. The aluminum oxide in the additive shell has a viscosity-increasing effect, which can increase the viscosity of the aluminum melt without the need to add a traditional viscosity-increasing agent.
[0010] In a preferred embodiment of the present invention, the calcium carbonate is spherical and has a particle size of 50-80 μm. After the decomposition of calcium carbonate, the pores generated in the inner shell are determined by the particle size of calcium carbonate, that is, the primary pore size in the composite material. The primary pore size is also distributed with bubble pores generated by calcium carbonate, which constitute the secondary pores of the composite material. And when the particle size of calcium carbonate is too large, it is necessary to ensure the integrity of its outer alumina shell, but in the preparation process, the shell is prone to incompleteness, resulting in pores overflowing from the shell in the finally prepared material. When the particle size of calcium carbonate is too small, the amount of gas generated in the shell is also too small, and the thermal insulation effect of the material is poor. Therefore, it is necessary to ensure that the calcium carbonate has a suitable particle size.
[0011] In a preferred embodiment of the present invention, the calcium carbonate is placed in a reaction chamber of a chemical vapor deposition device, a protective gas is introduced to exhaust the air, and then the protective gas is used as a carrier gas to introduce Al(CH 3 ) 3 , then pass H 2 O,Al(CH 3 ) 3 and H 2 O is deposited on the surface of calcium carbonate to form an aluminum oxide shell.
[0012] In a preferred embodiment of the present invention, Al(CH 3 ) 3 During the process, the temperature was controlled at 200-210°C and the introduction time was 10-20s. 2 During the process of O, the temperature is controlled at 200-210°C and the introduction time is 15-25s.
[0013] In a preferred embodiment of the present invention, the thickness of the aluminum oxide shell is 5-10 μm. The thickness of the aluminum oxide shell has an impact on the thermal conductivity. If the shell is too thick, it may lead to uneven distribution of bubbles, thereby affecting the overall thermal conductivity of the material. If the shell is too thin, there may be a problem of shell rupture, resulting in the overflow of bubbles generated by the decomposition of calcium carbonate. Therefore, the thickness of the aluminum oxide shell must be 5-10 μm.
[0014] In a preferred embodiment of the present invention, the amount of additive added is 1-3% of the mass of the aluminum melt. When the additive content is too low, the amount of bubbles generated is small, and when the additive content is too high, uneven distribution is likely to occur. In terms of cost, the amount of additive added in the present invention is 1-3% of the mass of the aluminum melt.
[0015] In a preferred embodiment of the present invention, the temperature is raised to 900-910°C to decompose calcium carbonate, and the temperature is kept for 30-40 minutes. At this temperature, calcium carbonate can be decomposed to generate gas, and keeping the temperature for a certain period of time can generate sufficient bubbles.
[0016] In a preferred embodiment of the present invention, the temperature for heating and melting aluminum is 670-700°C to ensure that the aluminum is melted, and the stirring temperature is 730-750°C. Stirring at this temperature not only makes the foaming agent evenly distributed, but also further increases the temperature inside the foaming agent, thereby preheating the subsequent decomposition.
[0017] The second object of the present invention is to provide a foam aluminum wall insulation material prepared by the above preparation method.
[0018] Compared with the prior art, the present invention has the following beneficial effects:
[0019] The present invention improves the preparation method of foamed aluminum and provides an improved method for preparing foamed aluminum by solution foaming. In the preparation process, only the additive of the present invention needs to be added without adding a tackifier. In the preparation process, the additive decomposes to generate bubbles, and the bubbles are not easy to float up, so a good porous structure can be formed in the aluminum matrix. The specific mechanism is:
[0020] The present invention uses chemical vapor deposition to generate aluminum oxide on the surface of calcium carbonate, and prepares a core-shell structure additive with a core of calcium carbonate and an outer shell of aluminum oxide. In the additive, calcium carbonate is used as a foaming agent, and its high-temperature decomposition is used to generate bubbles. Since there is an aluminum oxide shell layer on the outside of the calcium carbonate, it has a limiting effect on the generated bubbles, and the bubbles are not easy to float up. In addition, compared with the bubbles, the density of the shell layer and the decomposed products in the shell is higher than that of the simple bubbles, thereby reducing the probability of floating in the aluminum melt and ensuring the uniform distribution of bubbles in the system. After the calcium carbonate is decomposed, there are two pore structures in the system. On the one hand, there is an aluminum oxide shell generated after the decomposition of the calcium carbonate core, which is a cavity structure; on the other hand, there are tiny bubbles generated in the cavity structure. Therefore, there is a multi-level pore structure in the prepared composite material, and the pores are independent of each other, which improves the pore quality and thus reduces the thermal conductivity of the composite material.
[0021] In addition, the alumina in the additive shell has a viscosity-increasing effect, which can increase the viscosity of the aluminum melt. There is no need to add traditional viscosity-increasing agents, which reduces the types of raw materials added in the preparation process, improves the controllability of the preparation process, and is conducive to industrial production applications. BRIEF DESCRIPTION OF THE DRAWINGS
[0022] Figure 1 The figure is a schematic diagram of the preparation principle of the foam aluminum wall insulation material of the present invention.
[0023] Figure 2 This is a structural principle diagram of the foam aluminum wall insulation material of the present invention. DETAILED DESCRIPTION
[0024] In order to enable those skilled in the art to better understand and implement the technical solution of the present invention, the present invention is further described below in conjunction with specific embodiments and drawings, but the embodiments are not intended to limit the present invention.
[0025] The experimental methods and detection methods described in the following embodiments are conventional methods unless otherwise specified; the reagents and materials are commercially available unless otherwise specified.
[0026] It should be understood that the terms described in the present invention are only for describing special embodiments and are not intended to limit the present invention. In addition, for the numerical range in the present invention, it should be understood that each intermediate value between the upper and lower limits of the scope is also specifically disclosed. Each smaller range between the intermediate value in any stated value or stated range and any other stated value or intermediate value in the described range is also included in the present invention. The upper and lower limits of these smaller ranges can be independently included or excluded in the scope.
[0027] The invention improves the preparation of foamed aluminum by a melt foaming method, and provides a method for generating bubbles in an aluminum melt, wherein the bubbles are not easy to float up or break, thereby improving the formation quality of the bubbles in the aluminum matrix and improving the thermal insulation performance of the foamed aluminum.
[0028] The present invention provides a method for preparing a foam aluminum wall thermal insulation material, comprising the following steps:
[0029] An aluminum oxide shell layer is deposited on the surface of calcium carbonate by chemical vapor deposition to prepare an additive with a core-shell structure;
[0030] Aluminum is heated and melted to prepare an aluminum melt; the additive is added to the aluminum melt, stirred evenly, and then the temperature is increased to decompose the calcium carbonate in the additive to perform foaming treatment, and then the mixture is placed in a mold to be cooled to prepare a foamed aluminum wall insulation material.
[0031] like Figure 1 and Figure 2 As shown, the present invention uses chemical vapor deposition to generate aluminum oxide on the surface of calcium carbonate, and prepares a core-shell structure additive with a core of calcium carbonate and an outer shell of aluminum oxide. In the additive, calcium carbonate is used as a foaming agent. After the additive is added to the aluminum melt, since the melting point of Al is 660.4°C, the decomposition temperature of calcium carbonate is (898-910°C), and the melting point of aluminum oxide is 2054°C, aluminum oxide will not be destroyed when calcium carbonate decomposes. When the temperature is raised to the point where calcium carbonate decomposes to generate bubbles, since there is an aluminum oxide shell layer on the outside of calcium carbonate, it restricts the generated bubbles and the bubbles will not float. After calcium carbonate decomposes, there are two pore structures in the system. On the one hand, there is an aluminum oxide shell generated after the decomposition of the calcium carbonate core, which is a cavity structure (from the perspective of the entire aluminum melt system, it is a primary pore); on the other hand, there are tiny bubbles generated in the hollow structure (from the perspective of the entire aluminum melt system, it is a secondary pore). Therefore, there is a multi-level bubble structure in the prepared composite material, and the bubbles are independent of each other, which improves the bubble quality and reduces the thermal conductivity of the composite material. The alumina in the additive shell has a viscosity-increasing effect, which can increase the viscosity of the aluminum melt without the need to add a traditional viscosity-increasing agent.
[0032] The present invention will be specifically described below through the following examples and comparative examples.
[0033] Examples 1-3 and Comparative Examples 1-3 investigated the effect of the thickness of the alumina shell layer:
[0034] Example 1
[0035] A method for preparing a foam aluminum wall insulation material comprises the following steps:
[0036] Step 1: Place spherical calcium carbonate with a particle size of 50-60 μm in a tubular furnace quartz boat, introduce nitrogen to exhaust the air, then use nitrogen as a carrier gas and control the temperature at 200 °C to introduce Al(CH 3 ) 3 , the flow time is 10s, and then H 2 O, the introduction time is 15s, Al(CH 3 ) 3 and H 2 O is deposited on the surface of calcium carbonate to form an alumina shell. After the deposition is completed, the tube furnace is cooled to room temperature. The thickness of the alumina shell is about 5μm.
[0037] Step 2: Heat aluminum to 670°C to melt and prepare aluminum melt; add additives to the aluminum melt, the amount of the additives added is 2.5% of the mass of the aluminum melt, stir evenly at 740°C, raise the temperature to 910°C to decompose the calcium carbonate in the additive for foaming, and keep the temperature for 30 minutes. Then, place it in a mold to cool and prepare a foamed aluminum wall insulation material.
[0038] Example 2
[0039] A method for preparing a foam aluminum wall insulation material comprises the following steps:
[0040] Step 1: Place spherical calcium carbonate with a particle size of 50-60 μm in a tubular furnace quartz boat, introduce argon gas to exhaust the air, and then use argon as a carrier gas, control the temperature at 200 ° C, and introduce Al(CH 3 ) 3 , the introduction time is 15s, and then H 2 O, the introduction time is 20s, Al(CH 3 ) 3 and H 2 O is deposited on the surface of calcium carbonate to form an alumina shell. After the deposition is completed, the tube furnace is cooled to room temperature. The thickness of the alumina shell is about 8μm.
[0041] Step 2: heat aluminum to 670°C to melt and prepare an aluminum melt; add the additive to the aluminum melt, the additive amount is 2.5% of the mass of the aluminum melt, stir evenly at 740°C, heat to 910°C to decompose the calcium carbonate in the additive for foaming, keep warm for 30 minutes, then cool in a mold to prepare a foamed aluminum wall insulation material.
[0042] Example 3
[0043] A method for preparing a foam aluminum wall insulation material comprises the following steps:
[0044] Step 1: Place spherical calcium carbonate with a particle size of 50-60 μm in a tubular furnace quartz boat, introduce argon gas to exhaust the air, and then use argon as a carrier gas, control the temperature at 200 ° C, and introduce Al(CH 3 ) 3 , the passage time is 20s, and then H 2 O, the introduction time is 25s, Al(CH 3 ) 3 and H 2 O is deposited on the surface of calcium carbonate to form an alumina shell. After the deposition is completed, the tube furnace is cooled to room temperature. The thickness of the alumina shell is about 10 μm.
[0045] Step 2: heat aluminum to 670°C to melt and prepare an aluminum melt; add the additive to the aluminum melt, the additive amount is 2.5% of the mass of the aluminum melt, stir evenly at 740°C, heat to 910°C to decompose the calcium carbonate in the additive for foaming, keep warm for 30 minutes, then cool in a mold to prepare a foamed aluminum wall insulation material.
[0046] Comparative Example 1
[0047] A method for preparing a foam aluminum wall insulation material comprises the following steps:
[0048] Step 1: Place spherical calcium carbonate with a particle size of 50-60 μm in a tubular furnace quartz boat, introduce argon gas to exhaust the air, and then use argon as a carrier gas, control the temperature at 200 ° C, and introduce Al(CH 3 ) 3 , the passage time is 30s, and then H 2 O, the introduction time is 40s, Al(CH 3 ) 3 and H 2 O is deposited on the surface of calcium carbonate to form an alumina shell. After the deposition is completed, the tube furnace is cooled to room temperature. The thickness of the alumina shell is about 20 μm.
[0049] Step 2: heat aluminum to 670°C to melt and prepare an aluminum melt; add the additive to the aluminum melt, the additive amount is 2.5% of the mass of the aluminum melt, stir evenly at 740°C, heat to 910°C to decompose the calcium carbonate in the additive for foaming, keep warm for 30 minutes, then cool in a mold to prepare a foamed aluminum wall insulation material.
[0050] Comparative Example 2
[0051] A method for preparing a foam aluminum wall insulation material comprises the following steps:
[0052] Step 1: Place spherical calcium carbonate with a particle size of 50-60 μm in a tubular furnace quartz boat, introduce nitrogen to exhaust the air, then use nitrogen as a carrier gas and control the temperature at 200 °C to introduce Al(CH 3 ) 3 , the flow time is 5s, and then H 2 O, the introduction time is 8s, Al(CH 3 ) 3 and H 2 O is deposited on the surface of calcium carbonate to form an alumina shell. After the deposition is completed, the tube furnace is cooled to room temperature. The thickness of the alumina shell is about 1 μm.
[0053] Step 2: heat aluminum to 670°C to melt and prepare an aluminum melt; add the additive to the aluminum melt, the additive amount is 2.5% of the mass of the aluminum melt, stir evenly at 740°C, heat to 910°C to decompose the calcium carbonate in the additive for foaming, keep warm for 30 minutes, then cool in a mold to prepare a foamed aluminum wall insulation material.
[0054] Comparative Example 3
[0055] The foamed aluminum is prepared by the conventional method in the background art. The specific preparation method is:
[0056] Heat aluminum to 670°C to melt, then add calcium in an amount of 3% of the melt mass. After stirring evenly, add titanium hydride in an amount of 1.2% of the melt mass. Under stirring conditions, perform foaming treatment and then cool to room temperature.
[0057] The materials prepared in the above Examples 1-3 and Comparative Examples 1-3 were tested according to the standard GB / T10295-2008. The reduction rate of thermal conductivity relative to Comparative Example 3 is shown in Table 1:
[0058] Table 1 Reduction rate of thermal conductivity of materials prepared in Examples 1-3 and Comparative Examples 1-2
[0059]
[0060] From the results in Table 1, it can be seen that the thickness of the alumina shell has an impact on the thermal conductivity of the material. If the shell is too thick, it may lead to uneven distribution of bubbles, thus affecting the overall thermal conductivity of the material. If the shell is too thin, there may be a problem of shell rupture, resulting in the overflow of bubbles generated by the decomposition of calcium carbonate, which also affects the thermal conductivity of the material. Therefore, by weighing the above two factors and ensuring that the shell has an appropriate thickness, the material can be guaranteed to have excellent thermal insulation performance.
[0061] Examples 4-6 and Comparative Examples 4-5 investigated the effect of spherical calcium carbonate particle size:
[0062] Example 4
[0063] A method for preparing a foam aluminum wall insulation material comprises the following steps:
[0064] Step 1: Place spherical calcium carbonate with a particle size of 70-80 μm in a tubular furnace quartz boat, introduce nitrogen to exhaust the air, and then use nitrogen as a carrier gas and control the temperature at 200 ° C to introduce Al (CH 3 ) 3 , the time of introduction is 12s, and then H 2 O, the introduction time is 17s, Al(CH 3 ) 3 and H 2 O is deposited on the surface of calcium carbonate to form an alumina shell. After the deposition is completed, the tube furnace is cooled to room temperature. The thickness of the alumina shell is about 5μm.
[0065] Step 2: heat aluminum to 670°C to melt and prepare an aluminum melt; add the additive to the aluminum melt, the additive amount is 2.5% of the mass of the aluminum melt, stir evenly at 740°C, heat to 910°C to decompose the calcium carbonate in the additive for foaming, keep warm for 30 minutes, then cool in a mold to prepare a foamed aluminum wall insulation material.
[0066] Example 5
[0067] A method for preparing a foam aluminum wall insulation material comprises the following steps:
[0068] Step 1: Place spherical calcium carbonate with a particle size of 70-80 μm in a tubular furnace quartz boat, introduce nitrogen to exhaust the air, and then use nitrogen as a carrier gas and control the temperature at 200 ° C to introduce Al (CH 3 ) 3 , the introduction time is 15s, and then H 2 O, the introduction time is 22s, Al(CH 3 ) 3 and H 2 O is deposited on the surface of calcium carbonate to form an alumina shell. After the deposition is completed, the tube furnace is cooled to room temperature. The thickness of the alumina shell is about 7μm.
[0069] Step 2: heat aluminum to 670°C to melt and prepare an aluminum melt; add the additive to the aluminum melt, the additive amount is 2.5% of the mass of the aluminum melt, stir evenly at 740°C, heat to 910°C to decompose the calcium carbonate in the additive for foaming, keep warm for 30 minutes, then cool in a mold to prepare a foamed aluminum wall insulation material.
[0070] Example 6
[0071] A method for preparing a foam aluminum wall insulation material comprises the following steps:
[0072] Step 1: Place spherical calcium carbonate with a particle size of 70-80 μm in a tubular furnace quartz boat, introduce nitrogen to exhaust the air, and then use nitrogen as a carrier gas and control the temperature at 200 ° C to introduce Al (CH 3 ) 3 , the time of introduction is 20s, and then H 2 O, the introduction time is 25s, Al(CH 3 ) 3 and H 2 O is deposited on the surface of calcium carbonate to form an alumina shell. After the deposition is completed, the tube furnace is cooled to room temperature. The thickness of the alumina shell is about 10 μm.
[0073] Step 2: heat aluminum to 670°C to melt and prepare an aluminum melt; add the additive to the aluminum melt, the additive amount is 2.5% of the mass of the aluminum melt, stir evenly at 740°C, heat to 910°C to decompose the calcium carbonate in the additive for foaming, keep warm for 30 minutes, then cool in a mold to prepare a foamed aluminum wall insulation material.
[0074] Comparative Example 4
[0075] A method for preparing a foam aluminum wall insulation material comprises the following steps:
[0076] Step 1: Place spherical calcium carbonate with a particle size of 120-140 μm in a tubular furnace quartz boat, introduce nitrogen to exhaust the air, then use nitrogen as a carrier gas, control the temperature at 200 ° C, and introduce Al(CH 3 ) 3 , the time of introduction is 20s, and then H 2 O, the introduction time is 25s, Al(CH 3 ) 3 and H 2 O is deposited on the surface of calcium carbonate to form an alumina shell. After the deposition is completed, the tube furnace is cooled to room temperature. The thickness of the alumina shell is about 10 μm.
[0077] Step 2: heat aluminum to 670°C to melt and prepare an aluminum melt; add the additive to the aluminum melt, the additive amount is 2.5% of the mass of the aluminum melt, stir evenly at 740°C, heat to 910°C to decompose the calcium carbonate in the additive for foaming, keep warm for 30 minutes, then cool in a mold to prepare a foamed aluminum wall insulation material.
[0078] Comparative Example 5
[0079] A method for preparing a foam aluminum wall insulation material comprises the following steps:
[0080] Step 1: Place spherical calcium carbonate with a particle size of 10-20 μm in a tubular furnace quartz boat, introduce nitrogen to exhaust the air, then use nitrogen as a carrier gas, control the temperature at 200 ° C, and introduce Al(CH 3 ) 3 , the time of introduction is 20s, and then H 2 O, the introduction time is 25s, Al(CH 3 ) 3 and H 2 O is deposited on the surface of calcium carbonate to form an alumina shell. After the deposition is completed, the tube furnace is cooled to room temperature. The thickness of the alumina shell is about 10 μm.
[0081] Step 2: heat aluminum to 670°C to melt and prepare an aluminum melt; add the additive to the aluminum melt, the additive amount is 2.5% of the mass of the aluminum melt, stir evenly at 550°C, heat to 910°C to decompose the calcium carbonate in the additive for foaming, keep warm for 30 minutes, then cool in a mold to prepare a foamed aluminum wall insulation material.
[0082] The performance of the materials prepared in Examples 4-6 and Comparative Examples 4-5 was tested, and the reduction rate of the thermal conductivity relative to Comparative Example 3 is shown in Table 2:
[0083] Table 2 Reduction rate of thermal conductivity of materials prepared in Examples 4-6 and Comparative Examples 4-5
[0084]
[0085] As can be seen from Table 2, the particle size of calcium carbonate has an impact on the thermal conductivity of the material. When the particle size is too large, it is necessary to ensure the integrity of the outer aluminum oxide shell. However, during the preparation process, the shell is prone to incompleteness, resulting in pores overflowing the shell in the final prepared material. When the calcium carbonate particle size is too small, the amount of gas generated in the shell is also too small, and the effect of improving the thermal insulation of the material is poor. Therefore, it is necessary to ensure that the calcium carbonate has a suitable particle size.
[0086] Examples 7-9 and Comparative Examples 6-7 investigated the effect of the amount of additive added:
[0087] Example 7
[0088] A method for preparing a foam aluminum wall insulation material comprises the following steps:
[0089] Step 1: Place spherical calcium carbonate with a particle size of 60-80 μm in a tubular furnace quartz boat, introduce nitrogen to exhaust the air, then use nitrogen as a carrier gas, control the temperature at 200-250 ° C, and introduce Al(CH 3) 3 , the time of introduction is 16s, and then H 2 O, the introduction time is 23s, Al(CH 3 ) 3 and H 2 O is deposited on the surface of calcium carbonate to form an alumina shell. After the deposition is completed, the tube furnace is cooled to room temperature. The thickness of the alumina shell is about 9μm.
[0090] Step 2: heat aluminum to 670°C to melt and prepare an aluminum melt; add the additive to the aluminum melt, the additive amount is 1% of the mass of the aluminum melt, stir evenly at 740°C, heat to 910°C to decompose the calcium carbonate in the additive for foaming, keep warm for 30 minutes, then cool in a mold to prepare a foamed aluminum wall insulation material.
[0091] Example 8
[0092] A method for preparing a foam aluminum wall insulation material comprises the following steps:
[0093] Step 1: Place spherical calcium carbonate with a particle size of 60-80 μm in a tubular furnace quartz boat, introduce nitrogen to exhaust the air, then use nitrogen as a carrier gas, control the temperature at 200-250 ° C, and introduce Al(CH 3 ) 3 , the time of introduction is 16s, and then H 2 O, the introduction time is 23s, Al(CH 3 ) 3 and H 2 O is deposited on the surface of calcium carbonate to form an alumina shell. After the deposition is completed, the tube furnace is cooled to room temperature. The thickness of the alumina shell is about 9μm.
[0094] Step 2: heat aluminum to 670°C to melt and prepare an aluminum melt; add the additive to the aluminum melt, the additive amount is 2% of the mass of the aluminum melt, stir evenly at 740°C, heat to 910°C to decompose the calcium carbonate in the additive for foaming, keep warm for 30 minutes, then cool in a mold to prepare a foamed aluminum wall insulation material.
[0095] Example 9
[0096] A method for preparing a foam aluminum wall insulation material comprises the following steps:
[0097] Step 1: Place spherical calcium carbonate with a particle size of 60-80 μm in a tubular furnace quartz boat, introduce nitrogen to exhaust the air, then use nitrogen as a carrier gas, control the temperature at 200-250 ° C, and introduce Al(CH 3 ) 3, the time of introduction is 16s, and then H 2 O, the introduction time is 23s, Al(CH 3 ) 3 and H 2 O is deposited on the surface of calcium carbonate to form an alumina shell. After the deposition is completed, the tube furnace is cooled to room temperature. The thickness of the alumina shell is about 9μm.
[0098] Step 2: heat aluminum to 670°C to melt and prepare an aluminum melt; add the additive to the aluminum melt, the additive amount is 3% of the mass of the aluminum melt, stir evenly at 740°C, heat to 910°C to decompose the calcium carbonate in the additive for foaming, keep warm for 30 minutes, then cool in a mold to prepare a foamed aluminum wall insulation material.
[0099] Comparative Example 6
[0100] A method for preparing a foam aluminum wall insulation material comprises the following steps:
[0101] Step 1: Place spherical calcium carbonate with a particle size of 60-80 μm in a tubular furnace quartz boat, introduce nitrogen to exhaust the air, then use nitrogen as a carrier gas, control the temperature at 200-250 ° C, and introduce Al(CH 3 ) 3 , the time of introduction is 16s, and then H 2 O, the introduction time is 23s, Al(CH 3 ) 3 and H 2 O is deposited on the surface of calcium carbonate to form an alumina shell. After the deposition is completed, the tube furnace is cooled to room temperature. The thickness of the alumina shell is about 9μm.
[0102] Step 2: heat aluminum to 670°C to melt and prepare an aluminum melt; add the additive to the aluminum melt, the additive amount is 5% of the mass of the aluminum melt, stir evenly at 740°C, heat to 910°C to decompose the calcium carbonate in the additive for foaming, keep warm for 30 minutes, then cool in a mold to prepare a foamed aluminum wall insulation material.
[0103] Comparative Example 7
[0104] A method for preparing a foam aluminum wall insulation material comprises the following steps:
[0105] Step 1: Place spherical calcium carbonate with a particle size of 60-80 μm in a tubular furnace quartz boat, introduce nitrogen to exhaust the air, then use nitrogen as a carrier gas, control the temperature at 200-250 ° C, and introduce Al(CH 3 ) 3 , the time of introduction is 16s, and then H 2O, the introduction time is 23s, Al(CH 3 ) 3 and H 2 O is deposited on the surface of calcium carbonate to form an alumina shell. After the deposition is completed, the tube furnace is cooled to room temperature. The thickness of the alumina shell is about 9μm.
[0106] Step 2: heat aluminum to 670°C to melt and prepare an aluminum melt; add the additive to the aluminum melt, the additive amount is 0.2% of the mass of the aluminum melt, stir evenly at 740°C, heat to 910°C to decompose the calcium carbonate in the additive for foaming, keep warm for 30 minutes, then cool in a mold to prepare a foamed aluminum wall insulation material.
[0107] The performance of the materials prepared in Examples 7-9 and Comparative Examples 6-7 was tested, and the reduction rate of the thermal conductivity relative to Comparative Example 3 is shown in Table 3:
[0108] Table 3 Reduction rate of thermal conductivity of materials prepared in Examples 7-9 and Comparative Examples 6-7
[0109]
[0110] As can be seen from Table 3, the amount of additive added has an impact on the thermal insulation performance of the material. When the additive content is too low, the amount of bubbles generated is small, and the thermal conductivity is higher than that in Comparative Example 3. When the additive content is too high, uneven distribution is prone to occur. Therefore, it is necessary to control the additive content to a suitable range to ensure the thermal insulation performance of the material. When the additive content is 3%, it is equivalent to an additive content of 5%. From a cost perspective, it is sufficient to choose less than 3%.
[0111] In summary, it can be seen from the results in Tables 1 to 3 above that the materials prepared by the present invention have lower thermal conductivity and significantly improved thermal insulation performance compared to the materials prepared by the traditional method.
[0112] Obviously, those skilled in the art can make various changes and modifications to the present invention without departing from the spirit and scope of the present invention. Thus, if these modifications and variations of the present invention fall within the scope of the claims of the present invention and their equivalents, they are also intended to be included.
Claims
1. A method for preparing a foam aluminum wall insulation material, characterized in that: The following steps are involved: An aluminum oxide shell layer is deposited on the surface of calcium carbonate by chemical vapor deposition to prepare an additive with a core-shell structure; Aluminum is heated and melted to prepare an aluminum melt; the additive is added to the aluminum melt, stirred evenly, and then the temperature is increased to decompose the calcium carbonate in the additive to perform foaming treatment, and then the mixture is placed in a mold to be cooled to prepare a foamed aluminum wall insulation material.
2. The preparation method according to claim 1, characterized in that: The calcium carbonate is placed in a reaction chamber of a chemical vapor deposition device, a protective gas is introduced to expel the air, and then Al(CH3)3 is introduced using the protective gas as a carrier gas, and then H2O is introduced. Al(CH3)3 and H2O are deposited and reacted on the surface of the calcium carbonate to form an aluminum oxide shell layer.
3. The preparation method according to claim 2, characterized in that: During the introduction of Al(CH3)3, the temperature was controlled at 200-210°C and the introduction time was 10-20s; during the introduction of H2O, the temperature was controlled at 200-210°C and the introduction time was 15-25s.
4. The preparation method according to claim 1, characterized in that: The calcium carbonate is spherical and has a particle size of 50-80 μm.
5. The preparation method according to claim 1, characterized in that: The thickness of the alumina shell is 5-10 μm.
6. The preparation method according to claim 1, characterized in that: The amount of additive added is 1-3% of the mass of the aluminum melt.
7. The preparation method according to claim 1, characterized in that: Raise the temperature to 900-910℃ to decompose calcium carbonate, and keep warm for 30-40 minutes.
8. The preparation method according to claim 1, characterized in that: The stirring temperature is 730-750°C.
9. The preparation method according to claim 1, characterized in that: The temperature at which aluminum is heated to melt is 670-700°C.
10. A foamed aluminum wall insulation material prepared according to the preparation method according to any one of claims 1 to 9.