Silver-based brazing filler metal component regulation and control method for high-nitrogen steel / tungsten alloy connection

By constructing and adjusting crystal models of high-nitrogen steel and tungsten alloys, screening and testing target crystal planes, and determining the optimal silver-based solder composition, the problems of low brazing connection efficiency and insufficient joint strength were solved, and efficient brazing was achieved. welding effect.

CN118773746APending Publication Date: 2024-10-15JINHUA SHUANGHUAN BRAZING ALLOYS +2
View PDF 0 Cites 8 Cited by

Patent Information

Application Number
CN202410781324.7
Authority / Receiving Office
CN · China
Patent Type
Applications(China)
Current Assignee / Owner
Filing Date
2024-06-17
Publication Date
2024-10-15

AI Technical Summary

Technical Problem

It is difficult to quickly and efficiently regulate the composition of silver-based filler metal for brazing high-nitrogen steel and tungsten alloy with existing technology, resulting in low brazing connection efficiency and insufficient joint strength.

Method used

By constructing crystal models of high-nitrogen steel and tungsten alloy, conducting multiple crystal face cutting and convergence tests, screening target crystal faces, building a clean interface model and adjusting substitution atoms to obtain a doped interface model, and determining the optimal one based on performance testing. Silver-based solder components.

Benefits of technology

The rapid and efficient regulation of the brazing filler metal components for high-nitrogen steel/tungsten alloy brazing is achieved, which improves the efficiency and joint strength of the brazing connection and ensures the welding performance.

✦ Generated by Eureka AI based on patent content.

Smart Images

  • Figure CN118773746A_ABST
    Figure CN118773746A_ABST
Patent Text Reader

Abstract

The invention provides a silver-based brazing filler metal component regulation and control method for high-nitrogen steel / tungsten alloy connection. The method comprises the steps that an Fe crystal model corresponding to an Fe element in high-nitrogen steel, a W crystal model corresponding to a W element in tungsten alloy and a silver-based brazing filler metal crystal model corresponding to a first silver-based brazing filler metal component comprising an Ag element are constructed; performing multiple times of crystal face cutting on the Fe crystal model, the W crystal model and the silver-based brazing filler metal crystal model to obtain multiple crystal faces, and screening out three target crystal faces; respectively carrying out convergence test on the three obtained target crystal faces, and confirming the number of target atomic layers of each target crystal face according to a convergence test result so as to construct a clean interface model; replacing Ag atoms in the clean interface model by adopting at least one substitution atom so as to adjust the clean interface model to obtain different doped interface models; and on the basis of performance test results of the clean interface model and the doped interface model, the doped interface model with the optimal performance test result is determined, so that the optimal silver-based solder component is determined.
Need to check novelty before this filing date? Find Prior Art

Description

Technical Field

[0001] The present application relates to the field of welding materials, and in particular to a method for controlling the composition of a silver-based solder for high nitrogen steel / tungsten alloy connection. Background Art

[0002] In high nitrogen steel, nitrogen can significantly improve its yield strength and tensile strength without reducing the ductility and toughness of stainless steel through mechanisms such as fine grain strengthening, deformation strengthening, precipitation strengthening and solid solution strengthening, making it have the advantages of high hardness, high wear resistance, high strength and corrosion resistance. Tungsten alloy is a two-phase composite material composed of tungsten phase and bonding phase. It has the characteristics of high strength, high density, good thermal conductivity, high melting point, high sputtering resistance and low tritium retention. Therefore, it is widely used in military industry, aerospace, nuclear industry and civil industry. However, tungsten alloy has the disadvantages of high cost, high density and difficult processing, which is not conducive to lightweight and cost reduction. It is often used in connection with steel structure materials in industrial applications. Therefore, the research on brazing connection between tungsten alloy and high nitrogen steel has important application value.

[0003] However, the melting point and thermal expansion coefficient of tungsten alloy and steel are very different, and intermetallic compounds are easily generated in brazed joints, thereby reducing the strength of the joints. As a result, there are only a few studies on tungsten / steel brazing. At present, most brazing research at home and abroad is only driven by phenomenology, such as the vacuum diffusion brazing of W-(Ni-Cr-Fe-Si-B) mixed powder intermediate layer to connect tungsten and steel in the "Chinese Journal of Nonferrous Metals". The joint microstructure and performance are evaluated through a series of traditional experiments and characterization methods. This method is inefficient and the efficiency still needs to be improved.

[0004] How to quickly and efficiently regulate the composition of silver-based solder for high nitrogen steel / tungsten alloy brazing is one of the difficulties in this field. Based on this, it is urgent to develop relevant methods for regulating the composition of silver-based solder for high nitrogen steel / tungsten alloy brazing, improve research in related fields, and improve solder production efficiency and product quality. Summary of the invention

[0005] In view of this, the purpose of the present application is to provide a method for regulating the composition of silver-based solder for high nitrogen steel / tungsten alloy connection, which effectively solves the problem of not being able to quickly and efficiently regulate the solder composition for high nitrogen steel / tungsten alloy brazing.

[0006] In the first aspect, the present invention provides a method for controlling the composition of a silver-based solder for high nitrogen steel / tungsten alloy connection, the method comprising:

[0007] Constructing respectively the Fe crystal model corresponding to the Fe element in the high nitrogen steel, the W crystal model corresponding to the W element in the tungsten alloy, and the silver-based solder crystal model corresponding to the first silver-based solder component including the Ag element; wherein the silver-based solder crystal model includes Ag atoms;

[0008] The Fe crystal model, the W crystal model and the silver-based solder crystal model are subjected to multiple crystal plane cutting to obtain multiple crystal planes of the Fe crystal model, the W crystal model and the silver-based solder crystal model, and target crystal planes corresponding to the Fe crystal model, the W crystal model and the silver-based solder crystal are selected from the obtained multiple crystal planes;

[0009] Conducting convergence tests on the three target crystal planes obtained respectively, and confirming the target atomic layer of each crystal plane according to the convergence test results, so as to construct a clean interface model based on the target atomic layer of at least part of the crystal planes;

[0010] At least one substitution atom is used to replace the Ag atom in the clean interface model, so as to adjust the clean interface model to obtain different doped interface models; different doped interface models correspond to different second silver-based solder components;

[0011] Based on the performance test results of the clean interface model and the doped interface model, the doped interface model with the best performance test results is determined to determine the optimal silver-based solder composition.

[0012] In combination with the first aspect, the embodiment of the present application provides a first possible implementation of the first aspect, wherein the performance test results based on the clean interface model and the doped interface model determine the doped interface model with the best performance test results to determine the optimal silver-based solder component, including:

[0013] Performing a performance test on the clean interface model based on second preset parameters to obtain a performance test result corresponding to the clean interface model, wherein the second preset parameters include interface adhesion work, charge density, differential charge density, state density, and Mulliken layout number;

[0014] Testing the performance of multiple doping interface models based on the second preset parameters to obtain a performance test result corresponding to each doping interface model;

[0015] The obtained performance test results are compared to determine that the silver-based solder component corresponding to the best performance test result is the best silver-based solder component.

[0016] In combination with the first aspect, the embodiment of the present application provides a second possible implementation of the first aspect, wherein a Fe crystal model corresponding to the Fe element in the high nitrogen steel, a W crystal model corresponding to the W element in the tungsten alloy, and a silver-based solder crystal model corresponding to the first silver-based solder component including the Ag element are respectively constructed, including:

[0017] Based on the atomic structures corresponding to the Fe element, the W element and the first silver-based solder component including the Ag element, respectively, an initial Fe crystal model, a W crystal model and a silver-based solder crystal model are constructed by using crystal structure visualization software;

[0018] The initial Fe crystal model, W crystal model and silver-based solder crystal model are structurally optimized based on first preset parameters to obtain optimized Fe crystal model, W crystal model and silver-based solder crystal model; the first preset parameters include functional, pseudopotential, K-point grid, cutoff energy, maximum stress and maximum displacement.

[0019] In combination with the first aspect, the embodiment of the present application provides a third possible implementation scheme of the first aspect, wherein the crystal planes cut by the Fe crystal model, the W crystal model and the silver-based solder crystal model include plane (111), plane (100), plane (001) and plane (010).

[0020] In combination with the first aspect, the embodiment of the present application provides a fourth possible implementation of the first aspect, wherein the three target crystal planes obtained are respectively subjected to convergence tests, and the target atomic layer of each crystal plane is confirmed according to the convergence test results, including:

[0021] Conducting a convergence test on the three target crystal planes to obtain a convergence test result; the convergence test includes a surface energy convergence test and an atomic layer spacing test;

[0022] If any one of the surface energy convergence test result and the atomic layer spacing test result included in the convergence test result is stable at a fixed value, the number of atomic layers corresponding to the first appearance of the fixed value is taken as the target number of atomic layers of the crystal plane.

[0023] In combination with the first aspect, the embodiment of the present application provides a fifth possible implementation of the first aspect, wherein the step of selecting target crystal planes corresponding to the Fe crystal model, the W crystal model and the silver-based solder crystal from the obtained multiple crystal planes comprises:

[0024] Obtain the slab angles and edge lengths of the atomic layers of multiple crystal planes;

[0025] The target crystal plane is obtained by screening the lamella angles and side lengths of multiple crystal planes based on screening conditions, wherein the screening conditions are that the lamella angle of the atomic layer of the crystal plane reaches a preset angle and the mismatch degree of the side length of the atomic layer is lower than a preset threshold.

[0026] In combination with the first aspect, the embodiment of the present application provides a sixth possible implementation of the first aspect, wherein the Ag atom in the clean interface model is replaced by at least one substitution atom to adjust the clean interface model to obtain a different doping interface model, including:

[0027] Selecting different amounts of substitutional atoms to perform substitutional doping on some Ag atoms in the first silver-based solder component to obtain a plurality of second silver-based solder components, wherein the substitutional atoms include Cu atoms, Ti atoms, V atoms, and Ni atoms;

[0028] Different doping interface models were constructed based on a variety of second silver-based solder components.

[0029] In a second aspect, the present application also provides a silver-based solder component control device for high nitrogen steel / tungsten alloy connection, the device comprising:

[0030] A construction module is used to respectively construct an Fe crystal model corresponding to the Fe element in the high nitrogen steel, a W crystal model corresponding to the W element in the tungsten alloy, and a silver-based solder crystal model corresponding to the first silver-based solder component including the Ag element; wherein the silver-based solder crystal model includes Ag atoms;

[0031] A cutting module is used to perform multiple crystal face cutting on the silver-based solder crystal model to obtain multiple crystal faces of the silver-based solder crystal model;

[0032] A testing module, used to perform convergence tests on the three target crystal planes obtained respectively, and confirm the target atomic layer number of each target crystal plane according to the convergence test results, so as to construct a clean interface model based on the target atomic layer number of the target crystal plane;

[0033] An adjustment module, used to adjust the clean interface model based on the multiple second silver-based solder components respectively, to obtain the doping interface models corresponding to the multiple second silver-based solder components;

[0034] The determination module is used to determine the doping interface model with the best performance test results based on the performance test results of the clean interface model and the doping interface model, so as to determine the optimal silver-based solder component.

[0035] In a third aspect, an embodiment of the present application further provides an electronic device, comprising: a processor, a memory and a bus, wherein the memory stores machine-readable instructions executable by the processor, and when the electronic device is running, the processor and the memory communicate via the bus, and when the machine-readable instructions are executed by the processor, the steps of the silver-based solder component control method for high nitrogen steel / tungsten alloy connection are performed.

[0036] In a fourth aspect, an embodiment of the present application further provides a computer-readable storage medium having a computer program stored thereon, which, when executed by a processor, executes the steps of the method for controlling the composition of the silver-based solder for high nitrogen steel / tungsten alloy connection.

[0037] The silver-based solder component control method for high nitrogen steel / tungsten alloy connection provided in the embodiment of the present application first constructs an Fe crystal model corresponding to the Fe element in the high nitrogen steel, a W crystal model corresponding to the W element in the tungsten alloy, and a silver-based solder crystal model corresponding to the first silver-based solder component including the Ag element; wherein the silver-based solder crystal model includes Ag atoms; secondly, the Fe crystal model, the W crystal model, and the silver-based solder crystal model are subjected to multiple crystal face cutting to obtain multiple crystal faces of the Fe crystal model, the W crystal model, and the silver-based solder crystal model; target crystal faces corresponding to the Fe crystal model, the W crystal model, and the silver-based solder crystal are screened out from the obtained multiple crystal faces; then the obtained three target crystal faces are subjected to convergence tests respectively, and according to the convergence test results, The target atomic layer of each crystal plane is confirmed to construct a clean interface model based on the target atomic layer of at least part of the crystal plane, and then at least one substitutional atom is used to replace the Ag atoms in the clean interface model to adjust the clean interface model to obtain different doping interface models; different doping interface models correspond to different second silver-based solder components; the second silver-based solder component is obtained by doping at least one substitutional atom and the first silver-based solder component, and finally, based on the performance test results of the clean interface model and the doping interface model, the doping interface model with the best performance test results is determined to determine the optimal silver-based solder component, so as to quickly and efficiently obtain the regulated high nitrogen steel / tungsten alloy brazing solder component and ensure the performance of the high nitrogen steel / tungsten alloy brazing solder component. BRIEF DESCRIPTION OF THE DRAWINGS

[0038] In order to more clearly illustrate the technical solutions of the embodiments of the present application, the drawings required for use in the embodiments will be briefly introduced below. It should be understood that the following drawings only show certain embodiments of the present application and therefore should not be regarded as limiting the scope. For ordinary technicians in this field, other related drawings can be obtained based on these drawings without paying creative work.

[0039] Figure 1 A flow chart of a first method for controlling the composition of a silver-based solder for high nitrogen steel / tungsten alloy connection provided in an embodiment of the present application is shown;

[0040] Figure 2 An atomic layer schematic diagram of a crystal plane provided in an embodiment of the present application is shown;

[0041] Figure 3 A schematic diagram showing an interface in a cleaning interface model provided in an embodiment of the present application is shown;

[0042] Figure 4 A comparison diagram of the differential charge density diagrams of the clean interface model and the doped interface model provided in the embodiment of the present application is shown;

[0043] Figure 5 The localized electron function diagram of the clean interface model and the doped interface model provided in the embodiments of the present application is shown;

[0044] Figure 6 A schematic structural diagram of a first silver-based solder component control device for high nitrogen steel / tungsten alloy connection provided in an embodiment of the present application is shown;

[0045] Figure 7 A schematic structural diagram of an electronic device provided in an embodiment of the present application is shown. DETAILED DESCRIPTION

[0046] To make the purpose, technical scheme and advantages of the embodiments of the present application clearer, the technical scheme in the embodiments of the present application will be clearly and completely described below in conjunction with the drawings in the embodiments of the present application. It should be understood that the drawings in the present application only serve the purpose of explanation and description and are not used to limit the scope of protection of the present application. In addition, it should be understood that the schematic drawings are not drawn in real proportion. The flowchart used in this application shows the operations implemented according to some embodiments of the present application. It should be understood that the operations of the flowchart can be implemented out of sequence, and the steps without logical context can be reversed in order or implemented simultaneously. In addition, those skilled in the art can add one or more other operations to the flowchart under the guidance of the content of the present application, or remove one or more operations from the flowchart.

[0047] In addition, the described embodiments are only a part of the embodiments of the present application, rather than all the embodiments. The components of the embodiments of the present application described and shown in the drawings here can be arranged and designed in various configurations. Therefore, the following detailed description of the embodiments of the present application provided in the drawings is not intended to limit the scope of the application claimed for protection, but merely represents the selected embodiments of the present application. Based on the embodiments of the present application, all other embodiments obtained by those skilled in the art without making creative work belong to the scope of protection of the present application.

[0048] It should be noted that the term "comprising" will be used in the embodiments of the present application to indicate the existence of the features declared thereafter, but does not exclude the addition of other features.

[0049] The characteristics of tungsten alloy, such as high strength, high density, good thermal conductivity, high melting point, high sputtering resistance and low tritium retention, and the characteristics of steel, including high nitrogen steel, such as high hardness, high wear resistance, high strength and corrosion resistance, make the research on brazing connection of tungsten alloy and high nitrogen steel have important application value.

[0050] However, there are large differences in melting point and thermal expansion coefficient between tungsten alloy and steel including high nitrogen steel during welding, and intermetallic compounds are easily generated in the brazed joint, which can easily reduce the strength of the joint between tungsten alloy and high nitrogen steel. As a result, there are only a few studies on tungsten / steel brazing. So how to successfully weld tungsten alloy and high nitrogen steel together with guaranteed performance has become a big problem.

[0051] Based on this, the embodiments of the present application provide a method for controlling the composition of a silver-based solder for high nitrogen steel / tungsten alloy connection, which is described below through an embodiment.

[0052] Example 1

[0053] To facilitate understanding of this embodiment, the method for controlling the composition of the silver-based solder for high nitrogen steel / tungsten alloy connection disclosed in the embodiment of this application is first introduced in detail. Figure 1 In the flowchart of the silver-based solder composition control method for high nitrogen steel / tungsten alloy connection shown in FIG. 1 , the method comprises:

[0054] S101, constructing respectively an Fe crystal model corresponding to the Fe element in the high nitrogen steel, a W crystal model corresponding to the W element in the tungsten alloy, and a silver-based solder crystal model corresponding to the first silver-based solder component including the Ag element; wherein the silver-based solder crystal model includes Ag atoms;

[0055] S102, performing multiple crystal face cutting on the Fe crystal model, the W crystal model and the silver-based solder crystal model respectively to obtain multiple crystal faces of the Fe crystal model, the W crystal model and the silver-based solder crystal model, and selecting target crystal faces corresponding to the Fe crystal model, the W crystal model and the silver-based solder crystal respectively from the obtained multiple crystal faces;

[0056] S103, respectively performing convergence tests on the three target crystal planes obtained, and confirming the target atomic layer number of each target crystal plane according to the convergence test results, so as to construct a clean interface model based on the target atomic layer number of the target crystal plane;

[0057] S104, using at least one substitution atom to replace the Ag atom in the clean interface model, so as to adjust the clean interface model to obtain different doped interface models; different doped interface models correspond to different second silver-based solder components;

[0058] S105. Based on the performance test results of the clean interface model and the doped interface model, determine the doped interface model with the best performance test results to determine the optimal silver-based solder component.

[0059] In step S101, Fe crystal model, W crystal model and silver-based solder crystal model corresponding to Fe element, W element and the first silver-based solder component including Ag element are constructed respectively, then the Fe crystal model includes Fe atoms, the W crystal model includes W atoms, and the silver-based solder crystal model includes Ag atoms, wherein the Fe atoms are the Fe atoms in high nitrogen steel, the W atoms are the W atoms in tungsten alloy, and the Ag atoms correspond to the Ag atoms in the silver-based solder, which are used to weld high nitrogen steel and tungsten alloy so that the high nitrogen steel and tungsten alloy can jointly play corresponding roles and effects.

[0060] In the specific implementation process of step S101, since atoms generally flow to places with lower energy, in order to make the atoms close to the real state, it is necessary to optimize, that is, adjust the positions of the atoms.

[0061] Therefore, in the specific implementation process of step S101, one implementation method is: constructing a Fe crystal model corresponding to the Fe element in the high nitrogen steel, a W crystal model corresponding to the W element in the tungsten alloy, and a silver-based solder crystal model corresponding to the first silver-based solder component including the Ag element, respectively, including:

[0062] S1011, constructing an initial Fe crystal model, a W crystal model, and a silver-based solder crystal model based on the atomic structures corresponding to the Fe element, the W element, and the first silver-based solder component including the Ag element by using a crystal structure visualization software;

[0063] S1012. Structural optimization is performed on the initial Fe crystal model, W crystal model and silver-based solder crystal model based on first preset parameters to obtain optimized Fe crystal model, W crystal model and silver-based solder crystal model; the first preset parameters include functional, pseudopotential, K-point grid, cutoff energy, maximum stress and maximum displacement.

[0064] In step S1011, the crystal structure visualization software includes but is not limited to Materials Studio and VESTA. The initial Fe crystal model, W crystal model and silver-based solder crystal model are constructed based on Fe atoms, W atoms and Ag atoms corresponding to Fe element, W element and Ag element respectively by using the two softwares of Materials Studio and VESTA of the crystal structure visualization software, wherein the lattice constant of Fe is The lattice constant of Ag is The lattice constant of W is The initial Fe crystal model, W crystal model and silver-based solder crystal model are constructed with the help of software such as CASTEP that can realize structural softening, and the initial Fe crystal model, W crystal model and silver-based solder crystal model are structurally optimized based on first preset parameters, wherein the first preset parameters include functional, pseudopotential, K-point grid, cutoff energy, maximum stress and maximum displacement, wherein the first preset parameters can be set to: functional: GGA of PBE; pseudopotential: ultrasoft pseudopotential; K-point grid: 4×4×1; cutoff energy: 517eV; maximum stress: 0.05GPa; maximum displacement: The optimized initial Fe crystal model, W crystal model and silver-based solder crystal model obtained by optimizing the first preset parameters are closest to the performance of the actual silver-based solder produced by Ag atoms when welding tungsten alloy and high nitrogen steel.

[0065] In step S102, the obtained Fe crystal model, W crystal model and silver-based solder crystal model are cut multiple times to obtain multiple crystal planes corresponding to the Fe crystal model, W crystal model and silver-based solder crystal model, and the target crystal planes of the Fe crystal model, W crystal model and silver-based solder crystal model are respectively screened out from the multiple crystal planes corresponding to the Fe crystal model, W crystal model and silver-based solder crystal model.

[0066] In the specific implementation process of step S102, one implementation method is: the crystal planes cut from the Fe crystal model, the W crystal model and the silver-based solder crystal model include plane (111), plane (100), plane (001) and plane (010).

[0067] That is, the initial Fe crystal model, W crystal model and silver-based solder crystal model obtained in step S101 are respectively subjected to multiple crystal plane cutting, and the cut crystal planes include but are not limited to plane (111), plane (100), plane (001) and plane (010), thereby obtaining corresponding multiple crystal planes of the Fe crystal model, W crystal model and silver-based solder crystal model, each crystal plane including multiple atomic layers.

[0068] In the specific implementation process of step S102, another implementation method is: the step of selecting target crystal planes corresponding to the Fe crystal model, the W crystal model and the silver-based solder crystal from the obtained multiple crystal planes includes:

[0069] S1021, obtaining the slab angles and side lengths of the atomic layers of multiple crystal planes;

[0070] S1022, screening the slab angles and side lengths of multiple crystal planes based on screening conditions to obtain a target crystal plane, wherein the screening conditions are that the slab angle of the atomic layer of the crystal plane reaches a preset angle and the mismatch degree of the side length of the atomic layer is lower than a preset threshold.

[0071] In steps S1021-S1022, the lamina angle and side length of the atomic layer of each crystal face are determined from the multiple crystal faces corresponding to the Fe crystal model, the W crystal model and the silver-based solder crystal, that is, the lamina angle and side length of the atomic layer of the corresponding number of crystal faces are obtained according to the number of crystal faces obtained by cutting the silver-based solder crystal model, and the target crystal faces corresponding to the Fe crystal model, the W crystal model and the silver-based solder crystal are screened out from the multiple crystal faces corresponding to the Fe crystal model, the W crystal model and the silver-based solder crystal based on preset screening conditions. The screening condition is that the lamina angle of the atomic layer of the crystal face reaches a preset angle and the mismatch degree of the side length of the atomic layer of the crystal face is lower than a preset threshold. The preset angle and preset threshold are pre-set, and the specific values ​​can be set according to the actual situation, such as setting the preset threshold to 5%. The preset angle is generally set to 90 degrees. When a crystal face obtained by cutting does not meet the screening condition, this crystal face cannot be used as the target crystal face.

[0072] In step S103, the multiple target crystal planes obtained by screening are subjected to convergence tests to obtain convergence test results. The target atomic layer number of each target crystal plane is determined according to the convergence test results. The target atomic layer number is the atomic layer thickness that the target crystal plane should have, otherwise the crystal plane cannot maintain a stable state. Figure 2 As shown, the target atomic layers are 5, 6 and 7 from left to right, namely, the target crystal planes corresponding to the target atomic layers of 5, 6 and 7 are in a stable state, so as to construct a clean interface model based on the target atomic layers of the target crystal plane, and the specific construction method can be splicing, so that the constructed clean interface model is stable, thereby reducing the amount of calculation of the thickness of the atomic layer of the target crystal plane and reducing the calculation time.

[0073] In the specific implementation process of step S103, one implementation method is: the three target crystal planes are respectively subjected to convergence tests, and the target atomic layer number of each target crystal plane is confirmed according to the convergence test results, including:

[0074] S1031, performing a convergence test on the three target crystal planes to obtain a convergence test result; the convergence test includes a surface energy convergence test and an atomic layer spacing test;

[0075] S1032. If any one of the surface energy convergence test result and the atomic layer spacing test result included in the convergence test result is stable at a fixed value, the number of atomic layers corresponding to the first appearance of the fixed value is used as the target number of atomic layers of the crystal plane.

[0076] In step S1031, the calculation formulas of the surface energy convergence test and the atomic layer spacing test included in the convergence test are as follows:

[0077]

[0078]

[0079] Where E bulk and E slab Corresponding to the total energy of the single unit cell and the target crystal plane, γ surf is the surface energy test result, that is, the energy of cutting the target crystal surface. The single unit cell is any unit cell in the target crystal surface. N bulk and N slab They correspond to the number of atoms in the single unit cell and the target crystal plane, respectively, and A corresponds to the area of ​​the target crystal plane. and d ij They respectively represent the distance between the i-th layer and the j-th layer before and after relaxation of the target crystal plane, Δd is the rate of change of the atomic layer spacing of the atomic layers between the i-th layer and the j-th layer of the target crystal plane, that is, the atomic layer spacing test result. Here, a convergence test is performed on each screened target crystal plane to obtain the surface energy convergence test result and atomic layer spacing test result of each layer, where the surface energy convergence test results and atomic layer spacing test results are both specific values.

[0080] In step S1032, if the surface energy convergence test result or the atomic layer spacing test result included in the convergence test result is stable at a certain fixed value, it indicates that the target crystal plane is stable at this fixed value. The number of atomic layers of the target crystal plane corresponding to the first appearance of this fixed value is the target atomic layer number of the crystal plane, that is, the crystal plane at this target atomic layer number, i.e., atomic layer thickness, is in a stable state.

[0081] For example, the optimized Fe crystal model, W crystal model and silver-based solder crystal model are respectively cut on the (010) plane, and the convergence of the target crystal plane (010) after cutting is tested by calculating the surface energy. At the 5th layer of the crystal plane, the Fe, W and Ag atoms converge, that is, at the 5th layer, they can represent the real material properties, that is, the target atomic layer number of the target crystal plane obtained by cutting is 5 layers.

[0082] In step S104, in order to obtain the silver-based solder component with the best performance so that the performance of tungsten alloy and high nitrogen steel during welding is the best, the Ag atoms in the first silver-based solder component are adjusted using at least one substitutional atom to obtain multiple second silver-based solder components, and the clean interface models are adjusted based on the multiple second silver-based solder components, that is, the doped interface model is constructed based on the second silver-based solder component in the same way as the first silver-based solder component, that is, the doped interface models corresponding to the multiple second silver-based solder components are obtained in this way.

[0083] In the specific implementation process of step S104, one implementation method is: using at least one substitution atom to replace the Ag atom in the clean interface model to adjust the clean interface model to obtain a different doping interface model, including:

[0084] S1041, selecting substitutional atoms of different amounts for substitutional doping of some Ag atoms in the first silver-based solder component to obtain a plurality of second silver-based solder components, wherein the substitutional atoms include Cu atoms, Ti atoms, V atoms, and Ni atoms;

[0085] S1042. Construct different doping interface models based on various second silver-based solder components.

[0086] In step S1041, some Ag atoms in the silver-based solder crystal model are retained, and the content of the remaining Ag atoms is replaced by substitutional atoms, and the substitutional atoms are of different components, thereby obtaining a plurality of second silver-based solder components, wherein the substitutional atoms can be at least one of Cu atoms, Ti atoms, V atoms, and Ni atoms.

[0087] In step S1042, the obtained multiple second silver-based solder components are used to construct doping interface models in the same manner as the first silver-based solder component, thereby obtaining doping interface models corresponding to the multiple second silver-based solder components, and correspondingly, the obtained multiple doping interface models are structurally optimized based on first preset parameters, and the first preset parameters can be set to: functional: GGA of PBE; pseudopotential: ultrasoft pseudopotential; K-point grid: 4×4×1; cutoff energy: 517 eV; maximum stress: 0.05 GPa; maximum displacement: The doping interface model optimized by the first preset parameters can best represent the real silver-based solder obtained by the second silver-based solder component produced by Fe atoms, W atoms, Ag atoms and different substitutional atoms.

[0088] In step S105, performance tests are performed on the clean interface model and multiple doped interface models respectively to obtain performance test results based on the clean interface model and the doped interface model respectively, and the performance test results that meet the preset screening conditions are selected from the performance test results to obtain the optimal performance test results, and correspondingly, the optimal silver-based solder component is screened out from the first silver-based solder component and the multiple second silver-based solder components.

[0089] In the specific implementation process of step S105, one implementation method is: based on the performance test results of the clean interface model and the doped interface model, determining the doped interface model with the best performance test results to determine the optimal silver-based solder component includes:

[0090] S1051, performing a performance test on the clean interface model based on second preset parameters to obtain a performance test result corresponding to the clean interface model, wherein the second preset parameters include interface adhesion work, charge density, differential charge density, state density, and Mulliken layout number;

[0091] S1052, testing the performance of multiple doping interface models based on the second preset parameters to obtain a performance test result corresponding to each doping interface model;

[0092] S1053. Compare the obtained performance test results to determine that the silver-based solder component corresponding to the best performance test result is the best silver-based solder component.

[0093] In step S1051, the second preset parameter includes a calculation formula for the interface adhesion work:

[0094] W ad =(E x +E y +E z -E interface ) / A interface (3)

[0095] Among them, E X 、E y 、E z are the energies of the three atomic layers of Fe, W and Ag, E interface is the total energy of the interface structure; A interface is the interface area, W ad is the interface adhesion work, where the interface is the interface in the clean interface model; based on the second preset parameter, the clean interface model is performance tested to obtain a performance test result corresponding to the clean interface model, and the performance test result includes a bonding strength result and an electronic structure result of the clean interface model.

[0096] In step S1052, the performance of multiple doping interface models obtained from multiple second silver-based solder components is tested based on the second preset parameters to obtain performance test results corresponding to each doping interface model, wherein the calculation formula for the interface adhesion work is the same as formula (3), and the performance test results corresponding to each doping interface model include the bonding strength results and electronic structure results of the clean interface model.

[0097] In step S1053, the performance test results corresponding to the clean interface model obtained in step S1051 and step S1052 are compared with the performance test results corresponding to multiple doped interface models to obtain the optimal performance test result. The silver-based solder component corresponding to the doped interface model corresponding to the optimal performance test result is the optimal silver-based solder component. The silver-based solder produced according to the optimal silver-based solder component can best guarantee the performance of the joint obtained by welding tungsten alloy and high nitrogen steel.

[0098] For example, the bonding strength and electronic structure results of the clean interface model of high nitrogen steel (Fe) / Ag / tungsten alloy (W) and the doped interface model of high nitrogen steel (Fe) / AgCuTi / tungsten alloy (W) are calculated: by calculating the adhesion work of the clean interface model and multiple doped interface models respectively, the adhesion work of the clean interface of high nitrogen steel (Fe) / Ag / tungsten alloy (W) is 3.12 J / m 2 , the doping interface of high nitrogen steel (Fe) / AgCuTi / tungsten alloy (W) is 4.02J / m 2 That is, doping Cu and Ti into silver solder is more conducive to improving the bonding strength between the solder and the base material.

[0099] From the derived differential charge density diagrams of the clean interface model and the doped interface model, it can be concluded that the bonding strength results are as follows: Figure 4 As shown in the figure, there is no electron cloud overlap between Ag atoms and Fe atoms in the clean interface model, which indicates that there is no obvious charge transfer and electron sharing between Ag atoms and Fe atoms, and almost no bonding; the Ag atoms and W atoms are red, and there is electron cloud overlap, indicating that there is bonding between the two; in the doped interface, there is electron cloud overlap between Cu atoms and Fe atoms and W atoms, and the charge transfer between them is greater than that of Ag atoms, that is, the doped interface model improves the interface bonding strength relative to the clean interface model.

[0100] By analyzing the electronic localization functions of the clean interface model and the doped interface model, it can be seen that in the electronic structure results, such as Figure 5 As shown in the figure, in the clean interface model, Ag and Ag mainly show the characteristics of metallic bonds. In the doped interface model, Ag and Cu and Ti show the characteristics of ionic bonds and covalent bonds respectively. Cu and W and Fe show the characteristics of metallic bonds and ionic bonds. Through Mulliken layout analysis, as shown in Table 1, compared with Ag-Fe and Ag-W bonds, the covalent bond properties of Cu-Fe and Cu-W bonds are stronger, and the latter has a shorter bond length, indicating that in terms of electronic structure results, the bonding strength of Cu-Fe and Cu-W bonds is greater than that of Ag-Fe and Ag-W bonds. Therefore, the bonding strength of the doped interface model is higher than that of the clean interface model.

[0101] Table 1 Comparison of the Mulliken layout of the main chemical bonds of the clean interface model and the doped interface model

[0102]

[0103] In summary, by comparing the performance of the clean interface model of high nitrogen steel (Fe) / Ag / tungsten alloy (W) constructed based on the first silver-based solder component with the performance of the doped interface models of various high nitrogen steel (Fe) / AgCuTi / tungsten alloy (W) constructed based on various second silver-based solder components, it is finally established that the optimal silver-based solder component is the second silver-based solder component containing AgCuTi.

[0104] Example 2

[0105] The present application also provides a silver-based solder composition control device for high nitrogen steel / tungsten alloy connection, such as Figure 6 The block diagram of the silver-based solder component control device for high nitrogen steel / tungsten alloy connection shown in the figure, the function implemented by the silver-based solder component control device for high nitrogen steel / tungsten alloy connection corresponds to the steps of executing the silver-based solder component control method for high nitrogen steel / tungsten alloy connection on the terminal device. The device can be understood as a component of a server including a processor, and the device includes:

[0106] A construction module 601 is used to respectively construct an Fe crystal model corresponding to the Fe element in the high nitrogen steel, a W crystal model corresponding to the W element in the tungsten alloy, and a silver-based solder crystal model corresponding to the first silver-based solder component including the Ag element; wherein the silver-based solder crystal model includes Ag atoms;

[0107] A cutting module 602 is used to perform multiple crystal face cutting on the Fe crystal model, the W crystal model and the silver-based solder crystal model, respectively, to obtain multiple crystal faces of the Fe crystal model, the W crystal model and the silver-based solder crystal model, and to select target crystal faces corresponding to the Fe crystal model, the W crystal model and the silver-based solder crystal from the obtained multiple crystal faces;

[0108] A testing module 603 is used to perform convergence tests on the three target crystal planes obtained, respectively, and confirm the target atomic layer number of each target crystal plane according to the convergence test results, so as to construct a clean interface model based on the target atomic layer number of the target crystal plane;

[0109] An adjustment module 604 is used to replace the Ag atoms in the clean interface model with at least one substitution atom to adjust the clean interface model to obtain different doped interface models; different doped interface models correspond to different second silver-based solder components;

[0110] The determination module 605 is used to determine the doping interface model with the best performance test results based on the performance test results of the clean interface model and the doping interface model, so as to determine the optimal silver-based solder composition.

[0111] In a feasible implementation manner, the determination module 605 includes:

[0112] A first performance testing module is used to perform a performance test on the cleaning interface model based on second preset parameters to obtain a performance test result corresponding to the cleaning interface model, wherein the second preset parameters include interface adhesion work, charge density, differential charge density, state density and Mulliken layout number;

[0113] A second performance testing module, used to test the performance of multiple doping interface models based on second preset parameters to obtain a performance test result corresponding to each doping interface model;

[0114] The comparison module is used to compare the obtained performance test results and determine that the silver-based solder component corresponding to the best performance test result is the best silver-based solder component.

[0115] In a feasible implementation, the construction module 601 includes:

[0116] The first construction module is used to construct an initial Fe crystal model, a W crystal model and a silver-based solder crystal model through a crystal structure visualization software based on the atomic structures corresponding to the Fe element, the W element and the first silver-based solder component including the Ag element respectively;

[0117] The optimization module is used to perform structural optimization on the initial Fe crystal model, W crystal model and silver-based solder crystal model based on first preset parameters to obtain optimized Fe crystal model, W crystal model and silver-based solder crystal model; the first preset parameters include functional, pseudopotential, K-point grid, cutoff energy, maximum stress and maximum displacement.

[0118] In a feasible implementation, the cutting module 602 includes:

[0119] The crystal planes cut from the Fe crystal model, the W crystal model and the silver-based solder crystal model include plane (111), plane (100), plane (001) and plane (010).

[0120] In a feasible implementation, the testing module 603 includes:

[0121] A convergence test module is used to perform a convergence test on the three target crystal planes to obtain a convergence test result; the convergence test includes a surface energy convergence test and an atomic layer spacing test;

[0122] The stabilization module is used to set the number of atomic layers corresponding to the first appearance of the fixed value as the target number of atomic layers of the crystal plane if any one of the surface energy convergence test result and the atomic layer spacing test result included in the convergence test result is stabilized at a fixed value.

[0123] In a feasible implementation manner, the testing module 603 further includes:

[0124] An acquisition module, used for acquiring the slab angles and side lengths of the atomic layers of multiple crystal planes;

[0125] The screening module is used to screen the lamella angles and side lengths of multiple crystal planes based on screening conditions to obtain a target crystal plane, wherein the screening conditions are that the lamella angle of the atomic layer of the crystal plane reaches a preset angle and the mismatch degree of the side length of the atomic layer is lower than a preset threshold.

[0126] In a feasible implementation, the adjustment module 604 includes:

[0127] A doping module is used to select substitution atoms of different weights to perform substitution doping on some Ag atoms in the first silver-based solder component to obtain a plurality of second silver-based solder components, wherein the substitution atoms include Cu atoms, Ti atoms, V atoms, and Ni atoms;

[0128] The second building module is used to build different doping interface models based on multiple second silver-based solder components.

[0129] Example 3

[0130] An electronic device, such as Figure 7 As shown, it includes: a processor, a memory and a bus, the memory stores machine-readable instructions executable by the processor, when the electronic device is running, the processor and the memory communicate through the bus, and when the machine-readable instructions are executed by the processor, the steps of the silver-based solder component control method for high nitrogen steel / tungsten alloy connection are executed.

[0131] Example 4

[0132] A computer-readable storage medium stores a computer program, which, when executed by a processor, executes the steps of the silver-based solder composition control method for high-nitrogen steel / tungsten alloy connection.

[0133] Those skilled in the art can clearly understand that, for the convenience and simplicity of description, the specific working process of the system and device described above can refer to the corresponding process in the method embodiment, and will not be repeated in this application. In the several embodiments provided in this application, it should be understood that the disclosed system, device and method can be implemented in other ways. The device embodiments described above are merely schematic. For example, the division of the modules is only a logical function division. There may be other division methods in actual implementation. For example, multiple modules or components can be combined or integrated into another system, or some features can be ignored or not executed. Another point is that the mutual coupling or direct coupling or communication connection shown or discussed can be through some communication interfaces, indirect coupling or communication connection of devices or modules, which can be electrical, mechanical or other forms.

[0134] The modules described as separate components may or may not be physically separated, and the components shown as modules may or may not be physical units, that is, they may be located in one place or distributed on multiple network units. Some or all of the units may be selected according to actual needs to achieve the purpose of the solution of this embodiment.

[0135] In addition, each functional unit in each embodiment of the present application may be integrated into one processing unit, or each unit may exist physically separately, or two or more units may be integrated into one unit.

[0136] If the functions are implemented in the form of software functional units and sold or used as independent products, they can be stored in a non-volatile computer-readable storage medium that is executable by a processor. Based on this understanding, the technical solution of the present application can essentially be embodied in the form of a software product, or in other words, the part that contributes to the prior art or the part of the technical solution. The computer software product is stored in a storage medium, including several instructions for a computer device (which can be a personal computer, a platform server, or a network device, etc.) to perform all or part of the steps of the method described in each embodiment of the present application. The aforementioned storage medium includes: various media that can store program codes, such as USB flash drives, mobile hard disks, ROM, RAM, magnetic disks, or optical disks.

[0137] The above are only specific implementations of the present application, but the protection scope of the present application is not limited thereto. Any technician familiar with the technical field can easily think of changes or substitutions within the technical scope disclosed in the present application, which should be included in the protection scope of the present application. Therefore, the protection scope of the present application should be based on the protection scope of the claims.

Claims

1. A method for controlling the composition of silver-based solder for high nitrogen steel / tungsten alloy connection, characterized in that: The method comprises: Constructing respectively the Fe crystal model corresponding to the Fe element in the high nitrogen steel, the W crystal model corresponding to the W element in the tungsten alloy, and the silver-based solder crystal model corresponding to the first silver-based solder component including the Ag element; wherein the silver-based solder crystal model includes Ag atoms; The Fe crystal model, the W crystal model and the silver-based solder crystal model are subjected to multiple crystal plane cutting to obtain multiple crystal planes of the Fe crystal model, the W crystal model and the silver-based solder crystal model, and target crystal planes corresponding to the Fe crystal model, the W crystal model and the silver-based solder crystal are selected from the obtained multiple crystal planes; Conducting convergence tests on the three target crystal planes obtained respectively, confirming the target atomic layer number of each target crystal plane according to the convergence test results, and constructing a clean interface model based on the target atomic layer number of the target crystal plane; At least one substitution atom is used to replace the Ag atom in the clean interface model, so as to adjust the clean interface model to obtain different doped interface models; different doped interface models correspond to different second silver-based solder components; Based on the performance test results of the clean interface model and the doped interface model, the doped interface model with the best performance test results is determined to determine the optimal silver-based solder composition.

2. The method according to claim 1, characterized in that The method of determining the doping interface model with the best performance test results based on the performance test results of the clean interface model and the doping interface model to determine the optimal silver-based solder component includes: Performing a performance test on the clean interface model based on second preset parameters to obtain a performance test result corresponding to the clean interface model, wherein the second preset parameters include interface adhesion work, charge density, differential charge density, state density, and Mulliken layout number; Testing the performance of multiple doping interface models based on the second preset parameters to obtain a performance test result corresponding to each doping interface model; The obtained performance test results are compared to determine that the silver-based solder component corresponding to the best performance test result is the best silver-based solder component.

3. The method according to claim 1, characterized in that: The method of respectively constructing a Fe crystal model corresponding to the Fe element in the high nitrogen steel, a W crystal model corresponding to the W element in the tungsten alloy, and a silver-based solder crystal model corresponding to the first silver-based solder component including the Ag element comprises: Based on the atomic structures corresponding to the Fe element, the W element and the first silver-based solder component including the Ag element, respectively, an initial Fe crystal model, a W crystal model and a silver-based solder crystal model are constructed by using crystal structure visualization software; The initial Fe crystal model, W crystal model and silver-based solder crystal model are structurally optimized based on first preset parameters to obtain optimized Fe crystal model, W crystal model and silver-based solder crystal model; the first preset parameters include functional, pseudopotential, K-point grid, cutoff energy, maximum stress and maximum displacement.

4. The method according to claim 1, characterized in that: The crystal planes cut from the Fe crystal model, the W crystal model and the silver-based solder crystal model include plane (111), plane (100), plane (001) and plane (010).

5. The method according to claim 1, characterized in that The three target crystal planes are respectively subjected to convergence tests, and the target number of atomic layers of each target crystal plane is confirmed according to the convergence test results, including: Conducting a convergence test on the three target crystal planes to obtain a convergence test result; the convergence test includes a surface energy convergence test and an atomic layer spacing test; If any one of the surface energy convergence test result and the atomic layer spacing test result included in the convergence test result is stable at a fixed value, the number of atomic layers corresponding to the first appearance of the fixed value is taken as the target number of atomic layers of the crystal plane.

6. The method according to claim 1, characterized in that The step of selecting target crystal planes corresponding to the Fe crystal model, the W crystal model and the silver-based solder crystal from the obtained multiple crystal planes comprises: Obtain the slab angles and edge lengths of the atomic layers of multiple crystal planes; The target crystal plane is obtained by screening the lamella angles and side lengths of multiple crystal planes based on screening conditions, wherein the screening conditions are that the lamella angle of the atomic layer of the crystal plane reaches a preset angle and the mismatch degree of the side length of the atomic layer is lower than a preset threshold.

7. The method according to claim 1, characterized in that The step of replacing the Ag atoms in the clean interface model with at least one substitution atom to adjust the clean interface model to obtain different doping interface models includes: Selecting different amounts of substitutional atoms to perform substitutional doping on some Ag atoms in the first silver-based solder component to obtain a plurality of second silver-based solder components, wherein the substitutional atoms include Cu atoms, Ti atoms, V atoms, and Ni atoms; Different doping interface models were constructed based on a variety of second silver-based solder components.

8. A silver-based solder component control device for high nitrogen steel / tungsten alloy connection, characterized in that: The device comprises: A construction module is used to respectively construct an Fe crystal model corresponding to the Fe element in the high nitrogen steel, a W crystal model corresponding to the W element in the tungsten alloy, and a silver-based solder crystal model corresponding to the first silver-based solder component including the Ag element; wherein the silver-based solder crystal model includes Ag atoms; A cutting module is used to perform multiple crystal face cutting on the Fe crystal model, the W crystal model and the silver-based solder crystal model, respectively, to obtain multiple crystal faces of the Fe crystal model, the W crystal model and the silver-based solder crystal model, and to select target crystal faces corresponding to the Fe crystal model, the W crystal model and the silver-based solder crystal from the obtained multiple crystal faces; A testing module, used to perform convergence tests on the three target crystal planes obtained respectively, and confirm the target atomic layer of each crystal plane according to the convergence test results, so as to construct a clean interface model based on the target atomic layer of at least part of the crystal planes; An adjustment module, used to replace the Ag atoms in the clean interface model with at least one substitution atom, so as to adjust the clean interface model to obtain different doped interface models; different doped interface models correspond to different second silver-based solder components; The determination module is used to determine the doping interface model with the best performance test results based on the performance test results of the clean interface model and the doping interface model, so as to determine the optimal silver-based solder component.

9. An electronic device, characterized in that: include: A processor, a memory and a bus, wherein the memory stores machine-readable instructions executable by the processor, and when the electronic device is running, the processor and the memory communicate via the bus, and when the machine-readable instructions are executed by the processor, the steps of the silver-based solder component control method for high nitrogen steel / tungsten alloy connection as described in any one of claims 1 to 7 are performed.

10. A computer-readable storage medium, characterized in that: The computer readable storage medium stores a computer program, which, when executed by a processor, executes the steps of the method for controlling the composition of silver-based solder for high nitrogen steel / tungsten alloy connection as claimed in any one of claims 1 to 7.

Citation Information

Cited By

  • Method for predicting performance of high-entropy alloy brazing filler metal for brazing high-nitrogen steel / tungsten alloy

    CN119479889A

  • Method for predicting bonding performance of aluminum / aluminum-based brazing filler metal / high-nitrogen steel interface

    CN119489232A

  • High-nitrogen non-magnetic steel / ceramic heterogeneous brazing interface behavior prediction method

    CN119501218A

  • Method for predicting magnesium / high-nitrogen steel interface bonding performance based on first principle

    CN119517218A

  • Method and device for regulating and controlling performance of high-nitrogen steel / nickel-copper brazing filler metal through active elements

    CN119560080A