A kind of bio-based aramid fiber and preparation method thereof
The polymerization of m-phenylenediamine and furandiformyl chloride and the epoxy ring-opening reaction of epoxy monomers and m-phenylenediamine in an organic solvent, and the glass fibers modified by combining wet spinning process and silane coupling agents are carried out in an organic solvent. , solves the problem of low strength of bio-based aramid fiber, achieves the improvement of high strength and flame retardant performance, and expands its application range.
Patent Information
- Application Number
- CN202411259041.2
- Authority / Receiving Office
- CN · China
- Patent Type
- Patents(China)
- Current Assignee / Owner
- Filing Date
- 2024-09-10
- Publication Date
- 2024-11-26
- Estimated Expiration
- 2044-09-10
AI Technical Summary
The existing bio-based aramid fibers have problems in industrial applications, such as low strength, catalyst residue, and high cost. The fiber strength is improved by adding a third monomer, which cannot meet higher application needs.
The polymerization reaction is carried out by using m-phenylenediamine and furandiformyl chloride in the organic solvent, and the epoxy ring-opening reaction is carried out by epoxy monomer and m-phenylenediamine to form a block copolymer, combining wet spinning process and silane High-strength bio-based aramid fibers are prepared by modifying the coupling agent.
The high strength and flame retardant properties of bio-based aramid fiber are achieved, and the tensile strength reaches 8 cN/dtex or above, which expands its application field, avoids the use of catalysts and reduces production costs.
Smart Images

Figure SMS_1
Abstract
Description
Technical Field
[0001] The invention relates to a bio-based aramid fiber and a preparation method thereof, belonging to the technical field of bio-based aramid fibers. Background Art
[0002] Aromatic polyamides, such as meta-aramid, have excellent intrinsic flame retardant properties. They are widely used in flame retardant protective materials, high-temperature filter materials, honeycomb structures and skeleton reinforcement materials, etc., and play a very important role in process production and national defense and military industries.
[0003] Bio-based aramid material is a high-performance fiber material made from bio-based raw materials. It is a sustainable alternative with lower environmental impact and better biodegradability than traditional petroleum-based aramid materials. The production process of bio-based aramid materials does not require the use of toxic and harmful chemicals, has less environmental pollution, and can be recycled. Compared with traditional petroleum-based aramid materials, its production process has lower carbon emissions and can effectively reduce greenhouse gas emissions.
[0004] Bio-based materials as renewable materials have received extensive attention in recent years, but the bio-based aramid fibers prepared by conventional methods to replace isophthaloyl chloride have the problem of low strength, which seriously limits their application in the field of industrial reinforcement. At present, when preparing bio-based aramid fibers, the use of isocyanate for cross-linking often requires the use of a catalyst, which will remain in the fiber in large quantities, resulting in problems such as excessive heavy metals in the fiber, and the catalyst is expensive; or the method of adding a third monomer to prepare bio-based aramid fibers, but the degree of fiber strength improvement is low and cannot meet higher-level applications. Chinese patent application CN106011192A discloses a bio-based aramid based on furandicarboxylic acid and a preparation method thereof, which is prepared by polymerization reaction in a solvent using furandicarboxylic acid dimethyl ester and aromatic diamine as comonomers and Candida sp. 99-125 lipase as a catalyst. The strength performance of the bio-based aramid prepared by this preparation method is relatively low. Therefore, it is of great value to develop a high-strength bio-based polyamide fiber in the fiber industry. Summary of the invention
[0005] In view of the deficiencies in the prior art, the present invention provides a bio-based aramid fiber and a preparation method thereof. The bio-based aramid fiber has higher strength, thereby enabling the bio-based aramid fiber to have a wider range of applications.
[0006] The technical solution of the present invention to solve the above technical problems is as follows: a method for preparing bio-based aramid fiber, the preparation method comprising:
[0007] S1, in an organic solvent, meta-phenylenediamine and furan dicarboxylic acid chloride are polymerized to obtain a first polymerization solution;
[0008] In an organic solvent, an epoxy monomer and m-phenylenediamine undergo an epoxy ring-opening reaction to obtain a second polymerization liquid;
[0009] S2, after the first polymerization liquid and the second polymerization liquid are evenly mixed, furan dicarbonyl chloride is added to carry out polymerization reaction, and after the reaction is completed, the pH is adjusted to weak alkalinity to obtain a bio-based aramid polymer stock solution;
[0010] S3. The bio-based aramid polymer stock solution is formed by a wet spinning process to obtain the bio-based aramid fiber, wherein in the wet spinning process, glass fiber modified with a silane coupling agent is added to the coagulation bath.
[0011] Furthermore, the epoxy monomer is any one of 3-(oxiran-2-ylmethoxy)-N,N-bis(oxiran-2-ylmethyl)aniline, 4,5-epoxytetrahydrophthalic acid diglycidyl ester, N,N,O-triglycidyl p-aminophenol, and 1,3,5-triglycidyl-S-triazinetrione.
[0012] Furthermore, the organic solvent is any one or a combination of N,N-dimethylformamide, N,N-dimethylacetamide, dimethyl sulfoxide, and N-methylpyrrolidone.
[0013] Furthermore, in step S1, when preparing the first polymer solution, the molar ratio of m-phenylenediamine to furan dicarboxylic acid chloride is 1:(0.8-0.95);
[0014] When preparing the second polymerization solution, the molar ratio of the epoxy monomer to m-phenylenediamine is 1:(2-4);
[0015] The molar ratio of the m-phenylenediamine used in the first polymerization solution to the m-phenylenediamine used in the second polymerization solution is 10:(0.1-0.5);
[0016] The molar ratio of the m-phenylenediamine used in the first polymerization solution of step S1 to the furan dicarboxylic acid chloride used in step S2 is 1:(0.1-0.25).
[0017] Furthermore, in step S1, during the preparation of the first polymerization solution, the polymerization reaction temperature is 5-20°C;
[0018] In step S1, during the preparation of the second polymerization solution, the polymerization reaction temperature is 70-150°C.
[0019] Furthermore, in step S2, the polymerization reaction temperature is 15-30°C.
[0020] Furthermore, in step S3, the mass concentration of the glass fiber modified with the silane coupling agent in the coagulation bath is 1%-5%.
[0021] Furthermore, the coagulation bath temperature is 45-85° C., the coagulation bath is an aqueous solution of a polar solvent, the mass concentration of the polar solvent in the coagulation bath is 30-40%, and the coagulation bath length is 3-5 m.
[0022] Furthermore, the viscosity of the bio-based aramid polymer stock solution at 25° C. is 500-1000 Po, and the pH of the bio-based aramid polymer stock solution is 8-10.
[0023] The invention also discloses a bio-based aramid fiber, and the bio-based aramid fiber is prepared by adopting the preparation method of the invention.
[0024] The beneficial effects of the present invention are:
[0025] In the method for preparing bio-based aramid fiber of the present invention, epoxy monomers and meta-phenylenediamine are used to carry out epoxy ring-opening reaction. The reaction process does not use a catalyst and is simple. The multifunctional epoxy monomers cross-link the molecular chains in the reaction system to form a network structure inside the molecular chains, thereby improving the fiber strength. The reaction process is regulated by controlling the reaction temperature to avoid the problem of implosion. The process prepares a bulk polymer, and then furan dicarboxylic acid chloride is added to the reaction system to prepare a bio-based meta-aramid bulk polymer.
[0026] In addition, during the spinning process, by adding silane coupling agent to the glass fiber in the coagulation bath, it is coupled with the glass fiber during the coagulation and molding process of the aramid fiber, so that the prepared bio-based aramid fiber has higher flame retardant and strength properties, and the tensile strength can reach more than 8 cN / dtex.
[0027] In the method for preparing the bio-based aramid fiber of the present invention, the bio-based aramid fiber can be better formed by controlling the appropriate temperature and concentration conditions in the coagulation bath, and finally a high-strength bio-based aramid fiber is obtained. DETAILED DESCRIPTION
[0028] The specific implementation of the present invention is described in detail below. The present invention can be implemented in many other ways than those described herein, and those skilled in the art can make similar improvements without violating the connotation of the present invention, so the present invention is not limited by the specific embodiments disclosed.
[0029] Unless otherwise defined, all technical and scientific terms used herein have the same meaning as those commonly understood by those skilled in the art to which the present invention belongs. The terms used are only for describing specific embodiments and are not intended to limit the present invention.
[0030] A method for preparing bio-based aramid fiber, the preparation method comprising:
[0031] S1, in an organic solvent, meta-phenylenediamine and furan dicarboxylic acid chloride are polymerized to obtain a first polymerization solution;
[0032] In an organic solvent, an epoxy monomer and m-phenylenediamine undergo an epoxy ring-opening reaction to obtain a second polymerization liquid;
[0033] S2, after the first polymerization liquid and the second polymerization liquid are evenly mixed, furan dicarboxylic acid chloride is added to carry out block copolymerization reaction, and after the reaction is completed, the pH is adjusted to weak alkalinity to obtain a bio-based aramid polymer stock solution;
[0034] S3. The bio-based aramid polymer stock solution is formed by a wet spinning process to obtain the bio-based aramid fiber, wherein in the wet spinning process, glass fiber modified with a silane coupling agent is added to the coagulation bath, and during the coagulation and forming process of the aramid fiber, the glass fiber reinforces the aramid fiber to finally obtain the high-strength bio-based aramid fiber.
[0035] Specifically, the epoxy monomer is any one of 3-(oxiran-2-ylmethoxy)-N,N-bis(oxiran-2-ylmethyl)aniline, 4,5-epoxytetrahydrophthalic acid diglycidyl ester, N,N,O-triglycidyl p-aminophenol, and 1,3,5-triglycidyl-S-triazinetrione.
[0036] Specifically, the organic solvent is any one or a combination of N,N-dimethylformamide, N,N-dimethylacetamide, dimethyl sulfoxide, and N-methylpyrrolidone.
[0037] Specifically, in step S1, when preparing the first polymerization solution, the molar ratio of m-phenylenediamine to furan dicarboxylic acid chloride is 1:(0.8-0.95);
[0038] When preparing the second polymerization solution, the molar ratio of the epoxy monomer to m-phenylenediamine is 1:(2-4);
[0039] The molar ratio of the m-phenylenediamine used in the first polymerization solution to the m-phenylenediamine used in the second polymerization solution is 10:(0.1-0.5);
[0040] The molar ratio of the m-phenylenediamine used in the first polymerization solution of step S1 to the furan dicarboxylic acid chloride used in step S2 is 1:(0.1-0.25).
[0041] Specifically, in step S1, during the preparation of the first polymerization solution, the polymerization reaction temperature is 5-20°C;
[0042] In step S1, during the preparation of the second polymerization solution, the polymerization reaction temperature is 70-150°C.
[0043] Specifically, in step S2, the polymerization reaction temperature is 15-30°C.
[0044] Specifically, in step S3, the mass concentration of the glass fiber modified with the silane coupling agent in the coagulation bath is 1%-5%.
[0045] More specifically, glass fiber powder (the diameter of the glass fiber powder is 10 μm) is impregnated with silane coupling agent A110 and then dried to obtain glass fiber modified with silane coupling agent (A110-Fiberglass). A110-Fiberglass is added to the coagulation bath to achieve composite reinforcement between glass fiber and aramid fiber, thereby improving the strength and flame retardant properties of bio-based aramid fiber.
[0046] Specifically, the coagulation bath temperature is 45-85° C., the coagulation bath is an aqueous solution of a polar solvent, the mass concentration of the polar solvent in the coagulation bath is 30-40%, and the coagulation bath length is 3-5 m.
[0047] More specifically, the polar solvent is any one of N,N-dimethylformamide, N,N-dimethylacetamide, dimethyl sulfoxide, and N-methylpyrrolidone.
[0048] Specifically, the viscosity of the bio-based aramid polymer stock solution at 25° C. is 500-1000 Po, and the pH of the bio-based aramid polymer stock solution is 8-10.
[0049] The weight average molecular weight of the bio-based aramid polymer stock solution is 170,000-240,000, and the molecular weight distribution is 1.2-1.5.
[0050] More specifically, in step S2, an alkaline earth metal hydroxide or an organic amine is used to adjust the pH to 8-10, such as sodium hydroxide, calcium hydroxide, etc. Calcium hydroxide is used in the embodiment of the present invention, but it is not limited to these.
[0051] Specifically, the wet spinning process is as follows: preparing high-strength bio-based aramid fiber by coagulating the bio-based aramid polymer stock solution in a coagulation bath, stretching, washing, drying, heat treating, and curling.
[0052] More specifically, in the embodiment of the present invention, the stretching process conditions are: the draft ratio is 1.0-2.5 times, the stretching bath is a polar solvent aqueous solution with a concentration of 15-30%, and the heat treatment temperature is 350-450°C.
[0053] A bio-based aramid fiber is prepared by the preparation method of the present invention.
[0054] Example 1
[0055] Preparation of a bio-based aramid fiber:
[0056] (1) Preparation of the first polymerization solution:
[0057] Dissolving m-phenylenediamine in N,N-dimethylacetamide, then adding furan dicarboxylic acid chloride, controlling the reaction temperature to 5° C. to perform a polymerization reaction to obtain a first polymerization solution, wherein the molar ratio of m-phenylenediamine to furan dicarboxylic acid chloride is 1:0.8;
[0058] (2) Preparation of the second polymerization solution:
[0059] Dissolving 1,3,5-triglycidyl-S-triazinetrione in N,N-dimethylacetamide, adding m-phenylenediamine, and controlling the reaction temperature to 90° C. to perform polymerization reaction to obtain a second polymerization liquid, wherein the molar ratio of 1,3,5-triglycidyl-S-triazinetrione to m-phenylenediamine is 1:4;
[0060] The molar ratio of the intermediate phenylenediamine in step (1) to the intermediate phenylenediamine in step (2) is 10:0.2;
[0061] (3) Preparation of bio-based aramid polymer stock solution:
[0062] After the first polymerization liquid and the second polymerization liquid are evenly mixed, furan dicarbonyl chloride is added to react again, and the reaction temperature is controlled to be 20° C. After the reaction is completed, the pH is adjusted to 9 to obtain a bio-based aramid polymer stock solution, wherein the bio-based aramid polymer stock solution has a mass solid content of 10% and a viscosity of 873 Po.
[0063] The molar ratio of the intermediate phenylenediamine in step (1) to the furan dicarboxylic acid chloride in step (3) is 1:0.2.
[0064] (4) Wet spinning process:
[0065] The bio-based aramid polymer stock solution is coagulated in a coagulation bath, stretched, washed, dried, heat treated, and curled to prepare high-strength bio-based aramid fibers;
[0066] The mass concentration of the glass fiber modified with the silane coupling agent in the coagulation bath is 2%; the temperature of the coagulation bath is 60° C., the coagulation bath is an aqueous solution of N,N-dimethylacetamide, the mass concentration of N,N-dimethylacetamide in the coagulation bath is 35%, and the length of the coagulation bath is 4 m.
[0067] The stretching process conditions are: the draft ratio is 1.0 times, the stretching bath is an aqueous solution of N,N-dimethylacetamide, and the mass concentration of N,N-dimethylacetamide is 15%. The heat treatment temperature condition is 380°C.
[0068] Example 2
[0069] Preparation of a bio-based aramid fiber:
[0070] (1) Preparation of the first polymerization solution:
[0071] Dissolving m-phenylenediamine in N,N-dimethylformamide, then adding furan dicarboxylic acid chloride, controlling the reaction temperature to 8° C. to carry out polymerization reaction, to obtain a first polymerization solution, wherein the molar ratio of m-phenylenediamine to furan dicarboxylic acid chloride is 1:0.85;
[0072] (2) Preparation of the second polymerization solution:
[0073] Dissolving 3-(oxiran-2-ylmethoxy)-N,N-bis(oxiran-2-ylmethyl)aniline in N,N-dimethylformamide, adding m-phenylenediamine, and controlling the reaction temperature to be 100° C. to carry out polymerization reaction to obtain a second polymerization liquid, wherein the molar ratio of the 3-(oxiran-2-ylmethoxy)-N,N-bis(oxiran-2-ylmethyl)aniline to the m-phenylenediamine is 1:3.5;
[0074] The molar ratio of the intermediate phenylenediamine in step (1) to the intermediate phenylenediamine in step (2) is 10:0.5;
[0075] (3) Preparation of bio-based aramid polymer stock solution:
[0076] After the first polymerization liquid and the second polymerization liquid are uniformly mixed, furan dicarbonyl chloride is added to react again, and the reaction temperature is controlled to be 30° C. After the reaction is completed, the pH is adjusted to 10 to obtain a bio-based aramid polymer stock solution, wherein the bio-based aramid polymer stock solution has a mass solid content of 12% and a viscosity of 659 Po.
[0077] The molar ratio of the intermediate phenylenediamine in step (1) to the furan dicarboxylic acid chloride in step (3) is 1:0.15.
[0078] (4) Wet spinning process:
[0079] The bio-based aramid polymer stock solution is coagulated in a coagulation bath, stretched, washed, dried, heat treated, and curled to prepare high-strength bio-based aramid fibers;
[0080] The mass concentration of the glass fiber modified with the silane coupling agent in the coagulation bath is 3%; the temperature of the coagulation bath is 85° C., the coagulation bath is an aqueous solution of N,N-dimethylformamide, the mass concentration of N,N-dimethylformamide in the coagulation bath is 30%, and the length of the coagulation bath is 3 m.
[0081] The stretching process conditions are: the draft ratio is 2.5 times, the stretching bath is an aqueous solution of N,N-dimethylformamide, and the mass concentration of N,N-dimethylformamide is 30%. The heat treatment temperature condition is 420°C.
[0082] Example 3
[0083] Preparation of a bio-based aramid fiber:
[0084] (1) Preparation of the first polymerization solution:
[0085] Dissolving m-phenylenediamine in dimethyl sulfoxide, then adding furan dicarboxylic acid chloride, controlling the reaction temperature to be 14° C. to carry out polymerization reaction, to obtain a first polymerization solution, wherein the molar ratio of m-phenylenediamine to furan dicarboxylic acid chloride is 1:0.9;
[0086] (2) Preparation of the second polymerization solution:
[0087] Dissolving 4,5-epoxytetrahydrophthalic acid diglycidyl ester in dimethyl sulfoxide, adding m-phenylenediamine, and controlling the reaction temperature to be 130° C. to carry out polymerization reaction to obtain a second polymerization liquid, wherein the molar ratio of the 4,5-epoxytetrahydrophthalic acid diglycidyl ester to the m-phenylenediamine is 1:3;
[0088] The molar ratio of the intermediate phenylenediamine in step (1) to the intermediate phenylenediamine in step (2) is 10:0.1;
[0089] (3) Preparation of bio-based aramid polymer stock solution:
[0090] After the first polymerization liquid and the second polymerization liquid are uniformly mixed, furan dicarbonyl chloride is added to react again, and the reaction temperature is controlled to be 15° C. After the reaction is completed, the pH is adjusted to 8 to obtain a bio-based aramid polymer stock solution, wherein the mass solid content of the bio-based aramid polymer stock solution is 14% and the viscosity is 578 Po.
[0091] The molar ratio of the intermediate phenylenediamine in step (1) to the furan dicarboxylic acid chloride in step (3) is 1:0.1.
[0092] (4) Wet spinning process:
[0093] The bio-based aramid polymer stock solution is coagulated in a coagulation bath, stretched, washed, dried, heat treated, and curled to prepare high-strength bio-based aramid fibers;
[0094] The mass concentration of the glass fiber modified with the silane coupling agent in the coagulation bath is 4%; the temperature of the coagulation bath is 45° C., the coagulation bath is an aqueous solution of dimethyl sulfoxide, the mass concentration of dimethyl sulfoxide in the coagulation bath is 40%, and the length of the coagulation bath is 5 m.
[0095] The stretching process conditions are: the draft ratio is 2.0 times, the stretching bath is a dimethyl sulfoxide aqueous solution, and the mass concentration of dimethyl sulfoxide is 20%. The heat treatment temperature condition is 450°C.
[0096] Example 4
[0097] Preparation of a bio-based aramid fiber:
[0098] (1) Preparation of the first polymerization solution:
[0099] Dissolving m-phenylenediamine in N-methylpyrrolidone, then adding furan dicarboxylic acid chloride, controlling the reaction temperature to 20° C. to carry out polymerization reaction, to obtain a first polymerization solution, wherein the molar ratio of m-phenylenediamine to furan dicarboxylic acid chloride is 1:0.95;
[0100] (2) Preparation of the second polymerization solution:
[0101] Dissolving N,N,O-triglycidyl-p-aminophenol in N-methylpyrrolidone, adding m-phenylenediamine, and controlling the reaction temperature to be 150° C. to perform a polymerization reaction to obtain a second polymerization solution, wherein the molar ratio of N,N,O-triglycidyl-p-aminophenol to m-phenylenediamine is 1:3;
[0102] The molar ratio of the intermediate phenylenediamine in step (1) to the intermediate phenylenediamine in step (2) is 10:0.5;
[0103] (3) Preparation of bio-based aramid polymer stock solution:
[0104] After the first polymerization liquid and the second polymerization liquid are uniformly mixed, furan dicarbonyl chloride is added to react again, and the reaction temperature is controlled to be 30° C. After the reaction is completed, the pH is adjusted to 9 to obtain a bio-based aramid polymer stock solution, wherein the bio-based aramid polymer stock solution has a solid content of 15% and a viscosity of 593 Po.
[0105] The molar ratio of the intermediate phenylenediamine in step (1) to the furan dicarboxylic acid chloride in step (3) is 1:0.25.
[0106] (4) Wet spinning process:
[0107] The bio-based aramid polymer stock solution is coagulated in a coagulation bath, stretched, washed, dried, heat treated, and curled to prepare high-strength bio-based aramid fibers;
[0108] The mass concentration of the glass fiber modified with the silane coupling agent in the coagulation bath is 5%; the temperature of the coagulation bath is 70° C., the coagulation bath is an aqueous solution of N-methylpyrrolidone, the mass concentration of N-methylpyrrolidone in the coagulation bath is 35%, and the length of the coagulation bath is 4 m.
[0109] The stretching process conditions are: the draft ratio is 2.0 times, the stretching bath is an aqueous solution of N-methylpyrrolidone, and the mass concentration of N-methylpyrrolidone is 25%. The heat treatment temperature condition is 385°C.
[0110] Example 5
[0111] Preparation of a bio-based aramid fiber:
[0112] (1) Preparation of the first polymerization solution:
[0113] Dissolving m-phenylenediamine in N,N-dimethylacetamide, then adding furan dicarboxylic acid chloride, controlling the reaction temperature to 12° C. to perform a polymerization reaction to obtain a first polymerization solution, wherein the molar ratio of m-phenylenediamine to furan dicarboxylic acid chloride is 1:0.88;
[0114] (2) Preparation of the second polymerization solution:
[0115] Dissolving 1,3,5-triglycidyl-S-triazinetrione in N,N-dimethylacetamide, adding m-phenylenediamine, and controlling the reaction temperature to be 126° C. to perform polymerization reaction to obtain a second polymerization liquid, wherein the molar ratio of 1,3,5-triglycidyl-S-triazinetrione to m-phenylenediamine is 1:3.8;
[0116] The molar ratio of the intermediate phenylenediamine in step (1) to the intermediate phenylenediamine in step (2) is 10:0.5;
[0117] (3) Preparation of bio-based aramid polymer stock solution:
[0118] After the first polymerization liquid and the second polymerization liquid are uniformly mixed, furan dicarbonyl chloride is added to react again, and the reaction temperature is controlled to be 20° C. After the reaction is completed, the pH is adjusted to 9 to obtain a bio-based aramid polymer stock solution, wherein the mass solid content of the bio-based aramid polymer stock solution is 15% and the viscosity is 925 Po.
[0119] The molar ratio of the intermediate phenylenediamine in step (1) to the furan dicarboxylic acid chloride in step (3) is 1:0.25.
[0120] (4) Wet spinning process:
[0121] The bio-based aramid polymer stock solution is coagulated in a coagulation bath, stretched, washed, dried, heat treated, and curled to prepare high-strength bio-based aramid fibers;
[0122] The mass concentration of the glass fiber modified with the silane coupling agent in the coagulation bath is 1%; the temperature of the coagulation bath is 50° C., the coagulation bath is an aqueous solution of N,N-dimethylacetamide, the mass concentration of N,N-dimethylacetamide in the coagulation bath is 35%, and the coagulation bath length is 5 m.
[0123] The stretching process conditions are: the draft ratio is 1.5 times, the stretching bath is an aqueous solution of N,N-dimethylacetamide, and the mass concentration of N,N-dimethylacetamide is 20%. The heat treatment temperature condition is 410°C.
[0124] Example 6
[0125] Preparation of a bio-based aramid fiber:
[0126] (1) Preparation of the first polymerization solution:
[0127] Dissolving m-phenylenediamine in N,N-dimethylacetamide, then adding furan dicarboxylic acid chloride, controlling the reaction temperature to 10° C. to carry out polymerization reaction, to obtain a first polymerization solution, wherein the molar ratio of m-phenylenediamine to furan dicarboxylic acid chloride is 1:0.92;
[0128] (2) Preparation of the second polymerization solution:
[0129] Dissolving 1,3,5-triglycidyl-S-triazinetrione in N,N-dimethylacetamide, adding m-phenylenediamine, and controlling the reaction temperature to 70° C. to perform polymerization reaction to obtain a second polymerization liquid, wherein the molar ratio of 1,3,5-triglycidyl-S-triazinetrione to m-phenylenediamine is 1:3.3;
[0130] The molar ratio of the intermediate phenylenediamine in step (1) to the intermediate phenylenediamine in step (2) is 10:0.2;
[0131] (3) Preparation of bio-based aramid polymer stock solution:
[0132] After the first polymerization liquid and the second polymerization liquid are uniformly mixed, furan dicarbonyl chloride is added to react again, and the reaction temperature is controlled to be 15° C. After the reaction is completed, the pH is adjusted to 10 to obtain a bio-based aramid polymer stock solution, wherein the mass solid content of the bio-based aramid polymer stock solution is 15% and the viscosity is 743 Po.
[0133] The molar ratio of the intermediate phenylenediamine in step (1) to the furan dicarboxylic acid chloride in step (3) is 1:0.18.
[0134] (4) Wet spinning process:
[0135] The bio-based aramid polymer stock solution is coagulated in a coagulation bath, stretched, washed, dried, heat treated, and curled to prepare high-strength bio-based aramid fibers;
[0136] The mass concentration of the glass fiber modified with the silane coupling agent in the coagulation bath is 1%; the temperature of the coagulation bath is 65° C., the coagulation bath is an aqueous solution of N,N-dimethylacetamide, the mass concentration of N,N-dimethylacetamide in the coagulation bath is 30%, and the coagulation bath length is 5 m.
[0137] The stretching process conditions are: the draft ratio is 2.0 times, the stretching bath is an aqueous solution of N,N-dimethylacetamide, the mass concentration of N,N-dimethylacetamide is 15%, and the heat treatment temperature condition is 350°C.
[0138] Comparative Example 1
[0139] The bio-based aramid fiber was prepared by the same method as in Example 1, except that 1,3,5-triglycidyl-S-triazinetrione was not added during the preparation process, that is, the second polymerization solution was not prepared, and during the spinning process, no silane coupling agent-modified glass fiber was added to the coagulation bath.
[0140] Comparative Example 2
[0141] The bio-based aramid fiber was prepared by the same method as in Example 1, except that 1,3,5-triglycidyl-S-triazinetrione was not added during the preparation process, that is, the second polymerization solution was not prepared.
[0142] Comparative Example 3
[0143] The bio-based aramid fiber was prepared by the same method as in Example 1, except that during the spinning process, the glass fiber modified with the silane coupling agent was not added to the coagulation bath.
[0144] Comparative Example 4
[0145] The bio-based aramid fiber was prepared by the same method as in Example 1, except that the glass fiber (A110-Fiberglass) modified by the silane coupling agent was directly added to the bio-based aramid polymer stock solution and mixed evenly, wherein the amount of A110-Fiberglass added was 1% of the mass of the bio-based aramid polymer stock solution. The glass fiber (A110-Fiberglass) modified by the silane coupling agent was no longer added to the coagulation bath.
[0146] Comparative Example 5
[0147] The bio-based aramid fiber was prepared by the same method as in Example 1, except that the amount of 1,3,5-triglycidyl-S-triazinetrione was increased. In this comparative example 6, the molar ratio of 1,3,5-triglycidyl-S-triazinetrione to m-phenylenediamine in step (2) was 1:1.
[0148] Comparative Example 6
[0149] The bio-based aramid fiber was prepared by the same method as in Example 1, except that the reaction temperature in step (2) of this comparative example 7 was 160° C. (higher than the temperature condition specified in the present invention).
[0150] Comparative Example 7
[0151] The bio-based aramid fiber was prepared by the same method as in Example 1, except that the coagulation bath temperature of this comparative example 8 was 35° C. (lower than the coagulation bath temperature specified in the present invention).
[0152] Comparative Example 8
[0153] The bio-based aramid fiber was prepared by the same method as in Example 1, except that the mass concentration of the polar solvent in the coagulation bath of this comparative example 9 was 20% (lower than the coagulation bath concentration specified in the present invention).
[0154] The performance data of the bio-based aramid fibers prepared in the above examples and comparative examples were measured (measured in accordance with the national standard GB / T 8427-2019). The specific measurement results are shown in Table 1 below.
[0155] Table 1 Bio-based aramid fiber performance data
[0156]
[0157] It can be seen from the experimental data of Examples 1-6 that the bio-based aramid fiber prepared by the preparation method of the present invention has excellent strength performance, elongation at break and flame retardant performance. In the preparation method of the bio-based aramid fiber of the present invention, block copolymerization is achieved by using epoxy monomers and meta-phenylenediamine for epoxy ring-opening reaction, and the fiber molecular chains are cross-linked to improve the interaction force between the molecular chains, so that the bio-based aramid fiber has excellent strength performance. In addition, glass fiber with silane coupling agent added in the coagulation bath, in combination with a suitable spinning process, can realize the smooth spinning of bio-based aramid fiber, further reinforce the bio-based aramid fiber, and further improve the flame retardant and strength properties of the bio-based aramid fiber.
[0158] From the comparison of the data of Example 1 and Comparative Example 1, it can be seen that if the glass fiber without epoxy monomer and silane coupling agent is added during the preparation process, the fiber strength and flame retardancy are low. This is because there is no cross-linking structure in the fiber molecular chain and there is no reinforcing property of the glass fiber, resulting in low fiber strength and flame retardancy.
[0159] From the data comparison of Example 1 and Comparative Example 2, it can be seen that if epoxy monomers are not added during the preparation process, the fiber performance is slightly enhanced, and the improvement in fiber strength only relies on the composite reinforcement of glass fibers, lacks the formation of a cross-linked network structure, so the fiber strength is not significantly improved.
[0160] From the data comparison of Example 1 and Comparative Example 3, it can be seen that if no silane coupling agent is added to the glass fiber in the coagulation bath, the fiber performance is slightly enhanced, and the improvement in fiber strength only relies on the cross-linking structure of the epoxy monomer, and lacks the formation of a cross-linked network structure, so the fiber strength is not significantly improved, and the fiber flame retardant performance is not significantly improved.
[0161] From the data comparison of Example 1 and Comparative Example 4, it can be seen that if the glass fiber modified with silane coupling agent (A110-Fiberglass) is directly added to the bio-based aramid polymer stock solution, since the glass fiber is insoluble in polar solvents, the spinning cap will be blocked during the spinning process, resulting in spinning failure.
[0162] From the comparison of the data of Example 1 and Comparative Example 5, it can be seen that if the dosage ratio of 1,3,5-triglycidyl-S-triazinetrione is increased, excessive crosslinking in the polymer leads to modification failure and spinning failure.
[0163] From the data comparison of Example 1 and Comparative Example 6, it can be seen that if the temperature for preparing the second polymerization solution is higher than the temperature specified in the present invention, a large number of side reactions occur during the modification process, resulting in a reduction in the cross-linking structure of the polymer and a low improvement in fiber strength.
[0164] From the data comparison of Example 1 and Comparative Example 7, it can be seen that if the coagulation bath temperature is lower than the coagulation bath temperature specified in the present invention, the double diffusion rate of the solvent slows down, resulting in slow fiber formation and serious fiber adhesion, and it is impossible to obtain products for large-scale use.
[0165] From the data comparison between Example 1 and Comparative Example 8, it can be seen that if the coagulation bath concentration is lower than the coagulation bath concentration specified in the present invention, the fiber forming speed is fast, resulting in a serious fiber skin-core structure, an increase in the number of holes inside the fiber, an insignificant improvement in fiber strength, and the fiber is prone to parallel yarn formation.
[0166] The technical features of the above-described embodiments may be arbitrarily combined. To make the description concise, not all possible combinations of the technical features in the above-described embodiments are exhaustively listed. However, as long as there is no contradiction in the combination of these technical features, they should be considered to be within the scope of this specification.
[0167] For those skilled in the art, several modifications and improvements may be made without departing from the concept of the present invention, all of which belong to the protection scope of the present invention. The protection scope of the present invention shall be based on the attached claims.
Claims
1. A method for preparing bio-based aramid fiber, characterized in that: The preparation method is: S1, in an organic solvent, meta-phenylenediamine and furan dicarboxylic acid chloride are polymerized to obtain a first polymerization solution; In an organic solvent, an epoxy monomer and m-phenylenediamine undergo an epoxy ring-opening reaction to obtain a second polymer solution; S2, after the first polymerization liquid and the second polymerization liquid are evenly mixed, furan dicarbonyl chloride is added to carry out polymerization reaction, and after the reaction is completed, the pH is adjusted to weak alkalinity to obtain a bio-based aramid polymer stock solution; S3, the bio-based aramid polymer stock solution is formed by a wet spinning process to obtain the bio-based aramid fiber, wherein in the wet spinning process, a glass fiber modified with a silane coupling agent is added to the coagulation bath; In step S1, when preparing the first polymerization solution, the molar ratio of m-phenylenediamine to furan dicarboxylic acid chloride is 1:(0.8-0.95); When preparing the second polymerization solution, the molar ratio of the epoxy monomer to m-phenylenediamine is 1:(2-4); The molar ratio of the m-phenylenediamine used in the first polymerization solution to the m-phenylenediamine used in the second polymerization solution is 10:(0.1-0.5); The molar ratio of m-phenylenediamine used in the first polymerization solution of step S1 to furan dicarboxylic acid chloride used in step S2 is 1:(0.1-0.25); In step S1, during the preparation of the first polymerization solution, the polymerization reaction temperature is 5-20°C; In step S1, during the preparation of the second polymerization solution, the polymerization reaction temperature is 70-150°C; In step S2, the polymerization reaction temperature is 15-30°C; The coagulation bath temperature is 45-85° C., the coagulation bath is an aqueous solution of a polar solvent, the mass concentration of the polar solvent in the coagulation bath is 30-40%, and the coagulation bath length is 3-5 m.
2. The method for preparing bio-based aramid fiber according to claim 1, characterized in that: The epoxy monomer is any one of 3-(oxiran-2-ylmethoxy)-N,N-bis(oxiran-2-ylmethyl)aniline, 4,5-epoxytetrahydrophthalic acid diglycidyl ester, N,N,O-triglycidyl p-aminophenol, and 1,3,5-triglycidyl-S-triazinetrione.
3. The method for preparing bio-based aramid fiber according to claim 1, characterized in that: The organic solvent is any one or a combination of N,N-dimethylformamide, N,N-dimethylacetamide, dimethyl sulfoxide, and N-methylpyrrolidone.
4. The method for preparing bio-based aramid fiber according to claim 1, characterized in that: In step S3, the mass concentration of the glass fiber modified with the silane coupling agent in the coagulation bath is 1%-5%.
5. The method for preparing bio-based aramid fiber according to claim 1, characterized in that: The viscosity of the bio-based aramid polymer stock solution at 25° C. is 500-1000 Po, and the pH of the bio-based aramid polymer stock solution is 8-10.
6. A bio-based aramid fiber, characterized in that: The bio-based aramid fiber is prepared by the preparation method according to any one of claims 1 to 5.