Calcium sulfate whisker preparation process
By adding dispersants and regulators to the calcium sulfate whisker preparation process, controlling the pH value and activation index, and combining the crystallization, drying, aging and calcination steps, the problems of high purification costs and environmental pollution in the preparation of calcium sulfate whiskers are solved. , achieved efficient and low-cost preparation of calcium sulfate whiskers, improving the performance and utilization of the material.
Patent Information
- Application Number
- CN202410883968.7
- Authority / Receiving Office
- CN · China
- Patent Type
- Applications(China)
- Current Assignee / Owner
- Filing Date
- 2024-07-03
- Publication Date
- 2024-10-15
AI Technical Summary
The existing calcium sulfate whisker preparation process has problems such as high calcium sulfate purification cost, low raw material conversion rate and environmental pollution. Moreover, the preparation conditions have an impact on the whisker length, crystal form and cost, and there is a lack of effective recycling solutions.
By dissolving the calcium-containing waste residue in water and adding a dispersant, adding organic acids and inorganic salt regulators after concentration, controlling the pH value and activation index, crystallizing, vacuum filtration, drying, aging and high-temperature calcination to ensure the stability of calcium sulfate whiskers. High purity and crystalline integrity, and improved material utilization through mother liquor recovery and cooling screening.
It achieves the high purity and crystalline integrity of calcium sulfate whiskers, reduces production costs and energy consumption, improves production efficiency and the environmental friendliness of materials, and is in line with the development trend of green chemical industry.
Smart Images

Figure CN118773744A_ABST
Abstract
Description
Technical Field
[0001] The invention relates to the technical field of material preparation, in particular to a process for preparing calcium sulfate whiskers. Background Art
[0002] Whisker is a fibrous solid. Due to its tiny structure, there is almost no sliding condition inside it, so it has the strength of an ideal crystal. Whisker is a material that is resistant to high temperature, has good toughness, high strength, chemical corrosion resistance, easy surface treatment and low toxicity. It has a good affinity with polymers such as rubber and plastics and is widely used in plastics, rubber, friction materials, papermaking, environmental engineering and other industries. Calcium sulfate whiskers with fibrous structure have excellent mechanical properties, stable chemical properties, high temperature resistance, acid and alkali resistance, chemical corrosion resistance, good compatibility and non-toxicity. Compared with other inorganic whiskers, it has the characteristics of low price, simple preparation and non-toxicity. It is a new type of green and environmentally friendly material. It can not only be used in the construction and home improvement industries, but also in the food, medicine and agriculture fields. Therefore, calcium sulfate whiskers have an incomparable market value over other whisker materials.
[0003] The performance of calcium sulfate whiskers mainly depends on the aspect ratio and the degree of crystallization integrity. With the advancement of science and technology, it is possible to control the growth of calcium sulfate whiskers and prepare nanofibrous calcium sulfate whiskers. Calcium sulfate whiskers can be divided into CaSO4·2H2O, CaSO4·(1 / 2)H2O and CaSO4·H2O whiskers according to their water content, and they can be converted into each other.
[0004] At present, a large amount of calcium-containing waste residue is generated in the production process of barium chloride, the main component of which is calcium sulfate. The source of calcium sulfate is: after purifying calcium sulfate, it is recrystallized in a solvent to obtain calcium sulfate whiskers. However, there are some major problems in the preparation process of calcium sulfate whiskers. First, the purification of calcium sulfate needs to take into account the purity of calcium sulfate, the purification cost, and the raw material conversion rate; second, the preparation conditions of calcium sulfate whiskers. The selection of solution system and components, the control of pH value and temperature and other parameters will directly affect the length and crystal form of calcium sulfate whiskers, raw material conversion rate, environmental pollution, and cost.
[0005] Therefore, research and development of calcium sulfate whisker preparation technology to achieve recycling of waste residue at a low cost and in an environmentally friendly manner has become a current research hotspot. Summary of the invention
[0006] In view of the deficiencies in the prior art, the present invention provides a process for preparing calcium sulfate whiskers, which solves the problem that the process for preparing calcium sulfate crystals in the prior art is not perfect.
[0007] To achieve the above object, the present invention is implemented by the following technical scheme: a calcium sulfate whisker preparation process, comprising the following steps:
[0008] S1. The calcium-containing waste residue is dissolved in water to form a calcium sulfate solution, wherein a dispersant is added to improve the dissolution efficiency, the mass percentage of the dispersant is 0.1%-2%;
[0009] S2. The calcium sulfate solution in step S1 is concentrated, and a regulator is added during the concentration process, wherein the regulator is composed of an organic acid and an inorganic salt, and is used to adjust the activation index and pH value of the solvent, wherein the mass percentage of the organic acid is 0.5%-3%, the mass percentage of the inorganic salt is 1%-5%, the activation index is controlled within the range of 0.8-1.2, and the pH value is controlled within the range of 6.5-8.5;
[0010] S3. The concentrated solution is crystallized at a temperature of 40-60 ° C for 2-4 hours;
[0011] S4. After crystallization, the calcium sulfate whiskers are vacuum filtered by a filtration device to remove the mother liquor, and the mother liquor is recycled after treatment;
[0012] S5. After filtering, the calcium sulfate whiskers are dried in a drying device at a drying temperature of 80-120°C for 2-4 hours;
[0013] S6. After drying, the calcium sulfate whiskers are aged at a temperature of 40-60° C. for 24-48 hours;
[0014] S7. After the aging treatment, the calcium sulfate whiskers are calcined in a calcination device at a calcination temperature higher than 650° C., so that the crystal water content of the final product is controlled within 1%. After the above steps, a high-purity, crystalline, and complete calcium sulfate whisker product is obtained.
[0015] Preferably, the dispersant in S1 is selected from one or more of polyacrylic acid, sodium polyacrylate, polymethyl methacrylate and polyhydroxyethyl acrylate.
[0016] Preferably, the organic acid in S2 is selected from one or more of acetic acid, citric acid, malic acid and tartaric acid, and the inorganic salt is selected from one or more of sodium sulfate and potassium sulfate.
[0017] Preferably, the vacuum filtration is performed using a plate and frame filter press or a centrifuge.
[0018] Preferably, the drying equipment is an oven, a fluidized bed dryer or a spray dryer.
[0019] Preferably, the aging treatment is carried out in a sealed container to reduce the volatilization of water.
[0020] Preferably, the calcination process adopts one of static calcination or circulating belt rolling calcination to achieve the required high temperature.
[0021] Preferably, S7 further comprises cooling and screening the calcined calcium sulfate whiskers to obtain a product with uniform particle size distribution, wherein the cooling process adopts natural cooling or forced air cooling to room temperature, and the screening process adopts a vibrating screen or a rotary screen with a mesh size of 20-120.
[0022] The present invention provides a process for preparing calcium sulfate whiskers, which has the following beneficial effects:
[0023] 1. The present invention achieves strict control over the quality and purity of calcium sulfate whiskers by accurately controlling the parameters of each link, including the selection of dispersants, the use of regulators in the concentration process, crystallization and drying conditions, aging and calcination treatments, etc., and by adding a regulator composed of an organic acid and an inorganic salt in the concentration step, not only the activation index and pH value of the solvent are optimized, but also the dissolution efficiency and crystal quality are improved. In addition, through specific aging and high-temperature calcination treatments, the high purity and crystal integrity of the product are further ensured, so that it exhibits more excellent performance in application.
[0024] 2. The present invention not only significantly improves the production efficiency of calcium sulfate whiskers through vacuum filtration technology and efficient drying equipment, but also effectively reduces energy consumption and production costs. The temperature control technology in the crystallization process and aging steps ensures the uniformity and stability of whisker growth, thereby obtaining products with uniform particle size distribution and regular shape, which can provide better enhancement effect and processing performance. In addition, through the recycling of mother liquor and the cooling and screening process of the calcined product, the utilization rate and environmental friendliness of the material are further improved, which is in line with the development trend of current green chemical industry. BRIEF DESCRIPTION OF THE DRAWINGS
[0025] Figure 1 It is a schematic diagram of the process steps of an embodiment of the present invention;
[0026] Figure 2 This is a schematic diagram of the process steps of Comparative Example 1 of the present invention;
[0027] Figure 3 Schematic diagram of the process steps of Comparative Example 2 of the present invention. DETAILED DESCRIPTION
[0028] The following will be combined with the drawings in the specification of the present invention to clearly and completely describe the technical solutions in the embodiments of the present invention. Obviously, the described embodiments are only part of the embodiments of the present invention, not all of the embodiments. Based on the embodiments of the present invention, all other embodiments obtained by ordinary technicians in this field without creative work are within the scope of protection of the present invention.
[0029] Embodiment 1:
[0030] Please refer to the attached Figure 1 The present invention provides a process for preparing calcium sulfate whiskers, comprising the following steps: Step S1: taking 100 g of calcium-containing waste residue, dissolving it in 1000 mL of water, adding sodium polyacrylate as a dispersant, the amount of which is 1% of the mass of the waste residue. Stirring for 2 hours to ensure complete dissolution;
[0031] Step S2: Concentrate the solution to half of its original volume, and add a regulator consisting of acetic acid and sodium sulfate. The amount of acetic acid added is 2% of the mass of the waste residue, and the amount of sodium sulfate added is 3% of the mass of the waste residue. Adjust the activation index to 1.0 and control the pH at 7.0;
[0032] Step S3: transferring the solution to a crystallization container, controlling the crystallization temperature at 50° C., and the crystallization time for 3 hours;
[0033] Step S4: After the crystallization is completed, vacuum filtration is performed using a plate and frame filter press to remove the mother liquor;
[0034] Step S5: placing the filtered calcium sulfate whiskers in an oven and drying them at 100° C. for 3 hours;
[0035] Step S6: the dried whiskers are aged in a sealed container at a temperature of 50° C. for 48 hours;
[0036] Step S7: The aged whiskers are sent to a calcining device and calcined at 700° C. for 2 hours. The calcined product is naturally cooled to room temperature and sieved through a vibrating screen with a mesh size of 60.
[0037] Embodiment 2:
[0038] Please refer to the attached Figure 1 The present invention provides a calcium sulfate whisker preparation process, comprising the following steps: Step S1: Take 150g of calcium-containing waste residue, dissolve it in 1500mL of water, add polymethyl methacrylate as a dispersant, and the amount is 1.5% of the mass of the waste residue. Stir until it is completely dissolved;
[0039] Step S2: Concentrate the solution to 60% of the original volume, and add a regulator consisting of malic acid and potassium sulfate. The amount of malic acid added is 1.5% of the mass of the waste residue, and the amount of potassium sulfate added is 2% of the mass of the waste residue. Adjust the activation index to 0.9 and control the pH at 7.5;
[0040] Step S3: transferring the solution to a crystallization container, controlling the crystallization temperature at 45° C., and the crystallization time for 4 hours;
[0041] Step S4: After the crystallization is completed, vacuum filtration is performed using a centrifuge to remove the mother liquor;
[0042] Step S5: drying the filtered calcium sulfate whiskers in a fluidized bed dryer at 90° C. for 2 hours;
[0043] Step S6: the dried whiskers are aged in a sealed container at a temperature of 45° C. for 36 hours;
[0044] Step S7: The aged whiskers are fed into a circulating belt rolling calcination device and calcined at 680° C. for 1.5 hours. The calcined product is forced air cooled to room temperature and sieved through a rotary sieve with a mesh size of 40.
[0045] Embodiment three:
[0046] Please refer to the attached Figure 1 The present invention provides a process for preparing calcium sulfate whiskers, comprising the following steps: Step S1: Take 200 g of calcium-containing waste residue, dissolve it in 2000 mL of water, add polyhydroxyethyl acrylate as a dispersant, and stir until it is completely dissolved;
[0047] Step S2: Concentrate the solution to 70% of the original volume, and add a regulator consisting of tartaric acid and sodium sulfate. The amount of tartaric acid added is 0.5% of the mass of the waste residue, and the amount of sodium sulfate added is 1% of the mass of the waste residue. Adjust the activation index to 1.1 and control the pH at 8.0;
[0048] Step S3: transferring the solution to a crystallization container, controlling the crystallization temperature at 60° C., and the crystallization time for 2 hours;
[0049] Step S4: After the crystallization is completed, vacuum filtration is performed using a plate and frame filter press to remove the mother liquor;
[0050] Step S5: drying the filtered calcium sulfate whiskers at 80° C. for 4 hours using a spray dryer;
[0051] Step S6: the dried whiskers are aged in a sealed container at a temperature of 60° C. for 24 hours;
[0052] Step S7: The aged whiskers are sent to a static calcination device and calcined at 650° C. for 3 hours. The calcined product is naturally cooled to room temperature and sieved through a vibrating screen with a mesh size of 120.
[0053] Comparative Example 1:
[0054] Please refer to the attached Figure 2 The comparative example of the present invention provides a preparation process of calcium sulfate whiskers, comprising the following steps: Step S1: taking 100 g of calcium-containing waste residue, directly dissolving it in 1000 mL of water without adding any dispersant, and after stirring for 2 hours, it is found that the dissolution efficiency is low;
[0055] Step S2: When the solution was concentrated to half of its original volume, a large amount of undissolved solids were found to remain. The same amount of acetic acid and sodium sulfate as in Example 1 was tried to be added as a regulator, but the regulator effect was not obvious due to insufficient dissolution at the front end;
[0056] Step S3 to Step S7: Due to the problems in the initial step, the subsequent steps failed to obtain satisfactory calcium sulfate whisker products, the crystals were of different sizes, the purity was low, the final product had a wide particle size distribution and poor crystal integrity.
[0057] Comparative Example 2:
[0058] Please refer to the attached Figure 3 The comparative example of the present invention provides a process for preparing calcium sulfate whiskers, comprising the following steps: Steps S1 to S6: performed according to the steps of Example 2, but omitting the aging treatment in step S7, and directly calcining the dried calcium sulfate whiskers;
[0059] Step S7: After the whiskers were calcined at 680°C for 1.5 hours, it was found that too much stress was generated inside the whiskers, causing some whiskers to break, affecting the quality and application effect of the product. This comparison illustrates the importance of aging treatment for improving the intrinsic quality and final performance of whiskers.
[0060] Although embodiments of the present invention have been shown and described, it will be appreciated by those skilled in the art that various changes, modifications, substitutions and variations may be made to the embodiments without departing from the principles and spirit of the present invention, and that the scope of the present invention is defined by the appended claims and their equivalents.
Claims
1. A process for preparing calcium sulfate whiskers, characterized in that: The following steps are involved: S1. The calcium-containing waste residue is dissolved in water to form a calcium sulfate solution, wherein a dispersant is added to improve the dissolution efficiency, the mass percentage of the dispersant is 0.1%-2%; S2. The calcium sulfate solution in step S1 is concentrated, and a regulator is added during the concentration process, wherein the regulator is composed of an organic acid and an inorganic salt, and is used to adjust the activation index and pH value of the solvent, wherein the mass percentage of the organic acid is 0.5%-3%, the mass percentage of the inorganic salt is 1%-5%, the activation index is controlled within the range of 0.8-1.2, and the pH value is controlled within the range of 6.5-8.5; S3. The concentrated solution is crystallized at a temperature of 40-60 ° C for 2-4 hours; S4. After crystallization, the calcium sulfate whiskers are vacuum filtered by a filtration device to remove the mother liquor, and the mother liquor is recycled after treatment; S5. After filtering, the calcium sulfate whiskers are dried in a drying device at a drying temperature of 80-120°C for 2-4 hours; S6. After drying, the calcium sulfate whiskers are aged at a temperature of 40-60° C. for 24-48 hours; S7. After the aging treatment, the calcium sulfate whiskers are calcined in a calcination device at a calcination temperature higher than 650° C., so that the crystal water content of the final product is controlled within 1%. After the above steps, a high-purity, crystalline, and complete calcium sulfate whisker product is obtained.
2. A calcium sulfate whisker preparation process according to claim 1, characterized in that, The dispersant in S1 is selected from one or more of polyacrylic acid, sodium polyacrylate, polymethyl methacrylate and polyhydroxyethyl acrylate.
3. A calcium sulfate whisker preparation process according to claim 1, characterized in that, The organic acid in S2 is selected from one or more of acetic acid, citric acid, malic acid and tartaric acid, and the inorganic salt is selected from one or more of sodium sulfate and potassium sulfate.
4. A calcium sulfate whisker preparation process according to claim 1, characterized in that, The vacuum filtration is performed using a plate and frame filter press or a centrifuge.
5. A calcium sulfate whisker preparation process according to claim 1, characterized in that, The drying equipment is an oven, a fluidized bed dryer or a spray dryer.
6. A calcium sulfate whisker preparation process according to claim 1, characterized in that, The aging treatment is carried out in a sealed container to reduce the volatilization of water.
7. A process for preparing calcium sulfate whiskers according to claim 1, characterized in that, The calcination process adopts one of static calcination or circulating belt rolling calcination to achieve the required high temperature.
8. A process for preparing calcium sulfate whiskers according to claim 1, characterized in that, The S7 further includes cooling and screening the calcined calcium sulfate whiskers to obtain a product with uniform particle size distribution, wherein the cooling process uses natural cooling or forced air cooling to room temperature, and the screening process uses a vibrating screen or a rotary screen with a mesh size of 20-120.