Silicon carbide single crystal and method for producing same

By periodically increasing and decreasing the resistivity during the growth process of SiC single crystal, the problem of heterogeneous crystal generation is solved, the yield is improved, the cost is reduced, and etching losses are avoided.

CN118773740APending Publication Date: 2024-10-15DENSO CORP +2
View PDF 0 Cites 0 Cited by

Patent Information

Application Number
CN202410384431.6
Authority / Receiving Office
CN · China
Patent Type
Applications(China)
Current Assignee / Owner
Priority Date
2023-04-07
Filing Date
2024-04-01
Publication Date
2024-10-15

AI Technical Summary

Technical Problem

In the existing SiC single crystal growth technology, high-speed growth leads to the generation of heterogeneously oriented crystals, which leads to a decrease in product yield and an increase in costs. Moreover, existing methods that suppress heterogeneously oriented crystals through etching will reduce the growth rate.

Method used

By repeatedly slowly increasing and decreasing the resistivity during the growth process of the SiC single crystal, a SiC single crystal is formed that causes the resistivity to increase and decrease periodically, thereby suppressing the generation and expansion of differently oriented crystals and avoiding etching losses.

Benefits of technology

It is possible to suppress the generation of differently oriented crystals without reducing the growth rate, improve product yield, and reduce manufacturing costs.

✦ Generated by Eureka AI based on patent content.

Smart Images

  • Figure CN118773740A_ABST
    Figure CN118773740A_ABST
Patent Text Reader

Abstract

The resistivity is periodically, slowly and repeatedly increased and decreased during the growth of the SiC single crystal (3). By producing the SiC single crystal (3) by this way, even if a heterogeneously oriented crystal (30) occurs during the growth of the SiC single crystal (3), expansion of the heterogeneously oriented crystal (30) can be suppressed, and the heterogeneously oriented crystal (30) can disappear during the growth of the SiC single crystal (3). In addition, etching for removing the heterogeneously oriented crystal (30) is not required.
Need to check novelty before this filing date? Find Prior Art

Description

Technical Field

[0001] The present disclosure relates to a silicon carbide (hereinafter referred to as SiC) single crystal and a method for manufacturing the same. Background Art

[0002] Conventionally, there is known a gas growth method for growing a SiC single crystal on a seed crystal by supplying a SiC raw material gas to the growth surface of a seed crystal composed of a SiC single crystal. In the gas growth method, a SiC single crystal is manufactured by introducing a SiC raw material gas, and introducing H2 (hydrogen) gas as a carrier gas and N2 (nitrogen) gas as a dopant for adjusting the resistivity of the crystal.

[0003] In order to reduce the cost of SiC single crystal production, it is effective to increase the growth rate of SiC single crystal. However, if the growth rate is too high, multiple crystal grains called differentially oriented crystals will occur in the SiC single crystal, and the differentially oriented crystals may expand as they grow.

[0004] After a SiC single crystal ingot is obtained by growing a SiC single crystal, it is sliced ​​and processed into wafers, and then the wafers are subjected to semiconductor processing to produce devices, but devices in the region where the hetero-oriented crystals exist become scrap. Therefore, even if high-speed growth is performed with the goal of reducing costs, the product yield deteriorates, which in turn leads to increased costs.

[0005] In contrast, Patent Document 1 proposes a technique for removing hetero-orientation, which includes monitoring the growing SiC single crystal, injecting etching gas into the furnace when hetero-orientation occurs, and etching the entire SiC single crystal until the hetero-orientation disappears. This can suppress the generation of hetero-orientation crystals, thereby suppressing the deterioration of the product yield.

[0006] Prior art literature

[0007] Patent Literature

[0008] Patent Document 1: Japanese Patent Application Publication No. 2004-43211 Summary of the invention

[0009] However, in the technology of Patent Document 1, since etching is performed during the growth of the SiC single crystal, a loss of the SiC single crystal occurs in the growth of the SiC single crystal to the extent of etching, which reduces the actual growth rate and increases the manufacturing cost.

[0010] An object of the present disclosure is to provide a method for producing a SiC single crystal capable of suppressing a decrease in growth rate while suppressing the formation of hetero-oriented crystals, and a SiC single crystal in which hetero-oriented crystals are suppressed.

[0011] A first aspect of the present disclosure relates to a SiC single crystal in which, in at least a part of a region within the crystal, resistivity changes such as a gradual increase and decrease in resistivity are repeated in a growth direction.

[0012] In this way, a SiC single crystal is formed in which the resistivity increases and decreases slowly and repeatedly. Even if a hetero-oriented crystal occurs in such a SiC single crystal, it cannot be inherited during growth and its expansion is suppressed. Therefore, the SiC single crystal can be made into a SiC single crystal in which hetero-oriented crystals are suppressed.

[0013] The second aspect of the present disclosure relates to a method for manufacturing a SiC single crystal, which includes the following steps: a step of disposing a susceptor in a crucible having a hollow portion constituting a reaction chamber, and a step of disposing a seed crystal for growing a silicon carbide single crystal on a surface of the susceptor; and a step of supplying a raw material gas and a carrier gas of silicon carbide and an impurity gas containing a dopant for growing the silicon carbide single crystal from below the susceptor toward the surface of the seed crystal, and supplying the raw material gas to the seed crystal after heating and decomposing the raw material gas, thereby growing the silicon carbide single crystal on the surface of the seed crystal, wherein in the step of growing the silicon carbide single crystal, an operation of slowly increasing and slowly decreasing the resistivity relative to the growth distance of the silicon carbide single crystal is repeated to grow the silicon carbide single crystal.

[0014] In this way, by simply repeating the operation of slowly increasing and decreasing the resistivity during the growth of the SiC single crystal, the hetero-oriented crystals can be eliminated even without etching, and the decrease in the substantial growth rate of the SiC single crystal can be suppressed. Therefore, a method for manufacturing a SiC single crystal that can suppress the growth rate while suppressing the hetero-oriented crystals can be formed. BRIEF DESCRIPTION OF THE DRAWINGS

[0015] Figure 1 It is a cross-sectional view of the SiC single crystal production apparatus according to the first embodiment.

[0016] Figure 2 This is a graph showing the change in the flow rate of N2 serving as a doping gas relative to the growth time.

[0017] Figure 3 Yes Figure 2 This is a binarized image of a microscope image when the resistivity is repeatedly increased and decreased by varying the flow rate of the doping gas as shown.

[0018] Figure 4 This is a diagram showing a case where the resistivity is changed in a pulse shape with respect to the growth distance as a comparative example.

[0019] Figure 5 This is a diagram showing changes in the growth rate with respect to the growth time described in other embodiments.

[0020] Figure 6 This is a diagram showing a case where the resistivity is repeatedly and gradually increased and decreased with respect to the growth distance described in other embodiments. DETAILED DESCRIPTION

[0021] Hereinafter, embodiments of the present invention will be described based on the drawings.

[0022] In the following embodiments, the same or equivalent parts are denoted by the same reference numerals for description.

[0023] (First embodiment)

[0024] Figure 1 The SiC single crystal production apparatus 1 shown is an apparatus for producing a SiC single crystal ingot by long-length growth. According to the SiC single crystal production apparatus 1, a method for producing a SiC single crystal capable of increasing the growth rate while suppressing hetero-oriented crystals can be provided.

[0025] SiC single crystal manufacturing apparatus 1 Figure 1 The SiC single crystal manufacturing device 1 is arranged in a manner that the upper and lower directions of the paper face the sky-to-earth direction, and the SiC raw material gas is supplied to the surface of the seed crystal 2 formed by the SiC single crystal substrate, so that the SiC single crystal 3 grows on the surface of the seed crystal 2. Specifically, the SiC single crystal manufacturing device 1 includes: a gas supply unit 4, a gas introduction source 5, a gas exhaust port 6, a vacuum container 7, an insulating material 8, a heating container 9, a susceptor 10, a rotating crystal pulling mechanism 11, and first and second heating devices 12 and 13.

[0026] A gas supply unit 4 is provided below the SiC single crystal manufacturing apparatus 1 , and a raw material gas 20 including various gases that become SiC raw materials, a carrier gas 21 , and a doping gas 22 are introduced from a gas introduction source 5 into the SiC single crystal manufacturing apparatus 1 .

[0027] The gas supply unit 4 includes: a raw material gas supply unit 4a for supplying a raw material gas 20, a carrier gas supply unit 4b for supplying a carrier gas 21, and a doping gas supply unit 4c for supplying a doping gas 22. Although each of these gas supply units 4a to 4c is omitted in the figure, they are all composed of components that constitute a supply path. The raw material gas supply unit 4a introduces the raw material gas 20 from the raw material gas source 5a described later into the SiC single crystal manufacturing device 1. The carrier gas supply unit 4b introduces the carrier gas 21 from the carrier gas source 5b described later into the SiC single crystal manufacturing device 1. The doping gas supply unit 4c introduces the doping gas 22 from the doping gas source 5c described later into the SiC single crystal manufacturing device 1.

[0028] The gas introduction source 5 is a member for supplying a gas including a SiC raw material gas into the SiC single crystal manufacturing apparatus 1. In the present embodiment, the gas introduction source 5 is composed of a raw material gas source 5a, a carrier gas source 5b, and a doping gas source 5c.

[0029] The raw material gas source 5a supplies SiC raw material gas containing Si and C, for example, a raw material gas 20 containing a mixed gas of a silane-based gas such as silane and a hydrocarbon-based gas such as propane. The carrier gas source 5b supplies a carrier gas 21 such as H2. The doping gas source 5c supplies a doping gas 22 such as N2. Although not shown in the figure, each of these gas sources 5a to 5c is equipped with a heating device for controlling the temperature of each supplied gas and a flow control device for controlling the flow rate, etc., and the temperature and flow rate of each supplied gas can be controlled according to the growth status of the SiC single crystal 3.

[0030] The gas exhaust port 6 exhausts unreacted gas, carrier gas 21 , doping gas 22 , and the like in the raw material gas 20 supplied to the seed crystal 2 to the outside of the SiC single crystal manufacturing apparatus 1 as exhaust gas.

[0031] The vacuum container 7 is made of quartz glass or the like, and is formed into a cylindrical shape having a hollow portion. In the case of the present embodiment, it is formed into a cylindrical shape, and becomes a structure that can introduce and export the raw material gas 20, the carrier gas 21, and the doping gas 22. In addition, the vacuum container 7 is a structure that can reduce the pressure of the internal space contained therein by evacuating the vacuum container 7 while accommodating other components of the SiC single crystal manufacturing device 1. As described above, the bottom of the vacuum container 7 is provided with a raw material gas supply part 4a for supplying the raw material gas 20, a carrier gas supply part 4b for supplying the carrier gas 21, and a doping gas supply part 4c for supplying the doping gas 22. In addition, a through hole 7a is formed in the upper part of the vacuum container 7, specifically, in the upper position of the side wall, and a gas exhaust port 6 for exhausting waste gas such as unreacted gas in the raw material gas 20 is embedded in the through hole 7a.

[0032] The heat insulating material 8 is formed into a cylindrical shape having a hollow portion, and in the case of the present embodiment, is formed into a cylindrical shape, and is arranged coaxially with respect to the vacuum container 7. The heat insulating material 8 is formed into a cylindrical shape with a diameter reduced compared to the vacuum container 7, and is arranged inside the vacuum container 7, thereby controlling the heat transfer from the space inside the heat insulating material 8 to the vacuum container 7 side. The heat insulating material 8 is composed of graphite, for example, but it can also be formed into a structure that is difficult to be thermally etched by coating the surface with a high melting point metal carbide such as TaC (tantalum carbide) or NbC (niobium carbide). Furthermore, a through hole 8a is also formed in the upper part of the heat insulating material 8, specifically, at the upper position of the side wall, and the gas exhaust port 6 is embedded in the through hole 8a.

[0033] The heating container 9 is a component constituting a crucible that becomes a reaction container, and is formed in a tubular shape with a hollow portion, and in the case of the present embodiment, is formed in a cylindrical shape. The hollow portion of the heating container 9 forms a reaction chamber for growing the SiC single crystal 3 on the surface of the seed crystal 2. The heating container 9 is made of graphite, for example, but the surface can also be coated with a high melting point metal carbide such as TaC or NbC to form a structure that is difficult to be thermally etched. The heating container 9 is configured in a manner that surrounds the susceptor 10. Moreover, waste gas such as unreacted gas in the raw material gas 20 is introduced to the gas outlet 6 side through the inner circumferential surface of the heating container 9 and the outer circumferential surface of the seed crystal 2 and the susceptor 10. Through the heating container 9, the SiC raw material gas in the raw material gas 20 is decomposed before the raw material gas 20 from the raw material gas supply part 4a is introduced into the seed crystal 2. Furthermore, a through hole 9a is also formed in the upper part of the heating container 9, specifically at the upper position of the side wall, and the gas outlet 6 is embedded in the through hole 9a.

[0034] The susceptor 10 is a component for setting the seed crystal 2. The susceptor 10 is formed into a circular shape on one side of which the disc-shaped seed crystal 2 is set, for example, and the central axis of the susceptor 10 is coaxially arranged relative to the central axis of the heating container 9 or the central axis of the shaft 11a of the rotating crystal pulling mechanism 11 described later. The susceptor 10 is made of graphite, for example, but the surface can also be coated with a high melting point metal carbide such as TaC or NbC to form a structure that is difficult to be thermally etched. The seed crystal 2 is attached to one surface on the side of the raw material gas supply part 4a in the susceptor 10, and the SiC single crystal 3 is grown on the surface of the seed crystal 2. In addition, the susceptor 10 is connected to the shaft 11a on the surface opposite to the side on which the seed crystal 2 is set, and rotates with the rotation of the shaft 11a, and can be lifted above the paper surface along with the lifting shaft 11a.

[0035] The rotating crystal pulling mechanism 11 rotates and lifts the susceptor 10 via a shaft 11a made of a pipe or the like. In the present embodiment, the shaft 11a is in a straight line extending up and down, one end of which is connected to the surface on the opposite side of the attachment surface of the seed crystal 2 in the susceptor 10, and the other end is connected to the main body of the rotating crystal pulling mechanism 11. The shaft 11a is also made of graphite, for example, but the surface can also be coated with a high melting point metal carbide such as TaC or NbC to form a structure that is difficult to be thermally etched. With such a structure, the susceptor 10, the seed crystal 2 and the SiC single crystal 3 can be rotated and lifted, and the growth surface of the SiC single crystal 3 can be made into a desired temperature distribution while the temperature of the growth surface of the SiC single crystal 3 is adjusted to a temperature suitable for growth as the SiC single crystal 3 grows.

[0036] The first and second heating devices 12 and 13 are composed of heating coils such as induction heating coils or direct heating coils, and are arranged to surround the vacuum container 7. In the case of this embodiment, the first and second heating devices 12 and 13 are composed of induction heating coils. These first and second heating devices 12 and 13 are configured in a manner that can independently control the temperature of the target parts. The first heating device 12 is configured at a position corresponding to the lower position of the heating container 9, and the second heating device 13 is configured at a position corresponding to the susceptor 10. Therefore, the temperature of the lower part of the heating container 9 can be controlled by the first heating device 12 to heat and decompose the SiC raw material gas. In addition, the temperature around the susceptor 10, the seed crystal 2 and the SiC single crystal 3 can be controlled to a temperature suitable for the growth of the SiC single crystal 3 by the second heating device 13.

[0037] The SiC single crystal production apparatus 1 is configured in this manner. Next, a method for producing the SiC single crystal 3 using the SiC single crystal production apparatus 1 according to the present embodiment will be described.

[0038] First, the seed crystal 2 is attached to one surface of the susceptor 10. The surface of the seed crystal 2 opposite to the susceptor 10, i.e., the growth surface of the SiC single crystal 3, becomes an offset substrate having a predetermined offset angle of, for example, 4° or 8° relative to the (0001)C plane. Next, the susceptor 10 and the seed crystal 2 are arranged in the heating container 9. Then, the first and second heating devices 12 and 13 are controlled to set the desired temperature distribution. That is, the following temperature distribution is formed: while the SiC raw material gas contained in the raw material gas 20 is heated and decomposed, supplied to the surface of the seed crystal 2, and the SiC raw material gas is recrystallized on the surface of the seed crystal 2, the sublimation rate in the heating container 9 is increased compared to the recrystallization rate. In this way, the temperature of the bottom of the heating container 9 can reach a high temperature of more than 2000°C, for example, 2400°C, and at the same time, the temperature of the surface of the seed crystal 2 can reach a temperature lower than the temperature of the bottom of the heating container 9 and suitable for the recrystallization of the SiC single crystal 3, for example, about 2200°C.

[0039] Furthermore, while the vacuum container 7 is brought to a desired pressure, a raw material gas 20 including SiC raw material gas is introduced through the raw material gas supply unit 4a. Figure 1 As shown by the arrow in FIG. 2 , the raw material gas 20 is supplied to the seed crystal 2, and based on the gas supply, the SiC single crystal 3 is grown on the surface of the seed crystal 2. In addition, the carrier gas 21 is introduced through the carrier gas supply part 4b, and the doping gas 22 is introduced through the doping gas supply part 4c. Thus, the carrier gas 21 and the doping gas 22 flow inside the heating container 9, and the N contained in the doping gas 22 is doped into the SiC single crystal 3.

[0040] Then, by rotating the crystal pulling mechanism 11, the susceptor 10, the seed crystal 2 and the SiC single crystal 3 are rotated via the axis 11a, and the growth rate of the SiC single crystal 3 is increased accordingly. Thus, the height of the growth surface of the SiC single crystal 3 is kept substantially constant, and the temperature distribution of the growth surface temperature can be well controlled.

[0041] At this time, when the SiC single crystal 3 is grown, Figure 2 By periodically and repeatedly changing the flow rate of the doping gas 22 as shown, the content of N2 in the SiC single crystal manufacturing device 1 can be changed, and the resistivity in the SiC single crystal 3 can be periodically changed. Specifically, by adjusting the flow rate by the doping gas source 5c, the doping gas 22 introduced from the doping gas supply unit 4c into the heating container 9 can be periodically increased or decreased. Here, the doping gas 22 is periodically increased or decreased in a sine wave shape.

[0042] Thus, it was confirmed through experiments that by periodically changing the resistivity in the SiC single crystal 3, the hetero-oriented crystals can be eliminated at a micro-sized stage during growth, that is, they cannot be inherited in the growing crystal. When the resistivity changes periodically, the amount of N introduced as a dopant changes slowly during the process of slowly increasing or slowly decreasing the resistivity, and the hetero-oriented crystals can be eliminated at a micro-sized stage during the change.

[0043] Figure 3 Its morphology is shown. In the SiC single crystal 3, the color changes according to the resistivity. If the resistivity is high, the color is light, and if the resistivity is low, the color is dark. As shown in the figure, along the growth direction A1 of the SiC single crystal 3, it slowly changes from light color to dark color or from dark color to light color in each change cycle C1. In addition, it is known that: in the middle of the growth of the SiC single crystal 3, the hetero-oriented crystal 30 occurs, but even if the SiC single crystal 3 grows during the color change process, the hetero-oriented crystal 30 will not be inherited and disappears from the subsequent growth crystal.

[0044] After various tests, it was found that such phenomenon occurs when the resistivity is slowly increased or decreased repeatedly, but does not occur in a process where the resistivity is not slowly increased or decreased. For example, it is known that the amount of N2 introduced as a dopant is changed in a pulsed manner, such as Figure 4As shown in the figure, the marking doping technique is used to change the resistivity in a pulsed manner during growth for inspection. However, even if the amount of N2 introduced is changed in a pulsed manner, the hetero-oriented crystal 30 cannot be eliminated. This is considered to be because: even if the resistivity is simply changed in a pulsed manner, the hetero-oriented crystal 30 will occur regardless of whether the resistivity is high or low. In addition, the hetero-oriented crystal 30 will expand even if the resistivity does not change in either case. Therefore, it is considered necessary to repeatedly increase and decrease the resistivity slowly in order to eliminate the hetero-oriented crystal 30. It is also possible to have a portion that grows by temporarily not changing the resistivity, but it is best to define the growth amount of this portion within a range that can be allowed even if the hetero-oriented crystal 30 occurs and expands in this portion.

[0045] To obtain the effect of eliminating the hetero-oriented crystal 30, it is sufficient to have a certain degree of variation in resistivity, for example, the variation, i.e., the ratio of the variation relative to the central value of the resistivity, is preferably 0.5% or more. In addition, if the variation in resistivity becomes too large, it will also become the main cause of defects such as heterogeneous polymorphism or dislocation. Therefore, the variation in resistivity is preferably 50% or less.

[0046] In addition, the relationship between the resistivity change cycle and the disappearance effect of the hetero-oriented crystal 30 was investigated, and the results confirmed that if the resistivity change cycle is too large, the size of the generated polycrystal is too large and may not be eliminated. It is known that if the resistivity change cycle converted into the length of the SiC single crystal 3 is greater than 500μm, this phenomenon will occur. Furthermore, when converting the resistivity change cycle into the length of the SiC single crystal 3, it can be expressed as cycle time × growth rate = change cycle, Figure 2 The value obtained by multiplying the time of about one cycle represented by the growth time in φ by the growth rate of the SiC single crystal 3 at that time is the change cycle.

[0047] In addition, if the resistivity variation cycle is too long, the resistivity of the wafer will deviate due to the influence of the resistivity variation cycle, because the thickness of the SiC single crystal ingot when slicing the substrate is specified to be about 300μm or 500μm. In other words, if the resistivity variation is repeated many times in the thickness of the wafer, the resistivity of each wafer will be averaged regardless of the position of the SiC single crystal ingot at which the wafer is cut. However, if the resistivity variation cycle is long, the resistivity of the wafer will deviate due to the position of the SiC single crystal ingot being cut, and the characteristics of the device finally produced will also deviate.

[0048] In addition, the length of the resistivity change period converted into the SiC single crystal 3 is preferably 500 μm or less. In addition, if the resistivity deviation when forming the wafer is taken into account, the resistivity fluctuation range can be set to 0.5% or more and 10% or less, and the resistivity change period converted into the length of the SiC single crystal 3 is preferably set to 100 μm or less.

[0049] Furthermore, the periodic variation of resistivity does not necessarily have to exist in all regions of the SiC single crystal ingot, otherwise it will have no effect. As long as it exists in any region, it can suppress the hetero-oriented crystal 30 in the region, and can expand the effective area when manufacturing devices. In particular, it is effective to apply the periodic variation of resistivity to the crystallization region or facet region produced under the high-speed growth conditions where hetero-oriented crystal 30 is likely to occur. For example, if the raw material gas 20, carrier gas 21 and doping gas 23 are concentratedly supplied to the facet region while the flow rate of the doping gas 23 is changed, the resistivity can be periodically varied in the facet region.

[0050] As described above, the SiC single crystal 3 of the present embodiment is formed by slowly and repeatedly increasing and decreasing the resistivity periodically. Even if a hetero-oriented crystal 30 occurs in such a SiC single crystal 3, it will not be inherited during growth, and its expansion is also suppressed. Therefore, it is possible to manufacture a SiC single crystal 3 in which the hetero-oriented crystal 30 is suppressed.

[0051] Furthermore, by manufacturing SiC single crystal 3 in such a manner that the resistivity is periodically and slowly repeatedly increased and decreased as in this embodiment, even if hetero-oriented crystal 30 is generated during the growth of SiC single crystal 3, its expansion can be suppressed and it can be eliminated during the growth. Furthermore, etching for removing hetero-oriented crystal 30 is not required.

[0052] When manufacturing SiC single crystal 3 without changing the resistivity or by changing the resistivity in a pulsed manner, if hetero-oriented crystal 30 occurs, the hetero-oriented crystal 30 expands as it grows. Therefore, even if a SiC single crystal ingot is obtained by growing SiC single crystal 3, it is processed into a wafer by slicing, and a device is manufactured by semiconductor process on the wafer, the device in the area where the hetero-oriented crystal 30 exists becomes a waste. Moreover, the larger the range where the hetero-oriented crystal 30 exists, the more devices become waste, and the lower the product yield. On the other hand, when hetero-oriented crystal 30 occurs, although the hetero-oriented crystal 30 can be removed by etching the SiC single crystal 3, the occurrence of hetero-oriented crystal 30 must be monitored, and losses corresponding to the degree of etching occur in the growth of the SiC single crystal, which reduces the actual growth rate and increases the manufacturing cost.

[0053] In contrast, according to the present embodiment, only by slowly and periodically increasing and decreasing the resistivity during the growth of the SiC single crystal 3, the hetero-oriented crystal 30 can be eliminated even without etching, and the substantial growth rate of the SiC single crystal 3 can be suppressed from decreasing. In addition, this can also improve the product yield and reduce the manufacturing cost.

[0054] (Other Embodiments)

[0055] The present disclosure is described in accordance with the above-mentioned embodiments, but is not limited to the embodiments, and also includes various modifications and modifications within the scope of equality. Moreover, various combinations and methods, as well as other combinations and methods including only one element, or elements above or below it, are also within the scope and concept of the present disclosure.

[0056] For example, in the first embodiment, the resistivity of the SiC single crystal 3 is gradually increased or decreased by periodically and repeatedly changing the flow rate of the doping gas 22 . However, this can be performed by other methods other than adjusting the flow rate of the doping gas 22 .

[0057] That is to say, Figure 5 As shown, even if the growth rate is slowly increased or decreased relative to the growth time, the amount of dopant obtained can be changed, and the resistivity of the SiC single crystal 3 can be changed periodically. For example, if the flow rate of the doping gas 22 is set to a fixed condition, the growth rate of the SiC single crystal 3 can be increased by increasing the flow rate of the raw material gas 20, increasing the partial pressure of the raw material gas 20, and reducing the surface temperature of the SiC single crystal 3. Therefore, by adjusting one or more of the flow rate or partial pressure of the raw material gas 20, the surface temperature of the SiC single crystal 3, etc., the growth rate of the SiC single crystal 3 can be slowly increased or decreased periodically, and the resistivity of the SiC single crystal 3 can be changed periodically.

[0058] In the above description, the resistivity of the SiC single crystal 3 is periodically varied, but it is not necessary to vary it at a fixed period. Figure 6 As shown, the resistivity change may be irregular as long as the resistivity is changed by slowly increasing and slowly decreasing the resistivity relative to the growth distance of the SiC single crystal 3 repeatedly. In this case, the change cycle of each repeated increase and decrease can be converted into a length of the SiC single crystal 3 of less than 500 μm.

[0059] In addition, in the first embodiment, as the SiC single crystal manufacturing device 1, an example is given of an apparatus of an upward blowing method in which, after the raw material gas 20 is supplied to the growth surface of the SiC single crystal 3, the raw material gas 20 is further discharged upward through the outer peripheral surface of the SiC single crystal 3 and the lateral direction of the susceptor 10. However, it is not limited to this, and it may also be a method in which, after the raw material gas 20 is supplied to the growth surface of the SiC single crystal 3, it is returned to the same direction as the supply direction, that is, a back-blowing method. In addition, it may also be a method in which, after the raw material gas 20 is supplied to the growth surface of the SiC single crystal 3, it is discharged toward the outer peripheral direction of the heating container 9, that is, a side blowing method.

Claims

1. A silicon carbide single crystal, wherein: At least a part of the region within the crystal repeats a change in resistivity in which the resistivity gradually increases and decreases in the growth direction.

2. The silicon carbide single crystal according to claim 1, wherein: The variation range of the resistivity is 0.5% or more and 50% or less.

3. The silicon carbide single crystal according to claim 1, wherein: The repeated fluctuation period of the increase and decrease of the resistivity is 500 μm or less when converted into the length of the crystal.

4. The silicon carbide single crystal according to claim 1, wherein: The variation range of the resistivity is 0.5% or more and 10% or less, and a period of repeated increase and decrease of the resistivity is 100 μm or less when converted into a length of the crystal.

5. The silicon carbide single crystal according to any one of claims 1 to 4, wherein The portion where the resistivity changes repeatedly occurs is the small plane region.

6. A method for producing a silicon carbide single crystal, comprising the following steps: A susceptor (10) is arranged in a crucible (9) having a hollow portion constituting a reaction chamber, and a seed crystal (2) for growing a silicon carbide single crystal (3) is arranged on one surface of the susceptor; and A raw material gas (20) of silicon carbide, a carrier gas (21), and a doping gas (22) containing a dopant for growing the silicon carbide single crystal are supplied from below the susceptor toward the surface of the seed crystal, and the raw material gas is heated and decomposed and then supplied to the seed crystal, thereby growing the silicon carbide single crystal on the surface of the seed crystal. in, In the step of growing the silicon carbide single crystal, an operation of gradually increasing and an operation of gradually decreasing the resistivity with respect to a growth distance of the silicon carbide single crystal are repeated to grow the silicon carbide single crystal.

7. The method for producing a silicon carbide single crystal according to claim 6, wherein: In the step of growing the silicon carbide single crystal, the flow rate of the doping gas is periodically varied, thereby repeating an operation of gradually increasing and gradually decreasing the resistivity with respect to a growth distance of the silicon carbide single crystal.

8. The method for producing a silicon carbide single crystal according to claim 6, wherein: In the step of growing the silicon carbide single crystal, by changing any one or more of the flow rate or partial pressure of the raw material gas and the temperature of the growth surface of the silicon carbide single crystal, the operation of slowly increasing and slowly decreasing the resistivity relative to the growth distance of the silicon carbide single crystal is repeated.