Methods of depositing interstitial fill fluids and related systems and devices
By filling the gaps in the substrate with flowable intermediate materials treated with phosphorus compounds and moisture during the manufacturing process of semiconductor devices, the problem of difficulty in filling high-aspect ratio trenches in the existing technology is solved, and seamless filling and high-density trenches are achieved. Device manufacturing.
Patent Information
- Application Number
- CN202410412575.8
- Authority / Receiving Office
- CN · China
- Patent Type
- Applications(China)
- Current Assignee / Owner
- Priority Date
- 2023-04-06
- Filing Date
- 2024-04-08
- Publication Date
- 2024-10-15
AI Technical Summary
Existing deposition processes are difficult to effectively fill gaps in high aspect ratio trenches, resulting in gaps and seams during the manufacturing process of semiconductor devices, affecting device performance and density.
By forming a first layer containing silicon and nitrogen on a substrate and subjecting it to a phosphorus-containing compound and moisture, a flowable intermediate material is formed to fill the gap, using multiple deposition cycles and plasma treatments to ensure seamless filling.
It achieves efficient filling of gaps in high-aspect ratio trenches, avoids the formation of gaps and seams, and improves the density and performance of semiconductor devices.
Smart Images

Figure CN118773583A_ABST
Abstract
Description
Technical Field
[0001] The present disclosure generally relates to methods and systems suitable for forming electronic devices. More specifically, the present disclosure relates to methods and systems that can be used to deposit materials in gaps, trenches, etc. by plasma assisted deposition. Background Art
[0002] The reduction in size of semiconductor devices has led to a significant increase in the speed and density of integrated circuits. However, as the wiring pitch of large-scale integrated devices is miniaturized, due to the limitations of existing deposition processes, void-free filling of high aspect ratio trenches (e.g., trenches with an aspect ratio of 3 or higher) becomes increasingly important. Therefore, there is still a need for a process for effectively filling high aspect ratio features (e.g., gaps such as trenches on semiconductor substrates).
[0003] Any discussion set forth in this section, including discussion of problems and solutions, has been included in the present disclosure merely to provide context for the present disclosure. Such discussion should not be construed as an admission that any or all of the present inventions are previously known or constitute prior art. Summary of the invention
[0004] Various embodiments of the present disclosure relate to gap filling methods, structures and devices formed using such methods, and apparatus for performing such methods and / or for forming such structures and / or devices. The manner in which various embodiments of the present disclosure address the shortcomings of existing methods and systems is discussed in more detail below.
[0005] A method for filling a gap in a substrate is also described. The method includes providing a substrate into a reaction chamber, wherein the substrate includes at least one gap; forming a first layer on the substrate, wherein the first layer includes silicon and nitrogen; subjecting the first layer to a phosphorus-containing compound to form a flowable intermediate material that at least partially fills the at least one gap on the substrate, wherein the intermediate material includes silicon, oxygen, and hydrogen; and forming a solid material including silicon.
[0006] In some embodiments, subjecting the first layer to the phosphorus-containing compound further comprises subjecting the first layer to moisture.
[0007] In some embodiments, the moisture is selected from H2O, steam, or H2O2.
[0008] In some embodiments, the solid material comprises silicon dioxide.
[0009] In some embodiments, the phosphorus-containing compound comprises an amount of phosphorus such that the first layer comprises at least 4 atomic % phosphorus after being subjected to the phosphorus-containing compound.
[0010] In some embodiments, the step of forming the first layer includes performing a plurality of deposition cycles to form the silicon-containing layer. The deposition cycles include a silicon precursor pulse, which includes exposing the substrate to a silicon precursor; and a plasma pulse, which includes exposing the substrate to a plasma treatment, wherein the plasma treatment includes generating a plasma.
[0011] In some embodiments, subsequent deposition cycles are separated by purges.
[0012] In some embodiments, the precursor pulse and the plasma pulse at least partially overlap.
[0013] In some embodiments, the plasma is a direct plasma. In some embodiments, the plasma is a remote plasma. In some embodiments, the plasma is an indirect plasma.
[0014] In some embodiments, the plasma is generated using a plasma gas comprising N 2 and optionally one or more noble gases.
[0015] In some embodiments, the noble gas includes one or more of He and Ar.
[0016] In some embodiments, the silicon precursor includes silicon and optionally phosphorus.
[0017] In some embodiments, the method includes one or more super cycles including the steps of forming a first layer on a substrate, subjecting the first layer to a phosphorus-containing compound, and forming a solid material comprising silicon.
[0018] Further described herein is a semiconductor processing apparatus. The apparatus comprises: a reaction chamber comprising a substrate support for supporting a substrate; a heater constructed and arranged to heat a substrate in the reaction chamber; a plasma module comprising a radio frequency power source constructed and arranged to generate plasma; a plasma gas source in fluid communication with the plasma module; a silicon precursor source in fluid communication with the reaction chamber via one or more precursor valves; and a controller configured to cause the semiconductor processing apparatus to perform a method according to the method described herein.
[0019] This summary is provided to introduce some concepts in a simplified form. These concepts are further described in detail in the detailed description of the exemplary embodiments of the present disclosure below. This summary is not intended to identify the key features or essential features of the claimed subject matter, nor is it intended to be used to limit the scope of the claimed subject matter. BRIEF DESCRIPTION OF THE DRAWINGS
[0020] A more complete understanding of embodiments of the present disclosure can be obtained by referring to the detailed description and claims when considered in conjunction with the following illustrative drawings.
[0021] Figure 1 A schematic diagram showing an embodiment of the method described herein is shown.
[0022] Figure 2 A schematic diagram showing an embodiment of the method described herein is shown.
[0023] Figure 3 A schematic diagram showing an embodiment of the method described herein is shown.
[0024] Figure 4 A deposition assembly 400 according to the present disclosure is shown in schematic form.
[0025] It should be understood that the elements in the drawings are shown for simplicity and clarity and are not necessarily drawn to scale. For example, the sizes of some elements in the drawings may be exaggerated relative to other elements to help improve the understanding of the illustrated embodiments of the present disclosure. DETAILED DESCRIPTION
[0026] Although certain embodiments and examples are disclosed below, it will be appreciated by those skilled in the art that the present invention extends beyond the specifically disclosed embodiments and / or uses of the present invention and their obvious modifications and equivalents. Therefore, it is intended that the scope of the disclosed invention should not be limited by the specifically disclosed embodiments described below.
[0027] In the present disclosure, "gas" may include materials that are gaseous at normal temperature and pressure (NTP), evaporated solids and / or evaporated liquids, and may be composed of a single gas or a gas mixture depending on the context. Gases other than process gases, i.e., gases that are not introduced through gas distribution components, other gas distribution devices, etc., may be used, for example, to seal reaction spaces, and may include sealing gases, such as rare gases. In some cases, the term "precursor" may refer to a compound that participates in a chemical reaction that produces another compound, particularly a compound that constitutes a membrane matrix or a main skeleton of a membrane; the term "reactant" may be used interchangeably with the term precursor. Exemplary gases may include precursors and reactants.
[0028] As used herein, the term "comprising" means including certain features but does not exclude the presence of other features as long as they do not make the claim or embodiment unworkable. In some embodiments, the term "comprising" includes "consisting of". As used herein, the term "consisting of" means that other features are not present in the device / method / product except for the features following the phrase. When the term "consisting of" is used to refer to a compound or substance, it means that the compound contains only the listed ingredients.
[0029] As used herein, the term "consists of" means that other features are not present in the apparatus / method / product other than those following the phrase. When the term "consists of" is used to refer to a compound, substance, or composition of matter, it means that the compound, substance, or composition of matter contains only the listed ingredients. Nevertheless, in some embodiments, the compound, substance, or composition of matter may include other ingredients in addition to the listed ingredients as trace elements or impurities.
[0030] As used herein, the term "substrate" may refer to any one or more underlying materials, including any one or more underlying materials that may be modified or on which a device, circuit, or film may be formed. A "substrate" may be continuous or non-continuous; rigid or flexible; solid or porous; and combinations thereof. A substrate may be in any form, such as a plate or a workpiece. A plate-like substrate may include wafers of various shapes and sizes. A substrate may be made of semiconductor materials, including, for example, silicon, silicon germanium, silicon oxide, gallium arsenide, gallium nitride, and silicon carbide.
[0031] The continuous substrate may extend beyond the boundaries of the processing chamber in which the deposition process occurs. In some processes, the continuous substrate may be moved through the processing chamber so that the process continues until the end of the substrate is reached. The continuous substrate may be provided by a continuous substrate feeding system to allow the continuous substrate to be manufactured and output in any suitable form.
[0032] Non-limiting examples of continuous substrates may include sheets, nonwoven films, rolls, foils, meshes, flexible materials, bundles of continuous filaments or fibers (eg, ceramic fibers or polymer fibers). Continuous substrates may also include carriers or sheets on which non-continuous substrates are mounted.
[0033] It should be understood that the term "deposition" and the like as used herein may refer to a phase change from a gas phase to a solid phase through an intermediate mobile phase. In fact, the meaning of the term "deposition" may include a phase change from a gas phase to a liquid phase, and may include a process whereby a gaseous reactant forms a liquid, a liquid-like state, or a solidified fluid. Thus, the meaning of the term "deposition" may include similar terms such as condensation or formation.
[0034] In addition, in the present disclosure, any two numbers of a variable may constitute the workable range of the variable, and any range indicated may include or exclude endpoints. In addition, any values of the variables indicated (whether or not they are expressed as "about") may refer to exact values or approximate values, and include equivalents, and may refer to average values, medians, representative values, majority values, etc. In addition, in the present disclosure, the terms "include", "consist of" and "have" independently refer to "usually or broadly include", "comprise", "essentially consist of" or "consist of" in some embodiments. In the present disclosure, the meaning of any definition does not necessarily exclude common and customary meanings in some embodiments.
[0035] As used herein, the terms "film" and / or "layer" may refer to any continuous or discontinuous structure and material, such as a material deposited by the methods disclosed herein. For example, the film and / or layer may include a two-dimensional material, a three-dimensional material, nanoparticles, a partial or complete molecular layer or a partial or complete atomic layer or a cluster of atoms and / or molecules. The film or layer may be composed in part or in whole of a plurality of dispersed atoms on a substrate surface and / or embedded in a substrate and / or embedded in a device manufactured on the substrate. The film or layer may include a material or layer having pinholes and / or islands. The film or layer may be at least partially continuous. The film or layer may be patterned, such as subdivided, and may be included in a plurality of semiconductor devices.
[0036] As used herein, a "structure" may be or include a substrate as described herein. A structure may include one or more layers covering a substrate, such as one or more layers formed according to a method as described herein. Device portions and interconnects may be or include a structure.
[0037] As used herein, the term "deposition process" may refer to the introduction of precursors (and / or reactants) into a reaction chamber to deposit a layer on a substrate. A "cyclic deposition process" is an example of a "deposition process".
[0038] The term "cyclic deposition process" or "cyclic deposition process" may refer to sequentially exposing a substrate to precursors (and / or reactants) entering a reaction chamber and exposing the substrate to plasma-generated species to deposit layers on the substrate, and includes processing techniques such as plasma enhanced atomic layer deposition (PEALD).
[0039] Typically, for a PEALD process, during each cycle, a precursor is introduced into the reaction chamber and chemically adsorbed to a deposition surface (e.g., a substrate surface that may include previously deposited material or other material from a previous PEALD cycle) and forms a monolayer or sub-monolayer of material that does not readily react with additional precursors (i.e., a self-limiting reaction). Thereafter, the substrate is exposed to a plasma-generated substance that may be generated using any plasma, such as a direct, indirect, or remote plasma. The plasma may be generated capacitively, inductively, using microwave radiation, or by other means. The plasma-generated substance converts the chemically adsorbed precursor into the desired material on the deposition surface. A purge step may be used during one or more cycles, such as after each step or pulse of each cycle, to remove any excess precursor from the processing chamber and / or to remove any excess plasma-generated substance and / or reaction byproducts from the reaction chamber.
[0040] As used herein, the term "purge" may refer to the process of providing a purge gas to a reaction chamber between a precursor pulse and a plasma pulse. It should be understood that during the purge, the substrate is not exposed to the material generated by the plasma. For example, when using direct plasma, the plasma can be turned off during the purge process. For example, a purge can be provided between a precursor pulse and a reactant pulse, for example, using a purge gas such as nitrogen or a rare gas, so as to avoid or at least minimize the gas phase interaction between the precursor and the reactant. It should be understood that the purge can be performed in time or space, or both. For example, in the case of a time purge, a purge step can be used, for example, in a time sequence of providing a first precursor to a reaction chamber, providing a purge gas to the reaction chamber, and providing a second precursor to the reaction chamber, wherein the substrate on which the layer is deposited does not move. For example, in the case of a space purge, the purge step can take the following form: the substrate is moved from a first position where the first precursor is continuously supplied to a second position where the second precursor is continuously supplied through a purge gas curtain.
[0041] As used herein, "precursor" includes a gas or material that can be changed into a gaseous state and can be represented by a chemical formula that includes elements that can be introduced into the deposition process described herein.
[0042] In some embodiments, the term "gap filling fluid", also referred to as "flowable gap filling" or "flowable intermediate material", may refer to an oligomer that is liquid under the conditions deposited on a substrate and has the ability to crosslink and be used as a solid film.
[0043] In some embodiments, the term "filling ability" can refer to the ability to fill gaps with substantially no voids (e.g., no voids with a diameter of about 5 nm or more) and seams (e.g., no seams with a length of about 5 nm or more), wherein seamless / void-free bottom-up growth of the layer is observed. In some embodiments, the growth at the bottom of the gap can be at least about 1.5 times faster than the growth on the sidewalls of the gap and the top surface with the gap. A film with filling ability can be referred to as a "flowable film" or a "viscous film". The flowable or viscous behavior of the film is generally manifested as a concave surface at the bottom of the groove.
[0044] In the present disclosure, the depressions between adjacent protruding structures and any other recessed patterns may be referred to as "grooves" or "gaps". That is, a groove or gap may refer to any recessed pattern including a hole / through hole. In some embodiments, the groove or gap may have a width of about 5 nm to about 150 nm, or about 30 nm to about 50 nm, or about 5 nm to about 10 nm, or about 10 nm to about 20 nm, or about 20 nm to about 30 nm, or about 50 nm to about 100 nm, or about 100 nm to about 150 nm. When the length of a groove or gap is substantially the same as its width, it may be referred to as a hole or through hole. A hole or through hole typically has a width of about 20 nm to about 100 nm. In some embodiments, the depth of the groove is about 30 nm to about 100 nm, typically about 40 nm to about 60 nm. In some embodiments, the aspect ratio of the groove or gap is about 2 to about 10, typically about 2 to about 5. The size of the groove or gap may vary depending on processing conditions, film composition, intended application, etc.
[0045] A method for filling a gap in a substrate is described herein. The gap in the substrate may refer to a patterned recess or trench in the substrate. The gap filling method may be used in the manufacturing process of various semiconductor devices, including but not limited to cell isolation in 3D cross-point memory devices, self-aligned vias, dummy gates, reverse tone patterning, PC RAM isolation, cutting hard mask, and DRAM storage node contact isolation.
[0046] In particular, the presently described method includes providing a substrate into a reaction chamber. The substrate includes at least one gap. The method also includes forming a first layer on the substrate, wherein the first layer includes silicon and nitrogen; subjecting the first layer to a phosphorus-containing compound to form a flowable intermediate material that at least partially fills the at least one gap on the substrate, wherein the intermediate material includes silicon, oxygen, and hydrogen; and forming a solid material including silicon.
[0047] In some embodiments, the method includes completely filling the gap with the flowable intermediate material. In some embodiments, the method includes filling the gap with the flowable intermediate material without forming voids or seams. In other words, in some embodiments, the process according to the present method continues until the gap is completely filled with the material having the filling capacity, and substantially no voids or seams are formed in the filled gap. By studying the formed material in a scanning tunneling electron microscope, the presence of voids or seams can be observed.
[0048] In some embodiments, the gap has a depth of at least 5 nm to at most 500 nm, or at least 10 nm to at most 250 nm, or at least 20 nm to at most 200 nm, or at least 50 nm to at most 150 nm, or at least 100 nm to at most 150 nm.
[0049] In some embodiments, the gap has a width of at least 10 nm to at most 10000 nm, or at least 20 nm to at most 5000 nm, or at least 40 nm to at most 2500 nm, or at least 80 nm to at most 1000 nm, or at least 100 nm to at most 500 nm, or at least 150 nm to at most 400 nm, or at least 200 nm to at most 300 nm.
[0050] In some embodiments, the gap has a length of at least 10 nm to at most 10000 nm, or at least 20 nm to at most 5000 nm, or at least 40 nm to at most 2500 nm, or at least 80 nm to at most 1000 nm, or at least 100 nm to at most 500 nm, or at least 150 nm to at most 400 nm, or at least 200 nm to at most 300 nm.
[0051] In some embodiments, the distance that the flowable intermediate material extends into a particular gap is equal to at least 1.0 to at most 10.0 times the width of the gap. In some embodiments, the distance that the flowable intermediate material extends into a particular gap is equal to at least 1.5 to at most 9.0 times the width of the gap. In some embodiments, the distance that the flowable intermediate material extends into a particular gap is equal to at least 2.0 to at most 8.0 times the width of the gap. In some embodiments, the distance that the flowable intermediate material extends into a particular gap is equal to at least 3.0 to at most 6.0 times the width of the gap. In some embodiments, the distance that the flowable intermediate material extends into a particular gap is equal to at least 4.0 to at most 6.0 times the width of the gap. In some embodiments, the distance that the flowable intermediate material extends into a particular gap is equal to about 5.0 times the width of the gap. In other words, in some embodiments, the flowable intermediate material fills the gap up to any of the above distances from the bottom of the gap.
[0052] In some embodiments, the step of subjecting the first layer to a phosphorus-containing compound further comprises subjecting the first layer to moisture. In this disclosure, the term "moisture" refers to the presence of water or other fluids diffused as vapor or condensed on a surface. In some embodiments, moisture includes water molecules, in other words, H + HO - In some embodiments, the water is selected from H2O, steam or H2O2.
[0053] In some embodiments, the first layer further comprises oxygen. In some embodiments, the phosphorus-containing compound further comprises oxygen. In some embodiments, the first layer further comprises a phosphorus-containing compound. In some embodiments, when the first layer is subjected to the phosphorus-containing compound and the oxygen- and hydrogen-containing compound and the material polymerizes, a flowable intermediate material is obtained. The oxygen- and hydrogen-containing compound may be present in the first layer itself, in the phosphorus-containing compound, or alternatively in the moisture subjected to it. As a result, the first layer subjected to the phosphorus-containing compound and the oxygen- and hydrogen-containing compound reacts to form a flowable intermediate material comprising silicon, hydrogen, and oxygen.
[0054] The solid material is a material that flows into the gap and at least partially fills it. In some embodiments, the solid material comprises silicon dioxide. In some embodiments, the solid material comprises silicon nitride. In some embodiments, the solid material comprises silicon oxynitride.
[0055] In some embodiments, the phosphorus-containing compound comprises an amount of phosphorus such that the first layer comprises at least 2 atomic % phosphorus after being subjected to the phosphorus-containing compound. In some embodiments, the phosphorus-containing compound comprises an amount of phosphorus such that the first layer comprises at least 4 atomic % phosphorus after being subjected to the phosphorus-containing compound. In some embodiments, the phosphorus-containing compound comprises an amount of phosphorus such that the first layer comprises at least 6 atomic % phosphorus after being subjected to the phosphorus-containing compound. In some embodiments, the phosphorus-containing compound comprises an amount of phosphorus such that the first layer comprises at least 8 atomic % phosphorus after being subjected to the phosphorus-containing compound. In some embodiments, the phosphorus-containing compound comprises an amount of phosphorus such that the first layer comprises less than 12 atomic % phosphorus after being subjected to the phosphorus-containing compound. In some embodiments, the phosphorus-containing compound comprises an amount of phosphorus such that the first layer comprises less than 10 atomic % phosphorus after being subjected to the phosphorus-containing compound.
[0056] In some embodiments, the step of forming the first layer includes performing a plurality of deposition cycles to form the silicon-containing layer. The deposition cycles include a silicon precursor pulse, which includes exposing the substrate to a silicon precursor; and a plasma pulse, which includes exposing the substrate to a plasma treatment, wherein the plasma treatment includes generating a plasma.
[0057] In some embodiments, the first layer comprises silicon and nitrogen. In some embodiments, the first layer comprises silicon nitride. In some embodiments, the first layer comprises silicon, nitrogen, and phosphorus.
[0058] In some embodiments, the step of forming the first layer further includes a phosphorus precursor pulse, which includes exposing the substrate to a phosphorus precursor.
[0059] In some embodiments, subsequent deposition cycles are separated by purges.
[0060] In some embodiments, the precursor pulses and the plasma pulses at least partially overlap. In other words, in some embodiments, the precursor pulses and the plasma pulses occur at least partially simultaneously. In such embodiments, the cyclic deposition process does not include an intra-cycle purge. In some embodiments, the cyclic deposition process does not include an inter-cycle purge.
[0061] In some embodiments, the plasma is a direct plasma. In some embodiments, the plasma is a remote plasma. In some embodiments, the plasma is an indirect plasma.
[0062] In some embodiments, plasma is generated using a plasma gas that includes N2 and optionally one or more rare gases. In some embodiments, the rare gas includes one or more of He and Ar.
[0063] In some embodiments, the plasma gas is continuously provided to the reaction chamber. In some embodiments, the plasma gas is supplied to the reaction chamber as a carrier gas (i.e., as a gas to entrain the precursor) and / or as an additional gas. In some embodiments, the carrier gas is provided at a flow rate of at least 0.2 to at most 6.0 slpm, or at least 0.3 to at most 4 slpm, or at least 0.4 to at most 2 slpm, or at least 0.5 to at most 1 slpm.
[0064] In some embodiments, the plasma pulse comprises generating an RF plasma in the reaction chamber. In some embodiments, a plasma power of at least 10 W to at most 2000 W is used during the plasma pulse. In some embodiments, a plasma power of at least 100 W to at most 1500 W is used during the plasma pulse. In some embodiments, a plasma power of at least 300 W to at most 1000 W is used during the plasma pulse.
[0065] In some embodiments, the method is performed in a system comprising two electrodes, with the substrate being located between the two electrodes. The electrodes are positioned in parallel at a predetermined distance referred to as an electrode gap. In some embodiments, the electrode gap is at least 5 mm to at most 30 mm, at least 5 mm to at most 10 mm, or at least 10 mm to at most 20 mm, or at least 20 mm to at most 30 mm.
[0066] In some embodiments, a plasma frequency of at least 40 kHz to at most 2.45 GHz is used during the plasma pulses, or a plasma frequency of at least 40 kHz to at most 80 kHz is used during the plasma pulses, or a plasma frequency of at least 80 kHz to at most 160 kHz is used during the plasma pulses, or a plasma frequency of at least 160 kHz to at most 320 kHz is used during the plasma pulses, or a plasma frequency of at least 320 kHz to at most 640 kHz is used during the plasma pulses, or a plasma frequency of at least 640 kHz to at most 1280 kHz is used during the plasma pulses, or a plasma frequency of at least 1280 kHz to at most 2500 kHz is used during the plasma pulses, or a plasma frequency of at least 2.5 MHz to at least 5 MHz is used during the plasma pulses, or a plasma frequency of at least 5 MHz to at most 50 MHz is used during the plasma pulses, or a plasma frequency of at least 10 MHz to at most 150 MHz is used during the plasma pulses. A plasma frequency of at least 5 MHz to at most 10 MHz is used, or a plasma frequency of at least 10 MHz to at most 20 MHz is used during plasma pulses, or a plasma frequency of at least 20 MHz to at most 30 MHz is used during plasma pulses, or a plasma frequency of at least 30 MHz to at most 40 MHz is used during plasma pulses, or a plasma frequency of at least 40 MHz to at most 50 MHz is used during plasma pulses, or a plasma frequency of at least 50 MHz to at most 100 MHz is used during plasma pulses, or a plasma frequency of at least 100 MHz to at most 200 MHz is used during plasma pulses, or a plasma frequency of at least 200 MHz to at most 500 MHz is used during plasma pulses, or a plasma frequency of at least 500 MHz to at most 1000 MHz is used during plasma pulses, or a plasma frequency of at least 1 GHz to at most 2.45 GHz is used during plasma pulses. In an exemplary embodiment, the plasma is an RF plasma, and the RF power is provided at a frequency of 13.56 MHz.
[0067] In some embodiments, during the silicon precursor pulse and during the plasma pulse, no gas other than the silicon precursor and the plasma gas is introduced into the reaction chamber. Additionally or alternatively, in some embodiments, during at least one of the intra-cycle purge and the inter-cycle purge, no gas other than nitrogen and the optional noble gas is introduced into the reaction chamber.
[0068] In some embodiments, the method includes intermittently providing the precursor to the reaction space and applying the plasma continuously. Thus, in some embodiments, a continuous plasma is used instead of a plasma pulse. In some embodiments, the method includes intermittently providing the precursor to the reaction space and applying the plasma intermittently. Thus, in some embodiments, the silicon precursor is continuously provided to the reaction chamber and the plasma is intermittently generated.
[0069] In some embodiments, a pulsed plasma, such as a pulsed RF plasma, is generated in the reaction chamber. Thus, the method comprises a plurality of cycles, one cycle comprising a plasma-on pulse and a plasma-off pulse. In some embodiments, the plasma-on pulse lasts at least 0.7 seconds to at most 7.0 seconds, such as at least 0.7 seconds to at most 1.5 seconds. In some embodiments, the plasma-off pulse lasts at least 0.7 seconds to at most 2.0 seconds, such as at least 0.7 seconds to at most 1.5 seconds.
[0070] In some embodiments, the duration of the precursor pulse, ie, the precursor supply time, is at least 0.25 seconds to at most 4.0 seconds, or at least 0.5 seconds to at most 2.0 seconds, or at least 1.0 seconds to at most 1.5 seconds.
[0071] In some embodiments, the duration of the purge is at least 0.025 seconds to at most 2.0 seconds, or at least 0.05 seconds to at most 0.8 seconds, or at least 0.1 seconds to at most 0.4 seconds, or at least 0.2 seconds to at most 0.3 seconds.
[0072] In some embodiments, the silicon precursor includes silicon. In some embodiments, the silicon precursor further includes phosphorus. It should be understood that when the silicon precursor is composed of certain components, in some embodiments, other components may still be present in small amounts, for example as contaminants.
[0073] In some embodiments, the method includes one or more super cycles including the steps of forming a first layer on a substrate, subjecting the first layer to a phosphorus-containing compound, and forming a solid material comprising silicon.
[0074] In some embodiments, the method for filling the gap comprises at least 10 to at most 30,000 super cycles, or at least 10 to at most 3,000 super cycles, or at least 10 to at most 1,000 super cycles, or at least 10 to at most 500 super cycles, or at least 20 to at most 200 super cycles, or at least 50 to at most 150 super cycles, or at least 75 to at most 125 super cycles, for example 100 super cycles.
[0075] In some embodiments, the gap is completely filled with a flowable intermediate material. It should be understood that the flowable intermediate material can be described as a viscous material, i.e., a viscous phase deposited on a substrate. The flowable intermediate material is capable of flowing in the grooves on the substrate. Suitable substrates include silicon wafers. Therefore, the viscous material seamlessly fills the grooves in a bottom-up manner.
[0076] In some embodiments, the method is carried out at a temperature of at least -25°C to at most 800°C. In some embodiments, the method is carried out at a temperature of at least -25°C to at most 0°C. In some embodiments, the method is carried out at a temperature of at least 0°C to at most 25°C. In some embodiments, the method is carried out at a temperature of at least 25°C to at most 50°C. In some embodiments, the method is carried out at a temperature of at least 50°C to at most 75°C. In some embodiments, the method is carried out at a temperature of at least 150°C to at most 400°C. In some embodiments, the method is carried out at a temperature of at least 400°C to at most 700°C. This enhances the gap filling performance of the flowable intermediate material currently provided. In some embodiments, the temperature of the reaction chamber is at least 70°C to at most 90°C.
[0077] In some embodiments, the reaction chamber is maintained at a pressure of at least 600 Pa to at most 10,000 Pa. For example, the pressure in the reaction chamber can be maintained at a pressure of at least 600 Pa to at most 1,200 Pa, or at least 1,200 Pa to at most 2,500 Pa, or at least 2,500 Pa to at most 5,000 Pa, or at least 5,000 Pa to at most 10,000 Pa.
[0078] In some embodiments, the method is performed at a pressure of at least 500 Pa, preferably at a pressure of at least 700 Pa. More preferably, the method is performed at a pressure of at least 900 Pa. This enhances the gap-filling properties of the presently provided flowable intermediate material.
[0079] In some embodiments, the reaction chamber is maintained at a pressure of at least 500Pa to at most 1500Pa, and the reaction chamber is maintained at a temperature of at least 50°C to at most 150°C. In some embodiments, the method is performed at a pressure of at least 500Pa to at most 10000Pa and a temperature of at least 50°C to at most 200°C. In some embodiments, the method is performed at a pressure of at least 700Pa and a temperature of at least 50°C to at most 150°C. In some embodiments, the method is performed at a pressure of at least 900Pa and a temperature of at least 50°C to at most 75°C. In some embodiments, the method is performed at a pressure of about 1atm and a temperature of at least 50°C to at most 150°C.
[0080] According to an exemplary embodiment, when the gap filling step is completed, the flowable film is no longer flowable but solidified, so no separate curing process is required. In other embodiments, after the gap is filled, the flowable film is densified and / or solidified. Densifying and / or solidifying the flowable film can be accomplished by a curing step (also referred to as "curing").
[0081] Therefore, in some embodiments, the method includes a step of curing the flowable intermediate material. This step increases the thermal resistance of the flowable intermediate material. In other words, it increases the ability of the flowable intermediate material to resist deformation and / or mass loss at high temperatures. Additionally or alternatively, the curing step may solidify the flowable intermediate material.
[0082] In some embodiments, the flowable intermediate material is solidified after filling the gap. Optionally, after the flowable intermediate material fills the gap and before the solidification step, the flowable intermediate material is subjected to annealing. Suitable annealing times include from at least 10.0 seconds to at most 10.0 minutes, for example from at least 20.0 seconds to at most 5.0 minutes, for example from at least 40.0 seconds to at most 2.5 minutes. In some embodiments, the annealing time includes from at least 20 minutes to at most 60 minutes. Suitably, the annealing is carried out in a gas mixture comprising one or more gases selected from N2, He, Ar and H2. In some embodiments, the annealing is carried out at a temperature of at least 200°C, or at a temperature of at least 250°C, or at a temperature of at least 300°C, or at a temperature of at least 350°C, or at a temperature of at least 400°C, or at a temperature of at least 450°C. In some embodiments, the annealing is carried out at a temperature of at least 600°C to at most 800°C.
[0083] In some embodiments, the flowable intermediate material can be cured while filling the gap, for example by cyclically alternating filling the gap and curing pulses. Thus, in some embodiments, the methods described herein include one or more super cycles. A super cycle includes the following steps: performing a step of filling the gap and a step of curing. When a super cycle is repeated multiple times, a cyclic process is generated. When the currently disclosed method includes only one super cycle, the process results in the flowable intermediate material first filling the gap and then being cured.
[0084] In some embodiments, the curing step includes generating a plasma in a reaction chamber, thereby exposing the substrate to a direct plasma. Suitable direct plasmas include rare gas plasmas. When using direct plasma, a thin layer of flowable intermediate material can be effectively cured, producing a thin, high-quality layer. In some embodiments, particularly when a thicker layer of solidified flowable intermediate material is required, the method of filling the gap may include multiple cycles, wherein the steps of filling the gap with the flowable intermediate material and the curing step of using direct plasma treatment are alternately performed. In such an embodiment, the process of filling the gap preferably includes multiple cycles of steps for filling the gap, and the plasma treatment steps (also referred to as pulses) are alternately performed. The advantage of this cyclic process is that a larger portion of the flowable intermediate material is cured: the direct plasma can have a penetration depth of about 2 to 7 nm, so that the direct plasma treatment after deposition will only cure the top layer of the flowable intermediate material. In contrast, alternating the gap filling step and the plasma step allows a larger portion or even all of the flowable intermediate material to be cured, even when a curing technique that may have a low penetration depth is used, such as direct plasma.
[0085] Suitable plasma treatments include H2 plasma, O2 plasma, He plasma, H2 / He plasma, Ar plasma, Ar / O2, He / O2, N2 / O2, Ar / H2 plasma, and Ar / He / H2 plasma. It should be understood that H2 plasma refers to a plasma that uses H2 as a plasma gas. In addition, it should be understood that H2 / He plasma refers to a plasma that uses a mixture of H2 and He as a plasma gas. It should be understood that other plasmas are similarly defined.
[0086] In some embodiments, the curing step includes providing a remote plasma, such as a remote rare gas plasma, and exposing the substrate to one or more excited species, such as at least one of free radicals, ions, and UV radiation. In some embodiments, the curing step includes using an indirect plasma after filling the gap with the flowable intermediate material. The indirect plasma can have a greater penetration depth than the direct plasma, thereby avoiding the need for cyclic gap filling steps and curing steps. Therefore, the indirect plasma curing can be applied after the gap filling step.
[0087] In certain embodiments, the curing step comprises providing a remote plasma source, and one or more screens are positioned between the remote plasma source and the substrate. Therefore, the substrate can be exposed to the free radicals generated by the remote plasma source. The penetration depth of the free radical is significantly higher than the penetration length provided by the direct plasma, for example, significantly higher than the size of the gap filled by the method currently provided. Therefore, after all flowable intermediate materials are formed, a remote plasma process can be advantageously applied. Nevertheless, similar to the operation of the direct plasma, remote plasma curing can also be cyclically applied with alternating plasma curing and flowable intermediate material formation steps. The large penetration depth of remote plasma has the advantage that they allow the flowable intermediate material to be effectively cured. In certain embodiments, the plasma gas adopted in the remote plasma comprises a rare gas, for example, a rare gas selected from He and Ar.
[0088] The curing step may reduce the hydrogen concentration of the flowable intermediate material relative to its uncured state. For example, the hydrogen concentration is reduced by at least 0.01 atomic % to at most 0.1 atomic %, or by at least 0.1 atomic % to at most 0.2 atomic %, or by at least 0.2 atomic % to at most 0.5 atomic %, or by at least 0.5 atomic % to at most 1.0 atomic %, or by at least 1.0 atomic % to at most 2.0 atomic %, or by at least 2.0 atomic % to at most 5.0 atomic %, or by at least 5.0 atomic % to at most 10.0 atomic %.
[0089] In some embodiments, the curing step includes exposing the flowable intermediate material to a micropulse plasma. Applying a micropulse plasma may be particularly advantageous because the formed flowable intermediate material contains hydrogen. A micropulse plasma is a plasma treatment that includes applying a plurality of rapid successive on-off micropulses. A micropulse plasma may, for example, employ a rare gas as a plasma gas. When a 300 mm wafer is used as a substrate, a plasma gas flow rate of, for example, at least 5.0 slm, or at least 5.0 slm to at most 7.0 slm, or at least 7.0 slm to at most 10.0 slm is maintained during the micropulse plasma. For example, the on micropulse in the micropulse plasma can last from at least 1.0 microsecond to at most 1.0 second, or from at least 2.0 microseconds to at most 0.50 second, or from at least 5.0 microseconds to at most 250 milliseconds, or from at least 10.0 microseconds to at most 100.0 milliseconds, or from at least 25.0 microseconds to at most 50.0 milliseconds, or from at least 50.0 microseconds to at most 25.0 milliseconds, or from at least 100.0 microseconds to at most 10.0 milliseconds, or from at least 250.0 microseconds to at most 5.0 milliseconds, or from at least 0.50 milliseconds to at most 2.5 milliseconds. For example, the closed micropulse in the micropulse plasma can last at least 1.0 microsecond to at most 2.0 seconds, or at least 2.0 microseconds to at most 1.0 second, or at least 5.0 microseconds to at most 500 milliseconds, or at least 10.0 microseconds to at most 250.0 milliseconds, or at least 25.0 microseconds to at most 100.0 milliseconds, or at least 50.0 microseconds to at most 50.0 milliseconds, or at least 100.0 microseconds to at most 25.0 milliseconds, or at least 200.0 microseconds to at most 10.0 milliseconds, or at least 500.0 microseconds to at most 5.0 milliseconds, or at least 1.0 millisecond to at most 2.0 milliseconds. The micropulse plasma can be used cyclically, i.e., as a plasma pulse in a cyclic deposition process, and / or as a post-deposition process. In other words, the process of filling the gap can include alternating cycles of flowable intermediate material formation and micropulse plasma. Additionally or alternatively, after all flowable intermediate materials are formed, the substrate can be subjected to a micropulse plasma post-deposition process.
[0090] In some embodiments, the substrate is subjected to a micropulse plasma while providing plasma gas to the reaction chamber at a flow rate above a predetermined threshold. The combination of micropulse plasma and these high flow rates minimizes the redeposition of volatile byproducts released during the plasma-induced crosslinking process of the formed flowable intermediate material. In some embodiments, the flow rate of the plasma gas during the micropulse plasma treatment is at least 5.0 slm (standard liters per minute), preferably at least 10.0 slm. Those skilled in the art understand that the flow rate depends on the reaction chamber volume and substrate size, and the values provided here for 300 mm wafers and 1 liter reaction chamber volume can be easily converted to other substrate sizes and / or reactor volumes. In some embodiments, during the micropulse plasma treatment, a rare gas is used as the plasma gas. In some embodiments, the rare gas is selected from He and Ar.
[0091] In some embodiments, the curing step includes using ultraviolet (UV) light. In other words, the curing step may include exposing the substrate containing the flowable intermediate material to UV radiation. This curing step using UV light may be referred to as UV curing.
[0092] In some embodiments, UV curing is used as a post-deposition treatment. In other words, in some embodiments, the method may include forming a flowable intermediate material and subjecting the flowable intermediate material to UV curing.
[0093] In some embodiments, the method includes a cyclic process comprising multiple cycles, each cycle including a flowable intermediate material forming step and a UV curing step. The UV curing step can be separated by a purge step. Additionally or alternatively, subsequent cycles can be separated by a purge step. Suitable purge steps are described elsewhere herein.
[0094] In an exemplary embodiment, an exemplary curing step is discussed. The curing step can use a continuous direct plasma lasting between 10 seconds and 10 minutes. The flowable intermediate material forming step and the direct plasma curing step can be performed in a cycle, that is, the flowable intermediate material forming step and the curing step can be performed alternately. This allows all or at least most of the flowable intermediate material to be effectively cured. In order to cure the flowable intermediate material in the gap on a 300mm substrate, each direct plasma curing step can have, for example, 10 seconds to 10 minutes of Ar / O2 plasma (with 20 wt% O2 in the gas mixture), an RF power of 200 to 600W, and an operating pressure of 400 to 800Pa. The reactor volume is about 1 liter and the Ar / O2 flow rate is 2slm.
[0095] According to one embodiment, the method further comprises an annealing step, wherein the solid material is exposed to a temperature heated to between 200°C and 700°C. In some embodiments, the annealing step comprises heating the solid material to a temperature between 500°C and 700°C. In some embodiments, the annealing step further comprises exposing the solid material to moisture. In some embodiments, the moisture is water vapor. In some embodiments, the annealing step lasts 20 to 60 minutes. In some embodiments, the annealing step is performed in a N2 atmosphere.
[0096] According to an embodiment, forming the first layer further comprises a second plasma pulse, which comprises exposing the substrate to a plasma treatment, wherein the plasma treatment comprises generating a plasma. In some embodiments, the plasma is generated using a plasma gas, the plasma gas comprising a gas selected from the group consisting of NH3, H2, a mixture of H2 and N2, a mixture of H2 and He, a mixture of H2 and argon, and N2H2. The second plasma pulse reduces phosphorus impurities in the deposited layer. In some embodiments, the phosphorus impurities are less than 3%, and in some embodiments, the phosphorus impurities are less than 2%.
[0097] According to an embodiment, a liner layer is deposited into the gap before forming the first layer on the substrate. In some embodiments, the liner includes silicon oxynitride, which also includes a small amount of impurity phosphorus, such as less than 2.5% phosphorus. In some embodiments, the liner includes silicon nitride, which also includes a small amount of impurity phosphorus, such as less than 2.5% phosphorus. In some embodiments, the silicon nitride or silicon oxynitride layer does not contain any phosphorus. According to an embodiment, the method for filling the gap does not include a plasma step. In other words, the step of forming the first layer on the substrate is performed by a thermal deposition process without the need for plasma.
[0098] A semiconductor processing apparatus is further described herein. The apparatus includes a reaction chamber, an RF power supply, a gas injection system, a precursor gas source, a plasma gas source, an exhaust device, and a controller. The reaction chamber includes a substrate support and an upper electrode. The substrate support includes a lower electrode. The RF power supply is arranged to generate an RF power waveform. The gas injection system is connected to the reaction chamber fluid. The precursor gas source is arranged to introduce a silicon precursor into the reaction chamber. Optionally, the silicon precursor is introduced into the reaction chamber by a carrier gas. The plasma gas source is arranged to introduce a reactant into the reaction chamber. The exhaust device is appropriately arranged to remove reaction products and unused reactants from the reaction chamber. The controller is programmed or otherwise configured to implement the method described elsewhere herein. As will be appreciated by those skilled in the art, the controller communicates with various power supplies, heating systems, pumps, robots, and gas flow controllers or valves of the system.
[0099] In some embodiments, the precursor source includes a precursor receiver, such as a precursor tank, a precursor bottle, etc.; and one or more gas lines can operably connect the precursor receiver to the reaction chamber. In such embodiments, the precursor receiver can be suitably maintained at a temperature of at least 5°C to at most 50°C lower than the reaction chamber temperature, or at least 5°C to at most 10°C lower than the reaction chamber temperature, or at least 10°C to at most 20°C lower than the reaction chamber temperature, or at least 30°C to at most 40°C lower than the reaction chamber temperature, or at least 40°C to at most 50°C lower than the reaction chamber temperature. The gas line can be suitably maintained at a temperature between the temperature of the precursor receiver and the reaction chamber. For example, the gas line can be maintained at a temperature of at least 5°C to at most 50°C, or at least 5°C to at most 10°C, or at least 10°C to at most 20°C, or at least 30°C to at most 40°C, or at least 40°C to at most 50°C lower than the reaction chamber temperature. In some embodiments, the gas line and the reaction chamber are maintained at substantially the same temperature, which is higher than the temperature of the precursor receptor.
[0100] In some embodiments, the gas injection system includes a precursor delivery system that uses a carrier gas to transport the precursor to one or more reaction chambers. In some embodiments, a flow-through system is used to achieve continuous flow of the carrier gas. In the flow-through system, the carrier gas line is provided with a bypass line having a precursor reservoir (bottle), and the main line and the bypass line are switched, wherein when only the carrier gas is intended to be supplied to the reaction chamber, the bypass line is closed, and when both the carrier gas and the precursor gas are intended to be supplied to the reaction chamber, the main line is closed, the carrier gas flows through the bypass line and flows out of the bottle together with the precursor gas. In this way, the carrier gas can flow continuously into the reaction chamber, and the precursor gas can be transported in pulses by switching the main line and the bypass line.
[0101] Figure 1A schematic diagram of an embodiment of a method for filling a gap as described herein is shown. Method 100 includes a step 102 of providing a substrate into a reaction chamber. The substrate includes at least one gap. Then, the method includes a step 104 of forming a first layer on the substrate. The first layer includes silicon and nitrogen. In some embodiments, the first layer includes silicon nitride. The silicon nitride can be deposited by a cyclic deposition process, such as plasma enhanced atomic layer deposition. Other deposition methods, such as atomic layer deposition, chemical vapor deposition, or plasma enhanced chemical vapor deposition can be used. In the cyclic deposition process, a silicon precursor is provided to the reaction chamber in a silicon precursor pulse. Then, a plasma pulse is provided. The plasma pulse exposes the substrate to a plasma treatment including generating a plasma. The plasma is generated using a plasma gas. In an embodiment where the deposited first layer includes silicon nitride, the plasma gas includes nitrogen and optionally one or more rare gases. The plasma can be a direct plasma, a remote plasma, or an indirect plasma. In one embodiment, subsequent deposition cycles are separated by a purge. In another embodiment, the precursor pulse and the plasma pulse overlap at least partially.
[0102] Next, the method includes a step 106 of subjecting the first layer to a phosphorus-containing compound to form a flowable intermediate material. In an exemplary embodiment, the phosphorus-containing compound includes phosphoric acid. The phosphoric acid reacts with the formed first layer comprising silicon and nitrogen. The first layer is etched and modified to form a flowable intermediate material, which includes silicon, hydrogen and oxygen. In one embodiment, the flowable intermediate material includes silicic acid. The flowable intermediate material then flows into the gap of the substrate and at least partially fills the gap. The steps 104, 106 of forming the first layer on the substrate and subjecting the first layer to the phosphorus-containing compound can be repeated 110 times in sequence as needed. The number of cycles can be at least 10 cycles, or at least 50 cycles, or at least 100 cycles, or at least 200 cycles, or at least 400 cycles.
[0103] Finally, the method includes a step of forming a solid material 108. Once the flowable intermediate material at least partially fills the gap on the substrate, the material condenses and forms a solid material comprising silicon. In an exemplary embodiment, the solid material comprises silicon dioxide.
[0104] Figure 2Another schematic diagram of an embodiment of a method for filling a gap is shown. Method 200 includes a step 202 of providing a substrate into a reaction chamber. The substrate includes at least one gap. Then, the method includes a step 204 of forming a first layer on the substrate. The first layer includes silicon and nitrogen. In some embodiments, the first layer includes silicon nitride. The silicon nitride can be deposited by a cyclic deposition process, such as plasma enhanced atomic layer deposition. Other deposition methods, such as atomic layer deposition, chemical vapor deposition, or plasma enhanced chemical vapor deposition can be used. In the cyclic deposition process, a silicon precursor is provided to the reaction chamber in a silicon precursor pulse. Then, a plasma pulse is provided. The plasma pulse exposes the substrate to a plasma treatment including generating a plasma. The plasma is generated using a plasma gas. In an embodiment where the deposited first layer includes silicon nitride, the plasma gas includes nitrogen and optionally one or more rare gases. The plasma can be a direct plasma, a remote plasma, or an indirect plasma. In one embodiment, subsequent deposition cycles are separated by a purge. In another embodiment, the precursor pulse and the plasma pulse overlap at least partially.
[0105] Next, the method includes subjecting the first layer to a phosphorus-containing compound and moisture to form a flowable intermediate material 206. In an exemplary embodiment, the phosphorus-containing compound includes trimethyl phosphate. The moisture may be H + HO - any source of, for example, water, steam or hydrogen peroxide. The phosphorus-containing compound and moisture can be provided to the reaction chamber as pulses simultaneously or sequentially. The phosphorus-containing compound and moisture pulses can also partially overlap. The phosphorus-containing compound reacts with the moisture and further reacts with the surface of the first layer. The cycle comprising subjecting the first layer to the phosphorus-containing compound and moisture can be performed multiple times as needed. The number of cycles can be at least 10 cycles, or at least 50 cycles, or at least 100 cycles, or at least 200 cycles, or at least 400 cycles. In an exemplary embodiment, the phosphorus-containing compound and moisture form phosphoric acid. The phosphoric acid reacts with the formed first layer comprising silicon and nitrogen. The first layer is etched and modified to form a flowable intermediate material comprising silicon, hydrogen and oxygen. In one embodiment, the flowable intermediate material comprises silicic acid. Then, the flowable intermediate material flows into the gap of the substrate and at least partially fills the gap. Steps 204, 206 of forming the first layer on the substrate and subjecting the first layer to the phosphorus-containing compound and moisture can be repeated 210 times in sequence as needed. The number of cycles can be at least 10 cycles, or at least 50 cycles, or at least 100 cycles, or at least 200 cycles, or at least 400 cycles.
[0106] Finally, the method includes a step of forming a solid material 208. Once the flowable intermediate material at least partially fills the gap on the substrate, the material condenses and forms a solid material comprising silicon. In an exemplary embodiment, the solid material comprises silicon dioxide.
[0107] Figure 3 Another schematic diagram of an embodiment of a method for filling a gap is shown. Method 300 includes step 302 of providing a substrate into a reaction chamber. The substrate includes at least one gap. Then, the method includes step 304 of forming a first layer on the substrate. The first layer includes silicon, oxygen, nitrogen and phosphorus. In some embodiments, the first layer includes SiON:P. SiON:P can be deposited by a cyclic deposition process, such as plasma enhanced atomic layer deposition. Other deposition methods, such as atomic layer deposition, chemical vapor deposition or plasma enhanced chemical vapor deposition can be used. In the cyclic deposition process, a silicon precursor including silicon, oxygen and phosphorus is provided to the reaction chamber as a silicon precursor pulse. In an exemplary embodiment, the silicon precursor includes trimethylsilyl phosphite. Then, a plasma pulse is provided. The plasma pulse exposes the substrate to a plasma treatment including generating a plasma. The plasma is generated using a plasma gas. In an embodiment where the deposited first layer includes SiON:P, the plasma gas includes nitrogen and optionally one or more rare gases. The plasma can be a direct plasma, a remote plasma or an indirect plasma. In one embodiment, subsequent deposition cycles are separated by a purge. In another embodiment, the precursor pulse and the plasma pulse overlap at least partially.
[0108] Next, the method includes step 306 of subjecting the first layer to moisture to form a flowable intermediate material. The moisture may be H + HO - any source of, such as water, steam, or hydrogen peroxide. The moisture reacts with the surface of the first layer. In an exemplary embodiment, phosphorus in the first layer and the moisture form phosphoric acid. The phosphoric acid reacts with silicon and nitrogen in the first layer. The first layer is then etched and modified to form a flowable intermediate material comprising silicon, hydrogen, and oxygen. In an embodiment, the flowable intermediate material comprises silicic acid. The flowable intermediate material then flows into the gaps in the substrate and at least partially fills the gaps. Steps 304, 306 of forming the first layer on the substrate and subjecting the first layer to moisture can be repeated 310 times in sequence as needed. The number of cycles can be at least 10 cycles, or at least 50 cycles, or at least 100 cycles, or at least 200 cycles, or at least 400 cycles.
[0109] Finally, the method includes a step of forming a solid material 308. Once the flowable intermediate material at least partially fills the gap on the substrate, the material condenses and forms a solid material comprising silicon. In an exemplary embodiment, the solid material comprises silicon dioxide.
[0110] Figure 4A deposition assembly 400 according to the present disclosure is shown in schematic form. The deposition assembly 400 can be used to perform the methods described herein and / or form the structures or devices described herein or portions thereof.
[0111] In the illustrated example, the deposition assembly 400 includes one or more reaction chambers 402, a precursor injector system 401, a silicon precursor container 404, a plasma gas container 406, an exhaust source 410, and a controller 412. The deposition assembly 400 may include one or more additional gas sources (not shown), such as an inert gas source, a carrier gas source, and / or a purge gas source.
[0112] Reaction chamber 402 may include any suitable reaction chamber, such as an ALD or CVD reaction chamber as described herein.
[0113] The silicon precursor container 404 may include a container and one or more silicon precursors described herein—alone or mixed with one or more carrier gases (e.g., inert gases). The plasma gas container 406 may include a container and a plasma gas described herein—alone or mixed with one or more carrier gases. Although two source containers 404, 406 are shown, the deposition assembly 400 may include any suitable number of source containers. The source containers 404, 406 may be coupled to the reaction chamber 402 via lines 414, 416, which may each include a flow controller, a valve, a heater, etc. In some embodiments, the silicon precursor in the silicon precursor container 404 and the plasma gas in the plasma gas container 406 may be heated. In some embodiments, the containers are heated so that the precursors or reactants reach a temperature of, for example, between about 30°C and about 200°C, depending on the nature of the chemical in question.
[0114] Exhaust source 410 may include one or more vacuum pumps.
[0115] Controller 412 includes electronic circuits and software to selectively operate valves, manifolds, heaters, pumps and other components included in deposition assembly 400. Such circuits and components are used to introduce precursors, reactants and purge gases from corresponding sources. Controller 412 can control the timing of gas pulse sequences, the temperature of substrate and / or reaction chamber 402, the pressure in reaction chamber 402, and various other operations to provide proper operation of deposition assembly 400. Controller 412 can include control software to control the flow of precursors, reactants and purge gases into and out of reaction chamber 402 electrically or pneumatically. Controller 412 may include modules, such as software or hardware components, that perform certain tasks. Modules may be configured to reside on an addressable storage medium of a control system and configured to perform one or more processes.
[0116] Other configurations of the deposition assembly 400 are possible, including different numbers and types of precursor and reactant sources. In addition, it should be understood that there are many arrangements of valves, conduits, precursor sources, and auxiliary reactant sources that can be used to achieve the goal of selectively and in a coordinated manner to supply gases into the reaction chamber 402. In addition, as a schematic representation of the deposition assembly, many components are omitted for simplicity of illustration, and these components may include, for example, various valves, manifolds, purifiers, heaters, containers, vents, and / or bypasses.
[0117] During operation of deposition assembly 400, a substrate such as a semiconductor wafer (not shown) is transferred from, for example, a substrate handling system to reaction chamber 402. Once the substrate is transferred to reaction chamber 402, one or more gases (e.g., precursors, reactants, carrier gases, and / or purge gases) from a gas source are introduced into reaction chamber 402.
[0118] In some embodiments, the silicon precursor is supplied in pulses, the plasma gas is supplied in pulses, and the reaction chamber is purged between successive pulses of the silicon precursor and the plasma gas.
[0119] The illustrations presented herein are not intended to be actual views of any particular material, structure, or device but are merely idealized representations used to describe embodiments of the present disclosure.
[0120] The specific embodiments shown and described are illustrations of the present invention and its best mode and are not intended to limit the scope of these aspects and embodiments in any way. In fact, for the sake of brevity, the traditional manufacturing, connection, preparation and other functional aspects of the system may not be described in detail. In addition, the connecting lines shown in the various figures are intended to represent exemplary functional relationships and / or physical connections between various elements. Many alternative or additional functional relationships or physical connections may exist in actual systems, and / or may not exist in some embodiments.
[0121] It should be understood that the configurations and / or methods described herein are exemplary in nature, and these specific embodiments or examples should not be considered restrictive, as many variations are possible. The specific routines or methods described herein may represent one or more of any number of processing strategies. Therefore, the various actions shown may be performed in the order shown, in other orders, or may be omitted in some cases.
[0122] The subject matter of the present disclosure includes all novel and nonobvious combinations and subcombinations of the various processes, systems and configurations, and other features, functions, acts and / or properties disclosed herein, and any and all equivalents thereof.
Claims
1. A method for filling a gap in a substrate, the method comprising: - providing a substrate into a reaction chamber, wherein the substrate comprises at least one gap; - forming a first layer on the substrate, wherein the first layer comprises silicon and nitrogen; - subjecting the first layer to a phosphorus-containing compound to form a flowable intermediate material at least partially filling at least one gap on the substrate, wherein the intermediate material comprises silicon, oxygen and hydrogen; as well as - forming a solid material comprising silicon.
2. The method according to claim 1, wherein: The step of subjecting the first layer to a phosphorus-containing compound further comprises subjecting the first layer to moisture.
3. The method according to claim 2, wherein: The moisture is selected from H2O, steam or H2O2.
4. A method according to any one of the preceding claims, wherein: The solid material comprises silicon dioxide.
5. A method according to any one of the preceding claims, wherein: The phosphorus-containing compound comprises an amount of phosphorus such that the first layer comprises at least 4 atomic % phosphorus after being subjected to the phosphorus-containing compound.
6. A method according to any one of the preceding claims, wherein: The step of forming the first layer includes performing a plurality of deposition cycles to form the silicon-containing layer, the deposition cycles comprising: - a silicon precursor pulse, which comprises exposing the substrate to a silicon precursor; and - A plasma pulse comprising exposing the substrate to a plasma treatment, wherein the plasma treatment comprises generating a plasma.
7. The method according to claim 6, wherein: The plasma is a direct plasma.
8. The method according to claim 6, wherein: The plasma is a remote plasma.
9. The method according to claim 6, wherein: The plasma is an indirect plasma.
10. The method according to any one of claims 6 to 9, wherein: The plasma is generated using a plasma gas comprising N2 and optionally one or more noble gases.
11. The method according to claim 10, wherein: The rare gas includes one or more of He and Ar.
12. The method according to any one of claims 6 to 11, wherein: The silicon precursor comprises silicon and optionally phosphorus.
13. The method according to any one of claims 6 to 12, wherein: Subsequent deposition cycles are separated by purges.
14. The method according to any one of claims 6 to 13, wherein: The precursor pulse and the plasma pulse at least partially overlap.
15. A method according to any one of the preceding claims, wherein: The method includes one or more super cycles including the steps of forming a first layer on a substrate, subjecting the first layer to a phosphorus-containing compound, and forming a solid material comprising silicon.
16. The method according to any one of the preceding claims, further comprising an annealing step, wherein: The solid material is exposed to heating to a temperature between 500°C and 700°C.
17. The method according to claims 6 to 16, wherein: Forming the first layer further includes a second plasma pulse including exposing the substrate to a plasma treatment, wherein the plasma treatment includes generating a plasma.
18. The method according to claim 17, wherein: The plasma is generated using a plasma gas including a gas selected from the group consisting of NH3, H2, a mixture of H2 and N2, a mixture of H2 and He, a mixture of H2 and argon, and N2H2.
19. A method according to any one of the preceding claims, wherein: A liner layer is deposited in the gap before forming the first layer on the substrate.
20. A semiconductor processing device comprising: - a reaction chamber comprising a substrate support for supporting a substrate; - a heater constructed and arranged to heat a substrate in the reaction chamber; - a plasma module comprising a radio frequency power source constructed and arranged to generate a plasma; - a plasma gas source in fluid communication with the plasma module; - a silicon precursor source fluidly connected to the reaction chamber via one or more precursor valves; as well as - A controller configured to cause a semiconductor processing device to perform a method according to any one of claims 1 to 15.